Arsenic-molybdenum-oxygen cluster complex and preparation method thereof, modified compound of arsenic-molybdenum-oxygen cluster complex and preparation method thereof, modified electrode and application thereof
By using arsenic-molybdenum-oxygen cluster complexes combined with carboxylated multi-walled carbon nanotubes to modify the electrode, the problem of high cost of electrocatalysts in non-enzymatic electrochemical sensors has been solved, and high-sensitivity detection of H2O2 and cost reduction have been achieved.
Patent Information
- Application Number
- CN202410873582.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-29
AI Technical Summary
Among the existing electrochemical H2O2 detection methods, non-enzymatic electrochemical sensors require precious metal materials as electrocatalysts, resulting in high costs and limiting their wide application.
An arsenic-molybdenum-oxygen cluster complex and its modified complex were developed. By combining with carboxylated multi-walled carbon nanotubes, they are used to modify electrodes, improve the sensitivity of electrochemical detection, and reduce detection costs.
It achieves high-sensitivity electrochemical detection of H2O2, reduces detection costs, and expands the application scope of electrochemical detection.
Smart Images

Figure CN118852016A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electrochemical analysis, and specifically relates to an arsenic-molybdenum-oxygen cluster complex and a preparation method thereof, a modified composite of the arsenic-molybdenum-oxygen cluster complex and a preparation method thereof, a modified electrode and an application thereof. Background Art
[0002] Hydrogen peroxide (H2O2) is an important intermediate product in the human body's metabolism. The detection of H2O2 can be used to monitor the physiological indicators of the human body. Therefore, it is crucial to develop a fast, convenient and sensitive method for detecting H2O2. There are currently a variety of H2O2 detection technologies, such as chemiluminescence, fluorescence, liquid chromatography and electrochemical methods. Among these detection technologies, electrochemical methods have the advantages of fast detection speed, high sensitivity, high cost-effectiveness and strong portability. As an important component of electrochemical sensors, electrode materials have a great influence on the performance of the device. Depending on the electrode materials, electrochemical sensors used to detect H2O2 can be divided into enzyme sensors and non-enzyme sensors. Among them, enzyme sensors have problems such as poor structural stability, low repeatability and high cost; considering these shortcomings, non-enzyme electrochemical sensors have become the first choice for detecting H2O2. Non-enzyme electrochemical sensors require electrocatalysts in the process of detecting H2O2. Currently, effective electrocatalysts are mainly precious metal materials such as gold, platinum and palladium, but the high cost of existing electrocatalysts hinders their widespread application. Therefore, it is urgent to develop efficient and low-cost electrocatalytic materials for sensitive electrochemical detection of H2O2. Summary of the invention
[0003] In view of this, the present invention provides an arsenic molybdenum oxy-cluster complex and a preparation method thereof, a modified composite of the arsenic molybdenum oxy-cluster complex and a preparation method thereof, a modified electrode and an application thereof. The arsenic molybdenum oxy-cluster complex modified by the present invention has significant electrocatalytic reduction activity for H2O2, and the electrode modified by the complex can effectively improve the sensitivity of electrochemical detection of H2O2.
[0004] In order to solve the above technical problems, the present invention provides an arsenic-molybdenum-oxygen cluster complex having a chemical formula shown in Formula 1:
[0005] H9(C3N2H5) 15 [Mn(H2O)2][AsMo 10 O 35 ]2[Na(C3N2H4)2]2[AsMo 10 O 35 ]2·34H2O Formula 1;
[0006] The arsenic molybdenum oxygen cluster complex consists of 4 [AsMo 10 O 35 ] 7- Anion, 9 [H+ ], 15 [C3N2H5] + Cation, 1 [Mn(H2O)2] 2+ Unit, 2 [Na(C3N2H4)2] + The unit is composed of 34 crystal water molecules;
[0007] The [AsMo 10 O 35 ] 7- The Mo-O bond length in the anion is The [AsMo 10 O 35 ] 7- The length of the As-O bond in the anion is
[0008] 2 [AsMo 10 O 35 ] 7- Anion and 1 [Mn(H2O)2] 2+ The units are connected by coordination to form a sandwich structure {[Mn(H2O)2][AsMo 10 O 35 ]2} 12- Polyanion; the {[Mn(H2O)2][AsMo 10 O 35 ]2} 12- Mn in polyanions 2+ With two oxygen atoms in two water molecules and two [AsMo 10 O 35 ] 7- The four terminal O atoms of the anion are coordinated and connected;
[0009] [Na(C3N2H4)2] + Na in unit + With two N atoms of two C3N2H4 ligands and two [AsMo 10 O 35 ] 7- The two terminal oxygen atoms of the anion are coordinated.
[0010] Preferably, the space group of the arsenic molybdenum oxygen cluster complex is Pbca, and a is b is c is α is 110.145(3)°, β is 93.219(2)°, γ is 106.515(3)°, and Z is 1; the unit cell volume is
[0011] The present invention also provides a method for preparing the arsenic-molybdenum-oxygen cluster complex described in the above technical solution, comprising the following steps:
[0012] NaAsO2 and (NH4)6Mo7O 24 The mixed solution and the first pH value adjuster are first mixed to obtain an arsenic molybdenum oxy-cluster solution; the pH value of the system after the first mixing is 1.0;
[0013] The arsenic molybdenum oxy-cluster solution is mixed with manganese chloride, imidazole and a second pH value adjuster for a second time and then self-assembled in situ to obtain the arsenic molybdenum oxy-cluster complex; the pH value of the system after the second mixing is 3.5-4.5.
[0014] Preferably, the second mixed system contains NaAsO2, (NH4)6Mo7O 24 , the molar ratio of manganese chloride and imidazole is 0.269:0.404:0.695:1.469;
[0015] The first pH value adjusting agent is a hydrochloric acid solution; the second pH value adjusting agent is an ammonia solution;
[0016] The temperature of the in-situ self-assembly is 60-80° C., and the time is 30-40 minutes.
[0017] Preferably, the molar concentration of the hydrochloric acid solution is 3 to 5 mol / L, and the molar concentration of the ammonia solution is 0.5 to 1.5 mol / L.
[0018] The present invention also provides a modified composite of an arsenic-molybdenum-oxygen cluster complex, comprising an arsenic-molybdenum-oxygen cluster complex and a carboxylated multi-walled carbon nanotube, wherein the carboxylated multi-walled carbon nanotube is combined with the arsenic-molybdenum-oxygen cluster complex by intermolecular forces;
[0019] The arsenic molybdenum oxy-cluster complex is the arsenic molybdenum oxy-cluster complex described in the above technical solution or the arsenic molybdenum oxy-cluster complex prepared by the preparation method described in the above technical solution.
[0020] Preferably, the carboxylated multi-walled carbon nanotubes have an inner diameter of 5 to 8 nm, an outer diameter of 10 to 15 nm, a length of 2 to 8 μm, a carboxyl content of 1.0 to 2.0 mmol / g, and a specific surface area of ≥190 m 2 / g;
[0021] The mass ratio of the arsenic-molybdenum-oxygen cluster complex to the carboxylated multi-walled carbon nanotube is 1:0.8-1.2.
[0022] The present invention also provides a method for preparing the modified composite of the arsenic-molybdenum-oxygen cluster complex described in the above technical solution, comprising the following steps:
[0023] The arsenic molybdenum oxygen cluster complex and the carboxylated multi-walled carbon nanotube are ground and mixed to obtain the modified composite of the arsenic molybdenum oxygen cluster complex.
[0024] The present invention also provides a modified electrode, comprising a substrate and a coating coated on the surface of the substrate, wherein the coating is formed by film formation of a dispersion of a modified composite of an arsenic-molybdenum-oxygen cluster complex;
[0025] The preparation method of the dispersion of the modified composite of the arsenic molybdenum oxy-cluster complex comprises the following steps: mixing the modified composite of the arsenic molybdenum oxy-cluster complex, ethanol, a perfluorosulfonic acid type polymer solution and water to obtain the dispersion of the modified composite of the arsenic molybdenum oxy-cluster complex;
[0026] The modified composite of the arsenic molybdenum oxy-cluster complex is the modified composite of the arsenic molybdenum oxy-cluster complex described in the above technical solution or the modified composite of the arsenic molybdenum oxy-cluster complex prepared by the preparation method described in the above technical solution.
[0027] The present invention also provides the application of the modified electrode described in the above technical solution in electrochemical detection.
[0028] The present invention provides an arsenic-molybdenum-oxygen cluster complex having a chemical formula shown in Formula 1: H9(C3N2H5) 15 [Mn(H2O)2][AsMo 10 O 35 ]2[Na(C3N2H4)2]2[AsMo 10 O 35 ]2·34H2O Formula 1; the arsenic molybdenum oxygen cluster complex consists of 4 [AsMo 10 O 35 ] 7- Anion, 9 [H + ], 15 [C3N2H5] + Cation, 1 [Mn(H2O)2] 2+ Unit, 2 [Na(C3N2H4)2] + unit and 34 crystal water molecules; the [AsMo 10 O 35 ] 7- The Mo-O bond length in the anion is The [AsMo 10 O 35 ] 7- The length of the As-O bond in the anion is 2 [AsMo 10 O 35 ] 7- Anion and 1 [Mn(H2O)2] 2+ The units are connected by coordination to form a sandwich structure {[Mn(H2O)2][AsMo 10 O 35 ]2} 12-Polyanion; the {[Mn(H2O)2][AsMo 10 O 35 ]2} 12- Mn in polyanions 2+ With two oxygen atoms in two water molecules and two [AsMo 10 O 35 ] 7- The four terminal O atoms of the anion are coordinated and connected; the [Na(C3N2H4)2] + Na in unit + With two N atoms of two C3N2H4 ligands and two [AsMo 10 O 35 ] 7- The two terminal oxygen atoms of the anion are coordinated. The present invention uses the arsenic molybdenum oxygen cluster complex and the carboxylated multi-walled carbon nanotube as an electrode modification material, which can effectively improve the detection sensitivity of the electrochemical sensor and realize sensitive electrochemical detection of H2O2. The raw materials used in the preparation of the arsenic molybdenum oxygen cluster complex of the present invention are widely available and low in price, thereby reducing the cost of electrochemical detection and expanding the application range of electrochemical detection.
[0029] The preparation method of the novel arsenic-molybdenum-oxygen cluster complex provided by the invention is simple and easy to operate. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 To {B-β-AsMo9O 33} structure of two {Mo3O 13 {AsMo} is derived by inserting a {MoO6} octahedron into the cavity between the units. 10 O 35}Schematic diagram of building blocks;
[0031] Figure 2 [Mn(H2O)2] 2+ Polyhedral model diagram of unit coordination geometry, where white is O and pink is Mn;
[0032] Figure 3 [Na(C3N2H4)2] + The ball-and-stick model of the unit, where cyan is Na, gray is C, blue is N, and white is O;
[0033] Figure 4 For adjacent {[Mn(H2O)2][AsMo 10 O 35 ]2} 12- Polyanions react with [Na(C3N2H4)2] +Schematic diagram of the units alternately connected to form a one-dimensional chain structure, where - yellow is As, purple is Mo, pink is Mn, cyan is Na, gray is C, blue is N, and white is O;
[0034] Figure 5 is protonated imidazole [C3N2H5] + Cations and crystal water molecules fill the space between adjacent one-dimensional chain structures and interact with [AsMo 10 O 35 ] 7- Schematic diagram of the three-dimensional supramolecular structure formed by the oxygen atoms on the surface of the anion forming multi-point hydrogen bonds;
[0035] Figure 6 The powder X-ray diffraction pattern of the arsenic-molybdenum-oxygen cluster complex prepared in Example 1;
[0036] Figure 7 This is the infrared spectrum of the arsenic-molybdenum-oxygen cluster complex prepared in Example 1;
[0037] Figure 8 This is a thermogravimetric curve of the arsenic-molybdenum-oxygen cluster complex prepared in Example 1;
[0038] Fig. 9 This is the UV-visible absorption spectrum of the arsenic-molybdenum-oxygen cluster complex prepared in Example 1;
[0039] Fig.10 The SEM image and SEM-mapping image of the arsenic-molybdenum-oxygen cluster complex prepared in Example 1;
[0040] Fig.11 This is the EDS image of the arsenic-molybdenum-oxygen cluster complex prepared in Example 1;
[0041] Fig.12 The cyclic voltammetry curve of the arsenic-molybdenum-oxygen cluster complex / COOH-MCNTs / GCE prepared in Example 1;
[0042] Fig.13 Comparison of cyclic voltammetry curves of arsenic-molybdenum-oxygen cluster complex / COOH-MCNTs / GCE prepared in Example 1 at different scan rates;
[0043] Fig.14 Comparison of cyclic voltammetry curves of the arsenic-molybdenum-oxygen cluster complex / COOH-MCNTs / GCE prepared in Example 1 at different times;
[0044] Fig.15 Comparison of cyclic voltammetry curves of the arsenic-molybdenum-oxygen cluster complex / COOH-MCNTs / GCE prepared in Example 1 under different H2O2 concentrations;
[0045] Fig.16 The current-time response curve of the arsenic-molybdenum-oxygen cluster complex / COOH-MCNTs / GCE prepared in Example 1 to different concentrations of H2O2;
[0046] Fig.17 This is a linear relationship diagram between the current response signal of arsenic-molybdenum-oxygen cluster complex / COOH-MCNTs / GCE and the H2O2 concentration. DETAILED DESCRIPTION
[0047] The present invention provides an arsenic-molybdenum-oxygen cluster complex having a chemical formula shown in Formula 1:
[0048] H9(C3N2H5) 15 [Mn(H2O)2][AsMo 10 O 35 ]2[Na(C3N2H4)2]2[AsMo 10 O 35 ]2·34H2O Formula 1.
[0049] In the present invention, the arsenic molybdenum oxygen cluster complex is composed of 4 [AsMo 10 O 35 ] 7- Anion, 9 [H + ], 15 [C3N2H5] + Cation, 1 [Mn(H2O)2] 2+ Unit, 2 [Na(C3N2H4)2] + unit and 34 crystal water molecules.
[0050] In the present invention, {AsMo 10 O 35 The building units are preferably formed by 33} structure of two {Mo3O 13 It is derived by inserting a {MoO6} octahedron into the cavity between} units; Figure 1 is a schematic diagram of the derivation, wherein the yellow is As and the purple octahedron is {MoO6}. In the present invention, the [AsMo 10 O 35 ] 7- Mo in anion VI The atom is in a six-coordinate mode. In the present invention, the [AsMo 10 O 35 ] 7- The Mo-O bond length in the anion is In the present invention, the [AsMo 10 O 35 ] 7-As in anions III The atoms are located in the {AsO3} pyramidal geometry, and the [AsMo 10 O 35 ] 7- The length of the As-O bond in the anion is
[0051] In the present invention, 2 [AsMo 10 O 35 ] 7- Anion and 1 [Mn(H2O)2] 2+ The units are connected by coordination to form a sandwich structure {[Mn(H2O)2][AsMo 10 O 35 ]2} 12- Polyanion; the {[Mn(H2O)2][AsMo 10 O 35 ]2} 12- Mn in polyanions 2+ With two oxygen atoms in two water molecules and two [AsMo 10 O 35 ] 7- The four terminal O atoms of the anion are coordinated and connected; Mn 2+ The Mn-O w The bond length is preferably Mn 2+ With two [AsMo 10 O 35 ] 7- The bond length of Mn-O formed by the coordination of the four terminal O atoms of the anion is preferably
[0052] In the present invention, the {[Mn(H2O)2][AsMo 10 O 35 ]2} 12- Mn in polyanions 2+ It presents a distorted octahedral geometry. In the present invention, [Mn(H2O)2] 2+ The polyhedral model of the unit coordination geometry is shown in the figure Figure 2 As shown, white is O and pink is Mn.
[0053] In the present invention, the [Na(C3N2H4)2] + The two C3N2H4 ligands in the unit act as monodentate ligands and react with Na + Ion coordination forms a mononuclear [Na(C3N2H4)2] + In the present invention, the [Na(C3N2H4)2] +The fragment has a smaller size and steric hindrance, which is conducive to the reaction with [AsMo 10 O 35 ] 7- In the present invention, the [Na(C3N2H4)2] + Na in unit + With two N atoms of two C3N2H4 ligands and two [AsMo 10 O 35 ] 7- The two terminal oxygen atoms of the anion are coordinated. + The Na-N bond length formed by the coordination of the two N atoms of the two C3N2H4 ligands is preferably Na + With two [AsMo 10 O 35 ] 7- The Na-O bond length formed by the coordination of the two terminal oxygen atoms of the anion is preferably In the present invention, the [Na(C3N2H4)2] + The ball-and-stick model of the unit is Figure 3 As shown, cyan is Na, gray is C, blue is N, and white is O.
[0054] In the present invention, adjacent {[Mn(H2O)2][AsMo 10 O 35 ]2} 12- Polyanions react with [Na(C3N2H4)2] + The units are connected alternately to form a one-dimensional chain structure, as shown in the schematic diagram Figure 4 As shown, yellow is As, purple is Mo, pink is Mn, cyan is Na, gray is C, blue is N, and white is O.
[0055] In the present invention, the protonated imidazole [C3N2H5] + Cations and crystal water molecules fill the space between adjacent one-dimensional chain structures and interact with [AsMo 10 O 35 ] 7- The surface oxygen atoms of the anion (POM) form multi-point hydrogen bonds to form a three-dimensional supramolecular structure, as shown in the schematic diagram. Figure 5 In the present invention, the hydrogen bond preferably includes OH--O POM and NH--O POM , the OH--O POM The bond length is preferably The NH--O POM The bond length is preferably
[0056] In the present invention, the space group of the arsenic molybdenum oxygen cluster complex is preferably Pbca, and a is preferably b is preferably c is preferably α is preferably 110.145(3)°, β is preferably 93.219(2)°, γ is preferably 106.515(3)°, Z is preferably 1; the unit cell volume is preferably
[0057] In the present invention, the arsenic-molybdenum-oxygen cluster complex is preferably brown crystals.
[0058] The present invention also provides a method for preparing the arsenic-molybdenum-oxygen cluster complex described in the above technical solution, comprising the following steps:
[0059] NaAsO2 and (NH4)6Mo7O 24 The mixed solution and the first pH value adjuster are first mixed to obtain an arsenic molybdenum oxy-cluster solution; the pH value of the system after the first mixing is 1.0;
[0060] The arsenic molybdenum oxy-cluster solution is mixed with manganese chloride, imidazole and a second pH value adjuster for a second time and then self-assembled in situ to obtain the arsenic molybdenum oxy-cluster complex; the pH value of the system after the second mixing is 3.5-4.5.
[0061] The present invention combines NaAsO2 and (NH4)6Mo7O 24 The mixed solution and the first pH value adjusting agent are first mixed to obtain an arsenic molybdenum oxycarbon cluster solution. In the present invention, the NaAsO2 and (NH4)6Mo7O 24 The mixed solution preferably contains NaAsO2 and (NH4)6Mo7O 24 Dissolve in water to obtain (NH4)6Mo7O 24 Preferably (NH4)6Mo7O 24 ·4H2O. The present invention has no special requirements for the dissolution, as long as it can be completely dissolved. The present invention uses (NH4)6Mo7O 24 ·4H2O was used as the initial raw material to prepare the arsenic molybdenum oxygen cluster complex crystal. If Na2MoO4·2H2O was used to replace (NH4)6Mo7O 24 The product obtained by using 4H2O as raw material is brown powder, not crystal.
[0062] In the present invention, the first pH adjuster is preferably a hydrochloric acid solution, and the molar concentration of the hydrochloric acid solution is preferably 3-5 mol / L, more preferably 4 mol / L. In the present invention, the pH value of the first mixed system is 1.0; the present invention has no special limitation on the amount of the first pH adjuster, as long as the pH value of the first mixed system can be 1.0. The purpose of adjusting the pH here is to first generate saturated structured arsenic molybdenum oxygen clusters.
[0063] The present invention has no special requirements for the first mixing, as long as the mixing can be uniform.
[0064] After obtaining the arsenic molybdenum oxy-cluster solution, the present invention performs in-situ self-assembly after the arsenic molybdenum oxy-cluster solution is mixed with manganese chloride, imidazole, and a second pH regulator to obtain the arsenic molybdenum oxy-cluster complex. In the present invention, the second pH regulator is preferably an ammonia solution, and the molar concentration of the ammonia solution is preferably 0.5-1.5 mol / L, more preferably 1 mol / L. In the present invention, the pH value of the second mixed system is 3.5-4.5, preferably 4.0. The present invention has no special limitation on the amount of the second pH regulator, as long as the pH value of the second mixed system can meet the requirements. The present invention limits the pH value of the second mixed system to be within the above range, which is conducive to the formation of arsenic molybdenum oxy-cluster complex crystals, and the yield is highest when the pH value is 4.0; if the pH value is less than 3.5 or greater than 4.5, crystals cannot be obtained.
[0065] The present invention has no special requirements for the second mixing, as long as the mixing can be uniform.
[0066] In the present invention, the second mixed system contains NaAsO2, (NH4)6Mo7O 24 The molar ratio of manganese chloride to imidazole is preferably 0.269:0.404:0.695:1.469. The present invention uses imidazole as an organic ligand to prepare arsenic molybdenum oxygen cluster complexes; imidazole has a variety of coordination modes and a strong ability to bind transition metal ions, and is an effective linker for the coordination assembly of arsenic molybdenum oxygen cluster complexes. In addition, protonated imidazole can be used as a counter cation to bind to [AsMo 10 O 35 ] 7- The anion forms a hydrogen bond, thereby stabilizing the crystal structure and promoting the crystallization of the arsenic-molybdenum-oxygen complex. 2+ As the transition metal ion, the arsenic molybdenum oxygen cluster complex crystal was prepared. If Cu 2+ 、Co 2+ or Ni 2+ Replace Mn 2+ The result was an amorphous precipitate, which indicated that Mn 2+ Ions play a key role in the formation of AsMoO cluster complexes.
[0067] In the present invention, the temperature of the in-situ self-assembly is preferably 60-80° C., more preferably 60-70° C.; the time of the in-situ self-assembly is preferably 30-40 min, more preferably 30-35 min.
[0068] In the present invention, after the in-situ self-assembly, it is preferred that the method further includes: filtering the system after the in-situ self-assembly, cooling, standing and solid-liquid separation are performed in sequence to obtain the arsenic molybdenum oxygen cluster complex. The present invention has no special requirements for the filtration, and the conventional method in the art can be used. In the present invention, the temperature after cooling is preferably room temperature, and the temperature of the room temperature is preferably 20 to 35°C, more preferably 25 to 30°C. In the present invention, the standing time is preferably 6 to 8 days, more preferably 7 days. In the present invention, the standing process is the process of precipitating crystals. The present invention has no special requirements for the solid-liquid separation, as long as the crystals can be separated.
[0069] Polyoxometalates (polyoxometalates for short) are a class of extremely attractive nanoscale polyoxometalates, which have been widely used in many electrocatalytic processes due to their excellent structural stability and unique electrochemical redox properties. As a unique member of the polyoxometalate family, the Mo atom contained in the arsenic molybdenum oxygen cluster has a high oxidation state (+6) and can be easily converted between the reduced state and the oxidized state, thus having excellent electrocatalytic activity in the redox process. In addition, the redox properties of the arsenic molybdenum oxygen cluster can be easily achieved by adjusting the composition and spatial arrangement. Moreover, the introduction of As(III) will give the polyoxometalates excellent redox properties. However, due to the difficulty of the structural instability of the vacant arsenic molybdenum oxygen cluster, there are few reports on the preparation and separation of new arsenic molybdenum oxygen clusters. In particular, there is no report on the use of electrocatalytic materials based on new arsenic molybdenum oxygen cluster complexes for sensitive electrochemical detection of H2O2. The present invention uses a Mn(II) complex to coordinate and modify the arsenic molybdenum oxygen cluster to prepare a new arsenic molybdenum oxygen cluster complex.
[0070] The present invention also provides a modified composite of an arsenic-molybdenum-oxygen cluster complex, comprising an arsenic-molybdenum-oxygen cluster complex and a carboxylated multi-walled carbon nanotube, wherein the carboxylated multi-walled carbon nanotube is combined with the arsenic-molybdenum-oxygen cluster complex by intermolecular forces;
[0071] The arsenic molybdenum oxy-cluster complex is the arsenic molybdenum oxy-cluster complex described in the above technical solution or the arsenic molybdenum oxy-cluster complex prepared by the preparation method described in the above technical solution.
[0072] In the present invention, the inner diameter of the carboxylated multi-walled carbon nanotubes (COOH-MCNTs) is preferably 5 to 8 nm, more preferably 6 to 7 nm; the outer diameter of the carboxylated multi-walled carbon nanotubes is preferably 10 to 15 nm, more preferably 12 to 14 nm; the length of the carboxylated multi-walled carbon nanotubes is preferably 2 to 8 μm, more preferably 3 to 7 μm; the carboxyl content of the carboxylated multi-walled carbon nanotubes is preferably 1.0 to 2.0 mmol / g, more preferably 1.0 mmol / g; the specific surface area of the carboxylated multi-walled carbon nanotubes is preferably ≥190 m 2 / g, more preferably 190m 2 / g.
[0073] In the present invention, the mass ratio of the arsenic molybdenum oxo cluster complex to the carboxylated multi-walled carbon nanotube is preferably 1:0.8-1.2, more preferably 1:1.
[0074] In the present invention, the modified composite of the arsenic molybdenum oxygen cluster complex combines the excellent electrocatalytic activity of the arsenic molybdenum oxygen cluster complex with the good electron transfer performance of the carboxylated multi-walled carbon nanotubes; the synergistic signal amplification effect of the composite material on the H2O2 detection signal is utilized to improve the detection sensitivity of the sensor.
[0075] In the present invention, the method for preparing the modified composite of the arsenic-molybdenum-oxygen cluster complex described in the above technical solution comprises the following steps:
[0076] The arsenic molybdenum oxygen cluster complex and the carboxylated multi-walled carbon nanotube are ground and mixed to obtain the modified composite of the arsenic molybdenum oxygen cluster complex.
[0077] In the present invention, the grinding and mixing time is preferably 4 to 6 minutes, more preferably 5 minutes; the grinding is preferably carried out in an agate mortar; the grinding speed is preferably 55 to 65 r / min, more preferably 60 r / min; the grinding time is preferably 10 to 20 minutes, more preferably 15 to 18 minutes.
[0078] In the present invention, the carboxylated multi-walled carbon nanotubes are combined with the arsenic molybdenum oxygen cluster complexes through intermolecular forces during the grinding and mixing process, and the intermolecular forces include electrostatic attraction and / or hydrogen bonds.
[0079] In the present invention, the carboxylated multi-walled carbon nanotubes have a large specific surface area and excellent electron transfer performance. Compounding them with arsenic molybdenum oxygen cluster complexes can enhance the dispersion and conductivity of arsenic molybdenum oxygen cluster complexes on the electrode surface, further improve the electrocatalytic activity of arsenic molybdenum oxygen cluster complexes, synergistically expand the current detection signal, and improve the electrochemical detection sensitivity. The modified complex of arsenic molybdenum oxygen cluster complex provided by the present invention has excellent electrocatalytic activity, can be used as an electrode modification material, effectively improve the detection sensitivity of electrochemical sensors, and achieve highly sensitive electrochemical detection of H2O2. In the present invention, the carboxylated multi-walled carbon nanotubes are used as a carrier to immobilize arsenic molybdenum oxygen cluster complexes to effectively increase their dispersion and specific surface area on the electrode surface, thereby improving the electrocatalytic activity of arsenic molybdenum oxygen cluster complexes.
[0080] The present invention also provides a modified electrode, comprising a substrate and a coating coated on the surface of the substrate, wherein the coating is formed by film formation of a dispersion of a modified composite of an arsenic-molybdenum-oxygen cluster complex;
[0081] The preparation method of the dispersion of the modified composite of the arsenic molybdenum oxy-cluster complex comprises the following steps: mixing the modified composite of the arsenic molybdenum oxy-cluster complex, ethanol, a perfluorosulfonic acid type polymer solution and water to obtain the dispersion of the modified composite of the arsenic molybdenum oxy-cluster complex;
[0082] The modified composite of the arsenic molybdenum oxy-cluster complex is the modified composite of the arsenic molybdenum oxy-cluster complex described in the above technical solution or the modified composite of the arsenic molybdenum oxy-cluster complex prepared by the preparation method described in the above technical solution.
[0083] In the present invention, the substrate is preferably a glassy carbon electrode (GCE).
[0084] In the present invention, the ethanol is preferably anhydrous ethanol; the mass concentration of the perfluorosulfonic acid polymer (Nafion) solution is preferably 4-6%, more preferably 5%. In the present invention, the volume ratio of the ethanol, perfluorosulfonic acid polymer solution and water is preferably 760-800:18-22:180-220, more preferably 780:20:200. In the present invention, the mass ratio of the modified complex of the arsenic molybdenum oxygen cluster complex and the volume ratio of ethanol is preferably 8-12 mg:760-800 mL, more preferably 10 mg:780 mL. In the present invention, the mixing of the modified complex of the arsenic molybdenum oxygen cluster complex, ethanol, perfluorosulfonic acid polymer solution and water is preferably carried out under ultrasonic conditions, and the ultrasonic time is preferably 35-45 min, more preferably 40 min. The present invention has no special requirements for the power of the ultrasound, as long as it can be evenly dispersed.
[0085] The present invention preferably drips the dispersion of the modified complex of the arsenic molybdenum oxygen cluster complex onto the surface of the substrate and then dries to obtain the modified electrolyte. The present invention has no special requirements for the drip coating, and the conventional method in the art can be used. In the present invention, the drying is preferably carried out under an infrared lamp, and the drying time is preferably 1.8 to 2.2 hours, more preferably 2 hours.
[0086] In the present invention, the thickness of the coating is preferably 0.2 to 0.8 mm, more preferably 0.3 to 0.5 mm.
[0087] The modified electrode provided by the present invention shows excellent electrochemical detection performance for H2O2 detection, including a wide linear range of 50-50 μM and a high sensitivity of 0.2028 μA·μM -1 and a low detection limit of 1.47 μM.
[0088] The present invention also provides the application of the modified electrode in the above technical solution in electrochemical detection. In the present invention, the application of the modified electrode in electrochemical detection is preferably to use the modified electrode as an electrochemical sensor for hydrogen peroxide detection.
[0089] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0090] Example 1
[0091] 0.035 g NaAsO2 (0.269 mmol) and 0.5 g (NH4)6Mo7O 24 4H2O (0.404mmol) was dissolved in 20mL water to obtain NaAsO2 and (NH4)6Mo7O 24 Mixed solution; NaAsO2 and (NH4)6Mo7O 24 The mixed solution and a 4 mol / L HCl solution are mixed to adjust the pH value of the system to 1.0 to obtain an arsenic molybdenum oxy-cluster solution;
[0092] The arsenic molybdenum oxy-cluster solution, 0.1 g MnCl2·2H2O (0.695 mmol), 0.1 g imidazole (1.469 mmol), and an ammonia solution with a molar concentration of 1 mol / L were mixed to adjust the pH value of the system to 4.0, and then in-situ self-assembled for 30 min at 60° C.; the system after in-situ self-assembled was filtered, cooled to 30° C., and allowed to stand for 7 days, and solid-liquid separation was performed to obtain a brown crystalline arsenic molybdenum oxy-cluster complex.
[0093] 5 mg of arsenic molybdenum oxygen cluster complex was mixed with 5 mg of carboxylated multi-walled carbon nanotubes (COOH-MCNTs, inner diameter 7 nm, outer diameter 12 nm, length 7 μm, carboxyl content 1 mmol / g, specific surface area 190 m 2 / g) were ground and mixed in an agate mortar at a speed of 60r / min for 20min to obtain a modified composite of arsenic-molybdenum-oxygen cluster complex.
[0094] 10 mg of the modified composite of the arsenic molybdenum oxygen cluster complex, 200 μL of water, 780 μL of ethanol and 20 μL of a Nafion solution with a mass concentration of 5 wt% were ultrasonically dispersed for 40 min to obtain a dispersion of the modified composite of the arsenic molybdenum oxygen cluster complex;
[0095] The dispersion was transferred with a pipette, 3 μL was drop-coated on the surface of the glassy carbon electrode, and dried under an infrared lamp for 2 h to obtain a modified electrode (arsenic-molybdenum-oxygen cluster complex / COOH-MCNTs / GCE) with a coating thickness of 0.4 mm.
[0096] Detection of arsenic molybdenum oxygen cluster complexes:
[0097] The arsenic-molybdenum-oxygen cluster complex prepared in Example 1 was subjected to X-ray powder diffraction (XRD) detection to obtain an XRD spectrum, as shown in FIG. Figure 6 As shown. Figure 6 It was observed that the experimental XRD pattern of the arsenic molybdenum oxy-cluster complex prepared in Example 1 was basically consistent with the main peak position in the simulation spectrum (theory), thereby verifying the high purity of the arsenic molybdenum oxy-cluster complex.
[0098] The arsenic molybdenum oxygen cluster complex prepared in Example 1 was subjected to infrared detection to obtain an infrared spectrum. Figure 7 shown. Figure 7 Middle 900cm -1 、796cm -1 、732cm -1 、615cm -1 and 540cm -1 The four characteristic peaks at correspond to [AsMo 10 O 35 ] 7- Anion υ(As-O), υ(Mo=O t ), υ(Mo-Ob-Mo) and υ(Mo-Oc-Mo) stretching vibration. 2974~1046cm -1 The absorption peak in the region corresponds to the characteristic vibration of the imidazole ligand. -1 and 2843cm -1 The band at 1525cm is attributed to υ(CH) stretching vibration. -1 -1046cm -1The strong absorption peak at 413 cm-1 is attributed to the δ(NH) and δ(CH) bending vibrations, υ(C=C) and υ(C=N) stretching vibrations of the imidazole ring. -1 The band at is attributed to the stretching vibration of υ(Na-N), indicating that Na + Coordination between ions and imidazole ligands. 3138cm -1 The broad band at is the υ(OH) stretching vibration of the lattice water molecules.
[0099] The arsenic-molybdenum-oxygen cluster complex prepared in Example 1 was subjected to thermogravimetric analysis to obtain a thermogravimetric curve. Figure 8 shown. Figure 8 A three-step weight loss process is shown in the temperature range of 35 to 800°C. The first weight loss is 7.82% (calculated as 7.67%), which occurs between 35 and 287°C, due to the release of 34 lattice water molecules and 2 coordinated water molecules. In the temperature range of 287 to 492°C, the second weight loss is 15.19%, which is due to the removal of 19 imidazole molecules (calculated as 15.30%). When heated to 800°C, a third weight loss of 7.34% (calculated as 7.24%) was observed, due to the release of As2O3 and H2O during the decomposition of the POM framework, eventually forming mixed metal oxides. The total weight loss of 30.35% is very close to the expected theoretical value of 30.21%.
[0100] The arsenic molybdenum oxy-cluster complex prepared in Example 1 was subjected to ultraviolet-visible light detection in an aqueous solution with a pH value of 4.0 to obtain an ultraviolet-visible absorption spectrum. Fig. 9 shown. Fig. 9 In the wavelength range of 200-400 nm, two characteristic peaks appeared at 203 nm and 23 nm, belonging to O b,c →Mo and O d →Mo charge transfer. There is a broad absorption peak at about 450nm, which is attributed to Mn 2+ d→d electron transfer of ions.
[0101] The arsenic-molybdenum-oxygen cluster complex prepared in Example 1 was observed using a scanning electron microscope to obtain a SEM image and a SEM-mapping image, as shown in FIG. Fig.10 As shown. Fig.10 It can be seen that the arsenic-molybdenum-oxygen cluster complex has a rectangular structure with a smooth surface, clear edges, and a size between 5 and 10 μm.
[0102] The arsenic-molybdenum-oxygen cluster complex prepared in Example 1 was subjected to energy dispersive spectroscopy (EDS) analysis to obtain an EDS graph, as shown in FIG. Fig.11The combination of EDS and SEM-mapping images confirmed the uniform distribution of As, Mo, Mn, Na, C, N and O elements in the compound.
[0103] The results of the above XRD detection, infrared detection, thermogravimetric decomposition, ultraviolet detection, SEM detection and EDS detection prove that the arsenic molybdenum oxy-cluster complex prepared in Example 1 has the molecular formula shown in Formula 1. The crystallographic data of the arsenic molybdenum oxy-cluster complex prepared in Example 1 are shown in Table 1.
[0104] Table 1 Crystallographic data of arsenic-molybdenum-oxo cluster complexes
[0105]
[0106]
[0107] a R1=∑|F o |-|F c | / ∑|F c |;wR2=[∑w(F o 2 -F c 2 ) 2 / ∑w(F o 2 ) 2 ] 1 / 2
[0108] Performance test of modified electrode:
[0109] In a mixed solution of H2SO4 with a molar concentration of 0.1 mol / L and Na2SO4 with a molar concentration of 0.1 mol / L, in the potential range of -0.8 to +0.8 V, at a scanning rate of 100 mV / s, a three-electrode system was used to test the cyclic voltammetry (CV) behavior of the arsenic-molybdenum-oxygen cluster complex / COOH-MCNTs / GCE prepared in Example 1, and a cyclic voltammetry curve was obtained, as shown in FIG. Fig.12 shown. Fig.12 Two pairs of redox peaks are shown, with an average peak potential of E 1 / 2 =(E pa +E pc ) / 2 are -0.38V(II′), -0.03V(II-II′), respectively, which are attributed to Mo VI The oxidation peak (III') observed at +0.518 V is attributed to Mn 2+ oxidation peak.
[0110] The cyclic voltammetry (CV) behavior of the arsenic-molybdenum-oxygen cluster complex / COOH-MCNTs / GCE prepared in Example 1 was tested according to the above method, except that the scan rates were 40 mV·s -1 , 70mV·s -1 , 100mV·s -1 , 130mV·s -1 , 160mV·s -1 and 190mV·s -1 ; The cyclic voltammetry curves obtained at different scan rates are as follows: Fig.13 As shown. Fig.13 It can be seen from 40mV·s -1 Increase to 190mV·s -1 The current intensity of the CV curve gradually increases with the scanning rate. The peak current of II′ shows a good linear relationship with the scanning rate, which indicates that the redox process of the AsMoO2 complex is a surface-controlled process.
[0111] The CV curve of the arsenic-molybdenum-oxygen cluster complex / COOH-MCNTs / GCE prepared in Example 1 was tested according to the above method, with a scan rate of 100 mV·s -1 , and obtain the CV curves at different times, such as Fig.14 The stability of As-Mo-Oxygen Complex / COOH-MCNTs / GCE was evaluated by measuring the CV curves at different times. Fig.14 It shows that the peak current hardly decreases after 24 hours, which indicates that the AsMoO2 complex / COOH-MCNTs / GCE has good stability in the mixed solution of H2SO4 with a molar concentration of 0.1 mol / L and Na2SO4 with a molar concentration of 0.1 mol / L.
[0112] Fig.15 The CV curves of different H2O2 concentrations obtained by three-electrode system detection in a mixed solution of H2SO4 (0.1mol / L) and Na2SO4 (0.1mol / L) containing different H2O2 concentrations (0mmol / L, 0.1mmol / L, 0.2mmol / L, 0.3mmol / L and 0.4mmol / L) for AsMoO2 complex / COOH-MCNTs / GCE in the potential range of -0.8 to +0.8V and the scanning rate of 100mV / s. After adding 0.1mmol / LH2O2, the cathodic peak currents of I and II increased significantly, indicating that the reduced species of Mo center in the framework of AsMoO2 complex have significant electrocatalytic reduction activity for H2O2.
[0113] The present invention uses chronoamperometry (working potential is -0.4V) to evaluate the detection sensitivity of arsenic-molybdenum-oxygen cluster complex / COOH-MCNTs / GCE to H2O2. Fig.16 The current response curves of adding 50μM H2O2 to H2SO4 (0.1mol / L) and Na2SO4 (0.1mol / L) electrolyte solutions every 40s are shown. Arsenic molybdenum oxo-cluster complex / COOH-MCNTs / GCE reaches a steady-state current in a short time of less than 3s, indicating its fast current response to H2O2. In the range of 50-450μM, the response current of Arsenic molybdenum oxo-cluster complex / COOH-MCNTs / GCE increases linearly with the increase of H2O2 concentration.
[0114] According to the linear relationship between the current response signal of AsMoO2 / COOH-MCNTs / GCE and the detection results of H2O2 concentration, the linear regression equation is: H2O2 =0.2028C H2O2 +17.625(R 2 =0.998), the linear curve is as follows Fig.17 As shown. Fig.17 It can be seen that the sensitivity and detection limit (S / N = 3) are 0.2028 μA·μM respectively. -1 and 1.47 μM.
[0115] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. An arsenic molybdenum oxo complex, characterized in that: It has the chemical formula shown in Formula 1: H9(C3N2H5) 15 [Mn(H2O)2][AsMo 10 O 35 2[Na(C3N2H4)2]2[AsMo 10 O 35 2·34H2O Formula 1; The arsenic molybdenum oxygen cluster complex consists of 4 [AsMo 10 O 35 ] 7- Anion, 9 [H + ], 15 [C3N2H5] + Cation, 1 [Mn(H2O)2] 2+ Unit, 2 [Na(C3N2H4)2] + The unit is composed of 34 crystal water molecules; The [AsMo 10 O 35 ] 7- The Mo-O bond length in the anion is The [AsMo 10 O 35 ] 7- The length of the As-O bond in the anion is 2 [AsMo 10 O 35 ] 7- Anion and 1 [Mn(H2O)2] 2+ The units are connected by coordination to form a sandwich structure {[Mn(H2O)2][AsMo 10 O 35 ]2} 12- Polyanion; the {[Mn(H2O)2][AsMo 10 O 35 ]2} 12- Mn in polyanions 2+ With two oxygen atoms in two water molecules and two [AsMo 10 O 35 ] 7- The four terminal O atoms of the anion are coordinated and connected; [Na(C3N2H4)2] + Na in unit + With two N atoms of two C3N2H4 ligands and two [AsMo 10 O 35 ] 7- The two terminal oxygen atoms of the anion are coordinated.
2. The arsenic molybdenum oxo cluster complex according to claim 1, characterized in that: The space group of the arsenic-molybdenum-oxygen cluster complex is Pbca, and a is b is c is 24.7261 α is 110.145(3)°, β is 93.219(2)°, γ is 106.515(3)°, and Z is 1; the unit cell volume is 3. The method for preparing the arsenic molybdenum oxo complex according to claim 1 or 2, comprising the following steps: NaAsO2 and (NH4)6Mo7O 24 The mixed solution and the first pH value adjuster are first mixed to obtain an arsenic molybdenum oxy-cluster solution; the pH value of the system after the first mixing is 1.0; The arsenic molybdenum oxy-cluster solution is mixed with manganese chloride, imidazole and a second pH value adjuster for a second time and then self-assembled in situ to obtain the arsenic molybdenum oxy-cluster complex; the pH value of the system after the second mixing is 3.5-4.
5.
4. The preparation method according to claim 3, characterized in that: The second mixed system contains NaAsO2, (NH4)6Mo7O 24 , the molar ratio of manganese chloride and imidazole is 0.269:0.404:0.695:1.469; The first pH value adjusting agent is a hydrochloric acid solution; the second pH value adjusting agent is an ammonia solution; The temperature of the in-situ self-assembly is 60-80° C., and the time is 30-40 minutes.
5. The preparation method according to claim 4, characterized in that: The molar concentration of the hydrochloric acid solution is 3-5 mol / L, and the molar concentration of the ammonia solution is 0.5-1.5 mol / L.
6. A modified composite of an arsenic-molybdenum-oxo complex, characterized in that: It comprises an arsenic molybdenum oxygen cluster complex and a carboxylation multi-walled carbon nanotube, wherein the carboxylation multi-walled carbon nanotube is combined with the arsenic molybdenum oxygen cluster complex by intermolecular force; The arsenic molybdenum oxy-cluster complex is the arsenic molybdenum oxy-cluster complex according to claim 1 or 2 or the arsenic molybdenum oxy-cluster complex prepared by the preparation method according to any one of claims 3 to 5.
7. The modified composite of the arsenic-molybdenum-oxo complex according to claim 6, characterized in that: The carboxylated multi-walled carbon nanotube has an inner diameter of 5 to 8 nm, an outer diameter of 10 to 15 nm, a length of 2 to 8 μm, a carboxyl content of 1.0 to 2.0 mmol / g, and a specific surface area of 190 m 2 / g; The mass ratio of the arsenic-molybdenum-oxygen cluster complex to the carboxylated multi-walled carbon nanotube is 1:0.8-1.
2.
8. A method for preparing the modified composite of the arsenic molybdenum oxo complex according to claim 6 or 7, comprising the following steps: The arsenic molybdenum oxygen cluster complex and the carboxylated multi-walled carbon nanotube are ground and mixed to obtain the modified composite of the arsenic molybdenum oxygen cluster complex.
9. A modified electrode, characterized in that: The invention comprises a substrate and a coating coated on the surface of the substrate, wherein the coating is formed by film-forming a dispersion of a modified composite of an arsenic-molybdenum-oxygen cluster complex; The preparation method of the dispersion of the modified composite of the arsenic molybdenum oxy-cluster complex comprises the following steps: mixing the modified composite of the arsenic molybdenum oxy-cluster complex, ethanol, a perfluorosulfonic acid type polymer solution and water to obtain the dispersion of the modified composite of the arsenic molybdenum oxy-cluster complex; The modified composite of the arsenic molybdenum oxy-cluster complex is the modified composite of the arsenic molybdenum oxy-cluster complex according to claim 6 or 7 or the modified composite of the arsenic molybdenum oxy-cluster complex prepared by the preparation method according to claim 8.
10. Use of the modified electrode according to claim 9 in electrochemical detection.