Bio-based phosphorus-silicon-nitrogen synergistic flame retardant and preparation method thereof

By using phytic acid, silane coupling agent and trimethylol melamine to synthesize a bio-based phosphorus-silicon-nitrogen synergistic flame retardant, the problem of functional regulation and greening of the phosphorus-silicon-nitrogen synergistic high-efficiency flame retardant system is solved, and flame retardancy is achieved. Improved properties, hydrophobicity and anti-corrosion properties, suitable for a variety of application scenarios.

CN118852257APending Publication Date: 2024-10-29HEBEI UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410791067.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The existing phosphorus, silicon and nitrogen synergistic flame retardants are biased in terms of functional control, making it difficult to accurately meet the needs of different use scenarios. Moreover, they use petroleum-based materials as raw materials, which has environmental pollution problems. It is necessary to achieve phosphorus, silicon and nitrogen three-way synergistic and high-efficiency flame retardants. Green development of fuel system.

Method used

Phytic acid, silane coupling agent and trimethylol melamine are used as raw materials, and the bio-based phosphorus, silicon and nitrogen synergistic flame retardant is synthesized by adjusting the reaction molar ratio, and the silane coupling agent is used to react with phytic acid molecules to form ester groups. Combined with trimethylolated melamine, it achieves synergistic and efficient flame retardancy of phosphorus, silicon and nitrogen.

Benefits of technology

It achieves functional precision and green improvement of flame retardants, significantly improves flame retardancy, hydrophobicity and anti-corrosion properties, reduces economic costs, and is suitable for a variety of application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118852257A_ABST
    Figure CN118852257A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a bio-based phosphorus-silicon-nitrogen synergistic flame retardant, which comprises the following steps: by taking phytic acid as a basic skeleton for providing phosphate groups and phosphorus-silicon-nitrogen synergistic flame retardant synthesis, reacting a silane coupling agent with active hydrogen groups and trihydroxymethylated melamine with phytic acid molecules by utilizing six phosphate groups contained in the phytic acid molecules to prepare the bio-based phosphorus-silicon-nitrogen synergistic flame retardant. Forming an ester group with a phosphoric acid group of a phytic acid molecule, and further coupling to obtain the bio-based phosphorus-silicon-nitrogen synergistic flame retardant. The silane coupling agent with the active group contains amino, hydroxyl or epoxy group, and can react with phosphoric acid hydroxyl of phytic acid molecules to be connected to the phytic acid molecules. The molecules of the flame retardant contain a plurality of phosphate groups, silicon-containing functional groups and nitrogen-containing functional groups, so that the flame retardance, hydrophobicity and corrosion resistance of the bio-based phosphorus-silicon-nitrogen synergistic flame retardant are remarkably improved; and the atomic ratio of phosphorus, nitrogen and silicon in the flame retardant is flexibly regulated and controlled, so that the flame retardant product can more accurately meet the requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of flame retardant materials, and in particular to a bio-based phosphorus-silicon-nitrogen synergistic flame retardant and a preparation method thereof. Background Art

[0002] Phosphorus-silicon-nitrogen synergistic flame retardants have attracted much attention because of their flame retardancy, corrosion resistance, and hydrophobicity. However, during use, it was found that they could not accurately meet the needs of use due to their biased functions. In addition, most of the existing phosphorus-silicon-nitrogen synergistic flame retardants are based on petroleum. With the emergence of problems such as shortage of petroleum resources and environmental pollution and the enhancement of people's environmental awareness, biomass materials have emerged with their high phosphorus and hydroxyl content and green, sustainable and renewable characteristics. Therefore, how to flexibly adjust the design ratio of functional elements according to different usage scenarios to make them meet the needs more accurately, and how to chemically modify biomass materials to achieve the green development of phosphorus-silicon-nitrogen ternary synergistic and efficient flame retardant system, are two breakthroughs in the improvement of phosphorus-silicon-nitrogen flame retardant system. Summary of the invention

[0003] 1. Technical issues to be resolved

[0004] In view of the current problems of realizing the functional precision and greening of the phosphorus-silicon-nitrogen ternary synergistic high-efficiency flame retardant system, the present invention provides a bio-based phosphorus-silicon-nitrogen synergistic flame retardant and a preparation method thereof, and synthesizes a new bio-based phosphorus-silicon-nitrogen synergistic flame retardant with phytic acid, silane coupling agent and trimethylol melamine as raw materials. By adjusting the reaction molar ratio of phytic acid PA (providing a phosphorus source), trimethylol melamine (providing a nitrogen source) and silane coupling agent (providing a silicon source), the ratio of phosphorus-nitrogen-silicon in the flame retardant can be easily and flexibly adjusted according to different usage scenarios so that the product can more accurately match the needs, and the greening improvement of the phosphorus-silicon-nitrogen synergistic flame retardant is achieved.

[0005] (II) Technical solution

[0006] In a first aspect, the present invention provides a method for preparing a bio-based phosphorus-silicon-nitrogen synergistic flame retardant, which comprises: using phytic acid as a basic skeleton for the synthesis of a phosphorus-silicon-nitrogen synergistic flame retardant rich in phosphate groups, utilizing the six phosphate groups contained in the phytic acid molecule, reacting a silane coupling agent having an active hydrogen group and trimethylolated melamine with the phytic acid molecule to form an ester group with the phosphate group of the phytic acid molecule, and then coupling to synthesize a bio-based phosphorus-silicon-nitrogen synergistic flame retardant containing phosphorus-silicon-nitrogen; the silane coupling agent having an active group contains an amino, hydroxyl or epoxy group, which can react with the phosphoric acid hydroxyl group of the phytic acid molecule and connect to the phytic acid molecule.

[0007] According to a preferred embodiment of the present invention, the silane coupling agent having an active group is at least one of KH560 (γ-(2,3-epoxypropyl)propyltrimethoxysilane), KH-550 (3-aminopropyltriethoxysilane), KH-540 (3-aminopropyltrimethoxysilane), KH-602 (N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane), KH-792 (N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane) and KH-55 (3-hydroxypropyltrimethoxysilane). Preferably, the silane coupling agent is KH560.

[0008] The silane coupling agent in the present invention mainly serves the function of providing a silicon source. In order to smoothly couple with the phosphate group of the phytic acid molecule, the silane coupling agent must have an active group. Among them, KH560 contains an epoxy group at the end. When reacting with the phytic acid molecule, the epoxy group of KH560 opens to form an active group, which can react with the phosphate hydroxyl group of the phytic acid molecule. In addition, KH-550, KH540, KH-602 and KH-792 all contain amino groups (KH-602 and KH-792 also contain imino groups), and both amino groups and imino groups can react with the phosphate hydroxyl groups of the phytic acid molecule. KH-55 contains a hydroxyl group at the end, which can react with the phosphate hydroxyl group of the phytic acid molecule.

[0009] According to a preferred embodiment of the present invention, the preparation method is one of the following two synthetic routes:

[0010] Synthetic route 1:

[0011] Step 1: mixing the phytic acid from which water is removed by rotary evaporation with a silane coupling agent in an organic solvent, and heating the mixture for reaction to obtain a phytic acid esterification product (represented by PSi);

[0012] Step 2: Then, the trimethylol melamine is dissolved in an organic solvent to obtain a solution of the trimethylol melamine (represented by TM), and the solution is added to a solution of the phytated product (PSi), and the mixture is heated and stirred to react in the presence of anhydrous lithium chloride and p-dimethylaminopyridine, and then cooled, filtered, washed, and dried to obtain a bio-based phosphorus-silicon-nitrogen synergistic flame retardant (PSiN);

[0013] Synthesis route 2:

[0014] Step 1: adding phytic acid from which water is removed by rotary evaporation to an organic solvent, dissolving trimethylol melamine (TM) in the organic solvent to obtain a solution of trimethylol melamine, then adding phytic acid from which water is removed by rotary evaporation to the solution of trimethylol melamine, heating the mixture in the presence of anhydrous lithium chloride and p-dimethylaminopyridine to react, and obtaining an esterification product of phytic acid-trimethylol melamine (represented by PN);

[0015] Step 2: then add the silane coupling agent to the solution of the esterification product of phytic acid-trimethylol melamine, heat and stir to react, cool, filter, wash and dry to obtain a bio-based phosphorus-silicon-nitrogen synergistic flame retardant (PSiN).

[0016] According to a preferred embodiment of the present invention, the mass ratio of phytic acid, trimethylol melamine and silane coupling agent is 8-10:1-3:2-6.

[0017] According to a preferred embodiment of the present invention, the preparation method of trimethylol melamine (TM) is as follows: adding a sodium hydroxide solution with a mass concentration of 7-15% to a formaldehyde solution with a mass concentration of 35-40%, adjusting the pH to 8.5-9.5, heating to 45-55°C, adding melamine, heating to 80-90°C for reaction for 15-30 minutes, cooling, filtering, washing, and drying to obtain trimethylol melamine; the molar amount of formaldehyde is 3-3.5 times the molar amount of melamine. The three hydroxyl groups of melamine are methylhydroxylated by formaldehyde, so that melamine can undergo an esterification reaction with the phosphoric acid group of the phytic acid molecule, thereby introducing nitrogen elements into the phytic acid molecule.

[0018] The process of trimethylolation of melamine (MA) is as follows:

[0019]

[0020] According to a preferred embodiment of the present invention, the organic solvent used in the preparation method is N,N-dimethylformamide, and the amount thereof is: 10-20 parts of the organic solvent for every 8-16 parts of phytic acid.

[0021] According to a preferred embodiment of the present invention, in the preparation method, in step 1 of synthetic route 1 and step 2 of synthetic route 2, the reaction temperature of the silane coupling agent coupling to the phytic acid molecule is 45-55° C., and the reaction time is 2.5-4 h;

[0022] In step 2 of synthetic route 1 and step 1 of synthetic route 2, the reaction process temperature of trimethylol melamine and phytic acid molecules is 75-80° C., and the reaction time is 3-5 hours; and anhydrous lithium chloride and p-dimethylaminopyridine are used as catalysts in the reaction process, and the amount of anhydrous lithium chloride and p-dimethylaminopyridine is 0.3-0.8 parts by mass of anhydrous lithium chloride and 0.2-0.7 parts by mass of p-dimethylaminopyridine (DMAP) for every 1-6 parts of trimethylol melamine.

[0023] In a second aspect, the present invention provides a bio-based phosphorus-silicon-nitrogen synergistic flame retardant having one of the following structural formulas:

[0024]

[0025] In the above molecular structure, R 1 , R 2 , R 3 The structure is as follows:

[0026]

[0027] The molecules of the above product structure are synthesized by phytic acid PA, KH560 and trimethylol melamine (TM). Since the epoxy group at the end of KH560 forms a -C half bond and a -CO half bond when it is ring-opened, and the -CO half bond may be on the last carbon atom or on the penultimate carbon atom, these two ring-opening situations are random, so after the silane coupling agent KH560 and the phosphoric acid hydroxyl of the phytic acid molecule are coupled, the phosphoric acid hydroxyl of different phytic acid molecules will be randomly connected to the siloxane group of R1 or R3, and the phosphoric acid hydroxyl at different positions on the same phytic acid molecule will also be connected to the siloxane group of R1 or R3. Therefore, in the molecular structure of the phosphorus-silicon-nitrogen synergistic flame retardant prepared by KH560 in the following scheme, R1 / R3 is used to indicate that the group connected to this part is any one of R1 and R3.

[0028] The molecules of the three structural formulas (I), (II) and (III) were synthesized according to synthesis routes 1 and 2, respectively, to obtain the following six synthesis reaction processes.

[0029] ① In the compound of formula (I), the molar ratio of phytic acid, KH560 and trimethylol melamine (TM) is 1:1:1. According to the synthetic route 1: the method of the compound of formula (I) is as follows:

[0030] Step a:

[0031]

[0032] Step b:

[0033]

[0034] ② In the compound of formula (II), the molar ratio of phytic acid, KH560 and trimethylol melamine (TM) is 1:2:2. According to the synthetic route 1: the method of the compound of formula (II) is as follows:

[0035] Step a:

[0036]

[0037] Step b:

[0038]

[0039] ③ In the compound of formula (III), the molar ratio of phytic acid, KH560 and trimethylol melamine (TM) is 1:3:3. According to the synthesis route 1: the method of the compound of formula (III) is as follows:

[0040] Step a:

[0041]

[0042] Step b:

[0043]

[0044] ④ In the compound of formula (I), the molar ratio of phytic acid, KH560 and trimethylol melamine (TM) is 1:1:1. According to the synthetic route 2: the method of the compound of formula (I) is as follows:

[0045] Step a:

[0046]

[0047] Step b:

[0048]

[0049] ⑤ In the compound of formula (II), the molar ratio of phytic acid, KH560 and trimethylol melamine (TM) is 1:2:2. According to the synthetic route 2: the method of the compound of formula (II) is as follows:

[0050] Step a:

[0051]

[0052] Step b:

[0053]

[0054] ⑥ In the compound of formula (III), the molar ratio of phytic acid, KH560 and trimethylol melamine (TM) is 1:3:3. According to the synthetic route 2: the method of the compound of formula (III) is as follows:

[0055] Step a:

[0056]

[0057] Step b:

[0058]

[0059] The catalysts used in the reaction of trimethylol melamine with phytic acid PA or phytic acid esterification product (PSi) are anhydrous lithium chloride LiCl and p-dimethylaminopyridine DMAP.

[0060] Exemplarily, phytic acid can adopt a commercially available 70% phytic acid aqueous solution, and the water in the phytic acid aqueous solution needs to be removed by rotary evaporation before being added to the reaction system. The temperature of rotary evaporation to remove water is 40-60°C, and the vacuum degree is 0.09MPa-0.15MPa. Preferably, the temperature of rotary evaporation to remove water is 55°C, and the vacuum degree is 0.1MPa. In step 1 of synthetic route 1 and step 1 of synthetic route 2, an organic solvent is used for 25-30% of the total amount of organic solvent, and the remaining organic solvent is used up in step 2 of synthetic route 1 and step 2 of synthetic route 2. After the final reaction is completed, it is cooled to room temperature, filtered, washed three times with distilled water, dried in an 80°C forced air drying oven for 2-3h, and dried in a 110°C vacuum drying oven for 3-5h to constant weight to obtain a bio-based phosphorus-silicon-nitrogen synergistic flame retardant (PSiN) product.

[0061] (III) Beneficial effects

[0062] The bio-based phosphorus-silicon-nitrogen synergistic flame retardant provided by the present invention uses phytic acid as a basic framework for the synthesis of a phosphorus-silicon-nitrogen synergistic flame retardant rich in phosphoric acid groups, a silane coupling agent as a silicon source, and melamine as a nitrogen source. The six highly reactive phosphoric acid groups symmetrically connected around the phytic acid molecules are used to connect the silane coupling agent and melamine of a specific molecular ratio to the phytic acid molecules, respectively, to obtain a bio-based phosphorus-silicon-nitrogen synergistic flame retardant. The flame retardant molecular structure contains multiple phosphate groups, silicon-containing functional groups, and nitrogen-containing functional groups, which not only significantly improves the flame retardancy, hydrophobicity, and corrosion resistance of the bio-based phosphorus-silicon-nitrogen synergistic flame retardant. Since the phytic acid molecule has abundant active phosphoric acid groups, the atomic ratios of phosphorus, nitrogen, and silicon in the flame retardant can be flexibly adjusted according to the different usage scenarios of the phosphorus-silicon-nitrogen synergistic flame retardant so that the flame retardant product can meet the needs more accurately.

[0063] Before the reaction, melamine is modified by trihydroxy activation, so that it has higher reactivity with carboxyl and the like, and is more easily connected to the phosphate hydroxyl group of the phytic acid molecule. The bio-based phosphorus-silicon-nitrogen synergistic flame retardant of the present invention uses biomass materials (phytic acid) as basic raw materials, which is not only a breakthrough in realizing the greening of phosphorus-silicon-nitrogen flame retardant systems, but also reduces economic costs and has broad potential application fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0064] Figure 1 FTIR spectra of three different samples: phytic acid PA (curve a), phytic acid-trimethylol melamine esterification product PN (curve b), and synergistic flame retardant PSiN-III (curve c).

[0065] Figure 2This is a thermogravimetric (TG) curve of the phosphorus-silicon-nitrogen synergistic flame retardant (PSiN-III) and the reactants prepared in Example 4, wherein MA is melamine, TM is trimethylolated melamine, and PSiN is a phosphorus-silicon-nitrogen synergistic flame retardant.

[0066] Figure 3 It is a differential thermogravimetric (DTG) curve of the phosphorus-silicon-nitrogen synergistic flame retardant (PSiN-III) prepared in Example 4, wherein MA is melamine, TM is trimethylolated melamine, and PSiN is a phosphorus-silicon-nitrogen synergistic flame retardant. DETAILED DESCRIPTION

[0067] In order to better explain the present invention and facilitate understanding, the present invention is described in detail below through specific implementation modes in conjunction with the accompanying drawings.

[0068] Example 1

[0069] The present invention provides a method for preparing a bio-based phosphorus-silicon-nitrogen synergistic flame retardant (PSiN-1), which specifically comprises the following steps:

[0070] Step a, preparing the esterification product (PSi) of phytic acid-silane coupling agent

[0071] Weigh 8g of phytic acid solution (containing 5.6g of pure phytic acid, 0.0085mol), add it to 24.5mL of N,N-dimethylformamide (relative density 0.95g / mL), mix well, then transfer the above solution to a rotary evaporator, remove water by rotary evaporation at 55°C and vacuum degree of 0.1MPa, place it in a four-necked flask, add 2.00g (0.0085mol) of KH560, heat to 50°C, react for 3h, and obtain a solution of phytate ester (PSi). The reaction process is as follows:

[0072]

[0073] Step b, preparation of trimethylol melamine (TM):

[0074] 50 mL of formaldehyde aqueous solution was added to a three-necked flask, 10 wt% sodium hydroxide solution was added dropwise, the pH value of the system was adjusted to 8-9, then heated to 50°C, 27.93 g of melamine was added, stirred, heated to 85°C, reacted for 15 min, cooled to room temperature, filtered, washed three times with distilled water, dried in an air drying oven at 80°C for 3 h, and dried in a vacuum drying oven at 110°C for 5 h until constant weight, to obtain trimethylol melamine (TM). The reaction process is as follows:

[0075]

[0076] Step c, preparing a bio-based phosphorus-silicon-nitrogen synergistic flame retardant:

[0077] Weigh 1.83g (0.0085mol) of trimethylol melamine (containing 1.067g of melamine) prepared in step b and dissolve it in 45.5mL N, N-dimethylformamide to obtain a trimethylol melamine solution; add the trimethylol melamine solution to the solution of the phytate product (PSi) prepared in step a, heat to 80°C, add 0.3g of anhydrous lithium chloride and 0.2g of p-dimethylaminopyridine, stir, react for 4h, cool to room temperature, filter, wash three times with distilled water, dry in an air drying oven at 80°C for 3h, and dry in a vacuum drying oven at 110°C for 4h to constant weight to obtain a phosphorus-silicon-nitrogen synergistic flame retardant (PSiN-1) of formula (I). The reaction process is:

[0078]

[0079] Example 2

[0080] This embodiment provides a bio-based phosphorus-silicon-nitrogen synergistic flame retardant (PSiN-2), the preparation steps are the same as those in Example 1, except that the amount of raw materials used is: 4.00 g of KH560 (0.0169 mol), 3.66 g of trimethylolated melamine (0.0169 mol). The product structure is as follows, which is a phosphorus-silicon-nitrogen synergistic flame retardant of formula (II):

[0081]

[0082] Example 3

[0083] The embodiment of the present invention provides a bio-based phosphorus-silicon-nitrogen synergistic flame retardant (PSiN-3), and the preparation steps are the same as those in Example 1, except that the amount of raw materials used is: 6.00 g of KH560 (0.0254 mol), 5.49 g of trimethylolated melamine (0.0254 mol). The product structure is as follows, which is a phosphorus-silicon-nitrogen synergistic flame retardant of formula (III):

[0084]

[0085] Example 4

[0086] The embodiment of the present invention provides a method for preparing a bio-based phosphorus-silicon-nitrogen synergistic flame retardant, which specifically comprises the following steps:

[0087] Step a: Preparation of trimethylol melamine:

[0088] 50 mL of formaldehyde aqueous solution was added into a three-necked flask, 10 wt % sodium hydroxide solution was added dropwise, the pH value of the system was adjusted to 8-9, and then heated to 50° C., 27.93 g of melamine was added, stirred, heated to 85° C., reacted for 15 min, cooled to room temperature, filtered, washed three times with distilled water, dried in an air drying oven at 80° C. for 3 h, and dried in a vacuum drying oven at 110° C. for 5 h until constant weight was obtained to obtain 47.87 g of trimethylol melamine (TM).

[0089] Step b: Preparation of phosphorus nitrogen compound PN

[0090] Weigh 8 g of phytic acid solution (containing 5.6 g of phytic acid), add it to 24.5 mL of N, N-dimethylformamide, mix well, then transfer the above solution to a rotary evaporator, and perform rotary evaporation at 55° C. and a vacuum degree of 0.1 MPa for 30 min to remove water; weigh 5.5 g of TM and dissolve it in 20 ml of N, N-dimethylformamide, add it to a four-necked flask and heat it to 50° C., then add the above rotary evaporated phytic acid solution to the four-necked flask, heat it to 80° C., add 0.3 g of anhydrous lithium chloride and 0.2 g of p-dimethylaminopyridine, react for 3 h, and obtain a solution of the esterification product (PN) of phytic acid-trimethylol melamine;

[0091] Step c, preparing a bio-based phosphorus-silicon-nitrogen synergistic flame retardant:

[0092] Weigh 6.0 g of silane coupling agent and add it to the solution of the esterification product (PN) of phytic acid-trimethylol melamine prepared in step b, heat to 80° C., stir, react for 3 h, cool to room temperature, filter, wash three times with distilled water, dry in an air drying oven at 80° C. for 3 h, and dry in a vacuum drying oven at 110° C. for 5 h to constant weight to obtain a phosphorus-silicon-nitrogen synergistic flame retardant (PSiN-4) with a structure of formula (III).

[0093] Performance Testing

[0094] 1. The bio-based phosphorus-silicon-nitrogen synergistic flame retardant (PSiN) prepared in Examples 1-4 was tested for performance. The performance testing methods are as follows:

[0095] (1) Infrared spectroscopy (FT-IR) test

[0096] The KBr pellet method was used and the test was performed using a Nicolet 8700 Fourier transform infrared spectrometer. Resolution: 4 cm -1 , scanning range 4000cm -1 ~500cm -1 .

[0097] like Figure 1The FTIR spectra of the reaction raw materials and target products such as phytic acid PA (curve a), phytic acid-trimethylol melamine esterification product PN (curve b), and synergistic flame retardant PNSi (curve c, the molar ratio of PA:TM:KH560 in the flame retardant is 1:3:3). Figure 1 As shown in the three curves a, b, and c, 3400cm -1 The absorption peak near 1209cm is generated by the stretching vibration of OH in PA. -1 、1070cm -1 and 946cm -1 The absorption peaks near 1652 cm-1 are attributed to the stretching vibration absorption of P=O, PO and POC structures in PA molecules. -1 , 1335cm -1 New absorption peaks appear at 794 cm-1, corresponding to the stretching vibration absorption peaks of NH and CN in the TM structure, indicating that esterification reaction occurs between PA and TM. -1 The stretching vibration absorption peak of Si-C in the KH560 structure appears at 1261 cm -1 There is no absorption peak nearby, indicating the disappearance of the epoxy structure of KH560, proving that PA and KH560 undergo a ring-opening reaction. In summary, infrared spectroscopy proves that the target product, phosphorus-silicon-nitrogen synergistic flame retardant, is successfully prepared.

[0098] (2) Phosphorus content test

[0099] The phosphorus content of the samples was tested according to GB 5009.87-2016. (National Food Safety Standard, Determination of Phosphorus in Food). Each sample was tested three times and the results were averaged.

[0100] (3) Particle size analysis test

[0101] The prepared bio-based phosphorus-silicon-nitrogen synergistic flame retardant (PSiN) was evenly dispersed in an ultrasonic water bath and tested using a WJL602 laser particle size analyzer from Shanghai INESA Physical Optical Instrument Co., Ltd.

[0102] (4) Yield calculation

[0103] The yield is calculated based on the non-excess reactant components:

[0104] PSiN yield = (actual yield of PSiN / theoretical yield of PSiN)*100%.

[0105] (5) Carbonization rate

[0106] The carbonization rate at 700°C was obtained by thermogravimetric (TG) test data, and the test was performed using a Pyris1TGA thermogravimetric analyzer (PerkinElmer, USA). 2 Under the atmosphere, the heating rate was set to 10°C / min, and the temperature range was 30-1000°C from room temperature.

[0107] Figure 2 This is a thermal gravimetric (TG) curve of the phosphorus-silicon-nitrogen synergistic flame retardant (PSiN-III) prepared in Example 4 and the reactants. Figure 3 This is a differential thermogravimetric (DTG) curve of the phosphorus-silicon-nitrogen synergistic flame retardant (PSiN-Ⅲ) prepared in Example 4. It can be seen from the figure that melamine (MA) has a thermal decomposition stage with a temperature range of 260°C-405°C. The main thermal decomposition occurs in this temperature range, and the residual carbon rate at 700°C is only 7.21%. The trimethylolation product (TM) of melamine has two main thermal decomposition stages, the first thermal decomposition stage is at 125°C-225°C, the second thermal decomposition stage is between 370°C-450°C, the main thermal decomposition stage is the second stage, and the residual carbon rate at 700°C is 21.82%. The phosphorus-silicon-nitrogen synergistic flame retardant (PSiN-Ⅲ) has two thermal decomposition stages, the first thermal decomposition stage is at 275°C-375°C, the second thermal decomposition stage is at 450°C-550°C, the main thermal decomposition stage is the first stage, and the residual carbon rate at 700°C is as high as 32.18%. Thermogravimetric analysis shows that after melamine and silane coupling agents are bonded to phytic acid molecules, the thermal decomposition stage of the material changes significantly, and the thermal stability of the phosphorus-silicon-nitrogen synergistic flame retardant is significantly improved.

[0108] The specific test results are shown in Table 1:

[0109] Table 1 Results of performance tests of bio-based phosphorus-silicon-nitrogen synergistic flame retardants prepared in Examples 1-4

[0110]

[0111] It can be seen from the above table that the amounts of other raw materials added as defined in the present invention and other reaction conditions used in Examples 1-4 can achieve technical effects substantially equivalent to those of Examples 1-4 as long as they are within the range defined in the present invention.

[0112] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a bio-based phosphorus-silicon-nitrogen synergistic flame retardant, characterized in that: It includes: Phytic acid is used as a basic framework for the synthesis of a synergistic flame retardant rich in phosphate groups and phosphorus-silicon-nitrogen. The six phosphate groups contained in the phytic acid molecule are utilized to react a silane coupling agent with an active hydrogen group and trimethylol melamine with the phytic acid molecule to form an ester group with the phosphate group of the phytic acid molecule, thereby coupling to synthesize a bio-based phosphorus-silicon-nitrogen synergistic flame retardant containing phosphorus-silicon-nitrogen. The silane coupling agent with an active group contains an amino, hydroxyl or epoxy group, which can react with the phosphoric acid hydroxyl group of the phytic acid molecule and connect to the phytic acid molecule.

2. The preparation method according to claim 1, characterized in that: The silane coupling agent having an active group is at least one of KH560, KH-550, KH-540, KH-602, KH-792 and KH-55.

3. The preparation method according to claim 2, characterized in that: The preparation method is one of the following two synthetic routes: Synthesis route 1: Step 1: adding phytic acid to an organic solvent to remove water by rotary evaporation to obtain a phytic acid organic solvent from which water has been removed by rotary evaporation, then adding a silane coupling agent to the phytic acid organic solvent from which water has been removed by rotary evaporation, mixing, and heating to react to obtain a phytic acid esterification product; Step 2: Then dissolving the trimethylol melamine in an organic solvent to obtain a solution of the trimethylol melamine, adding the solution to the solution of the phytated product, heating and stirring to react in the presence of anhydrous lithium chloride and p-dimethylaminopyridine, cooling, filtering, washing, and drying to obtain a bio-based phosphorus-silicon-nitrogen synergistic flame retardant; Synthesis route 2: Step 1: adding phytic acid to an organic solvent and performing rotary evaporation to remove water to obtain a phytic acid organic solvent from which water has been removed by rotary evaporation, and dissolving trimethylolated melamine in an organic solvent to obtain a trimethylolated melamine solution, and then adding the phytic acid from which water has been removed by rotary evaporation to the trimethylolated melamine solution, and heating the reaction in the presence of anhydrous lithium chloride and p-dimethylaminopyridine to obtain an esterification product of phytic acid-trimethylolated melamine; Step 2: then add the silane coupling agent to the solution of the esterification product of phytic acid-trimethylol melamine, heat and stir to react, cool, filter, wash and dry to obtain a bio-based phosphorus-silicon-nitrogen synergistic flame retardant.

4. The preparation method according to claim 3, characterized in that: The mass ratio of phytic acid, trimethylol melamine and silane coupling agent is 8-10:1-6:2-6.

5. The preparation method according to claim 3 or 4, characterized in that: The preparation method of trimethylol melamine is as follows: adding a sodium hydroxide solution with a mass concentration of 7-15% to a formaldehyde solution with a mass concentration of 35-40%, adjusting the pH to 8.5-9.5, heating to 45-55° C., adding melamine, heating to 80-90° C., reacting for 15-30 minutes, cooling, filtering, washing, and drying to obtain trimethylol melamine; the molar amount of formaldehyde is 3-3.5 times the molar amount of melamine.

6. The preparation method according to claim 1, characterized in that: The organic solvent used in the preparation method is N,N-dimethylformamide, and the usage amount thereof is: 10-20 parts of the organic solvent are used for every 8-16 parts of phytic acid.

7. The preparation method according to claim 1, characterized in that: In the preparation method, In step 1 of synthetic route 1 and step 2 of synthetic route 2, the reaction temperature of the silane coupling agent and phytic acid is 45-55° C., and the reaction time is 2.5-4 h; In step 2 of synthetic route 1 and step 1 of synthetic route 2, the reaction temperature of the reaction process of coupling trimethylol melamine to phytic acid molecules is 75-80° C., and the reaction time is 3-5 hours; and anhydrous lithium chloride and p-dimethylaminopyridine are used as catalysts in the reaction process, and the amount of anhydrous lithium chloride and p-dimethylaminopyridine is 0.3-0.8 parts by mass of anhydrous lithium chloride and 0.2-0.7 parts by mass of p-dimethylaminopyridine for every 1-6 parts by mass of trimethylol melamine.

8. A bio-based phosphorus-silicon-nitrogen synergistic flame retardant having one of the following structural formulas: In the above structure, the structures of R1, R2 and R3 are as follows: