Ultra-slip antifouling coating with synergistic function of dispersing and killing fouling organisms and its preparation

Through the synergy between layer-by-layer self-assembly technology and D-cysteine ​​and nanosilver, a SLIC-D coating with super-slip, dispersing and bactericidal functions is formed, which solves the problem of lubricant loss and bactericidal use in the prior art. Too many problems have achieved efficient and long-term marine pollution prevention effects.

CN118852934BActive Publication Date: 2024-11-29NORTHEASTERN UNIV CHINA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411351178.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-11-29
Estimated Expiration
2044-09-26

AI Technical Summary

Technical Problem

The existing ultra-slip anti-fouling coating has limited effect in preventing marine biological adhesion, lubricants are easily lost, and excessive use of fungicides cannot be effectively avoided from adhesion of biological membranes, making it difficult to achieve long-term efficient anti-fouling.

Method used

Using layer-by-layer self-assembly technology, combined with D-cysteine ​​and nanosilver, the SLIC-D coating with ultra-slip, dispersing and bactericidal functions is formed through S-Ag coordination reaction, reducing the use of bacterial agents and enhancing the coating. Antibacterial and antifouling properties.

Benefits of technology

It realizes a triple synergistic effect of difficult adsorption, easy dispersion and strong sterilization, significantly improves the anti-fouling effect, reduces the amount of fungicide, enhances the stability and durability of the coating, and effectively prevents marine biological pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118852934B_ABST
    Figure CN118852934B_ABST
Patent Text Reader

Abstract

An ultra-slip antifouling coating with a synergistic function of dispersing and killing fouling organisms and its preparation belong to the field of marine antifouling technology. The present invention adopts a simple self-assembly system as the main body of the coating, uses PAA and PAH layer-by-layer self-assembly as the substrate, designs a micro-nano structure to reduce the loss of lubricating oil, introduces D-cysteine ​​and nano-silver particles for synergistic sterilization, and forms a triple synergistic system of "difficult to adsorb, easy to disperse, and strong sterilization", which not only greatly reduces the use of bactericides, but also gives the coating the function of actively dispersing biofilms, solves the problems faced by existing ultra-slip coatings, greatly inhibits the formation of marine biological fouling, and provides a way for the development of efficient antifouling coatings in marine engineering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of marine antifouling, and particularly relates to an ultra-slip antifouling coating with synergistic functions of dispersing and killing fouling organisms and a preparation method thereof. Background Art

[0002] Marine biofouling is the phenomenon of excessive reproduction and spread of harmful organisms in the marine ecosystem due to human activities. It not only has serious negative impacts on many aspects of human life, but also has great harm to the maintenance of marine ecological balance. Among the many anti-fouling technologies, anti-fouling coating is one of the most effective and feasible methods to avoid marine biofouling. Among them, super-slip anti-fouling coatings have attracted continuous attention from researchers due to their low surface energy, low Young's modulus and dynamic lubricating surface.

[0003] Compared with traditional low surface energy coatings, super-slip coatings can significantly prevent the adhesion of marine organisms by constructing a dynamic lubricating surface. However, relying solely on a single dynamic anti-fouling mode, the physical "anti-adhesion" effect is limited, and the static anti-fouling effect is insufficient, which cannot meet the actual needs of marine anti-fouling. On the other hand, the lubricant infused into the super-slip coating is usually a non-polar liquid such as silicone oil, fluoroether or liquid paraffin. Such substances do not have a bactericidal effect and are extremely easy to lose, which greatly limits their application in the actual ocean. At present, it is common to add bactericides to super-slip coatings to improve the bactericidal and anti-fouling effects. However, the use of bactericides can cause bacteria to develop certain drug resistance, and the introduction of such materials cannot fundamentally avoid the attachment of biofilms. It can be concluded that achieving efficient and long-term service of super-slip coatings is the primary problem that needs to be overcome at this stage.

[0004] Super-slip coatings face problems such as easy loss of lubricants, excessive use of bactericides, and easy accumulation of biofilms. How to better fix lubricants, reduce the use of bactericides, and solve the problem of biofilm accumulation is still the focus of current research. Patent CN115895310A discloses a bionic super-slip long-lasting antifouling coating based on a micro-nano porous structure and its preparation method and application. Patent CN113512160A discloses a method for preparing an antifouling surface by grafting organic-inorganic hybrid particles with lubricating oil. However, the antifouling coatings prepared in the above two patents simply use super-slip function to prevent fouling. Such coatings have the same shortcomings: (1) lack of effective antifouling agents and cannot effectively prevent marine biological fouling; (2) cannot prevent lubricating oil loss; (3) cannot fundamentally prevent biofilm attachment.

[0005] Recently, D-amino acids have been shown to play a very important role in the decomposition of bacterial biofilms. Its mechanism of action is to significantly inhibit the growth and metabolism of bacteria on the surface of metal substrates by interfering with the synthesis of proteins and polysaccharides in bacteria, thereby effectively blocking the formation of biofilms from the root. Based on the above mechanism, by fully introducing D-amino acids and related bactericides into super-slip coatings, based on the synergistic effect between D-amino acids and bactericides, it is expected to better exert the real-time antifouling effect of the composite coating and effectively reduce the amount of bactericides. That is, D-amino acids can affect the synthesis of proteins and polysaccharides, thereby affecting the attachment of biofilms and dispersing mature biofilms. Therefore, the synergistic use of bactericides and D-amino acids can effectively improve the antifouling effect and significantly reduce the amount of bactericides. Therefore, the coating prepared using this system is environmentally friendly and can be used as an effective strategy for marine antifouling. The above strategy can provide a new strategy for the development of stronger and more durable antibacterial surfaces, and is expected to achieve the successful preparation of antifouling coatings with triple synergistic effects of difficult adsorption, easy dispersion and strong bactericidal effects. Summary of the invention

[0006] In view of the problems in the prior art, the present invention provides a transparent super-slip anti-fouling coating with synergistic functions of dispersing and killing fouling organisms and a preparation method thereof. The main purpose is to prepare a super-slip marine coating with strong anti-fouling ability by a simple process.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] The preparation of a super-slip anti-fouling coating with the synergistic function of dispersing and killing fouling organisms comprises the following steps:

[0009] Step 1. Preparation of LBL coating: The metal sample is placed in positively charged polydiallyldimethylammonium chloride (PDDA) for pretreatment, and then immersed in negatively charged polyacrylic acid (PAA) and positively charged polyacrylamine hydrochloride (PAH) in sequence. The above process is repeated 4 to 10 times. PAA and PAH react with each other due to electrostatic interaction to form LBL coating, which is then dried.

[0010] Step 2. Preparation of LBL-Ag coating with bactericidal function: Place the dried metal sample with LBL coating in a silver acetate aqueous solution and soak it in water. + Introduced onto the surface of the LBL coating to form an LBL-Ag coating, and then dried;

[0011] Step 3. Prepare a SLIC coating with super-slip function: evenly coat polymethylhydrogensiloxane (PMHS) on the surface of the LBL-Ag coating by spin coating to form a SLIC coating;

[0012] Step 4. Prepare a SLIC-D coating with a dispersing function: place the SLIC coating in a D-cysteine ​​(D-Cys) aqueous solution to cause a S-Ag coordination reaction, and then dry it to finally obtain an ultra-slippery antifouling coating SLIC-D coating with a synergistic function of dispersing and killing fouling organisms.

[0013] In the step 1, the metal sample is surface-polished with 240, 400, 600, 800, or 1000-grit sandpaper, ultrasonically cleaned in a mixed solution of ethanol and acetone for 20 min to 40 min, and then dried.

[0014] In step 1, the concentration of PDDA, PAA and PAH is 1 mg·mL -1 -10mg·mL -1 of aqueous solution.

[0015] In the step 1, each soaking is 10 minutes to 30 minutes. After soaking, ultrapure water is used for washing to remove unreacted residues.

[0016] In the step 1, the metal sample after forming the LBL coating is allowed to stand at 50° C.-80° C. for 10 min-60 min for drying.

[0017] In step 2, the concentration of the silver acetate aqueous solution is 1 mmol·L -1 -10mmol·L -1 .

[0018] In step 2, the soaking time is 1 h to 10 h.

[0019] In the step 2, the drying process is: standing at 50°C-80°C for 10min-60min.

[0020] In step 3, the spin coating volume of PMHS is 1 μL-100 μL, the spin coating speed is slow at first and then fast, the spin coating speed in the first stage is 400 rpm-800 rpm, the spin coating time is 1 s-50 s, and the spin coating speed in the second stage is 800 rpm-1600 rpm, and the spin coating time is 1 s-100 s.

[0021] In the step 3, the spin-coated metal sample is placed at 70° C.-150° C. for 10 min-60 min to form a SLIC coating.

[0022] In step 4, D-cysteine ​​is present at a concentration of 1 mmol·L -1 -10mmol·L -1 Homogeneous aqueous solution.

[0023] In step 4, the reaction time is 1 h to 10 h, and the drying process is: standing at 50° C. to 80° C. for 10 min to 60 min.

[0024] An ultra-slip antifouling coating with synergistic functions of dispersing and killing fouling organisms is prepared by the above method. Based on layer-by-layer self-assembly technology, D-cysteine ​​and nanosilver synergistically kill bacteria, and PMHS is introduced to provide ultra-slip function.

[0025] The coating has a protein resistance of 67.28%-80.27%, a bacteria resistance of 96.64%-97.87%, and an algae resistance of 82.82%-96.03%; the coating has a light transmittance of 86.7%-88.46% at a wavelength of 400nm-800nm, and a bactericidal rate of 96.64%-97.87%; the water contact angle of the coating is 105.6 ° ~108.2 ° , the water sliding angle is 4.2 ° ~9.57 ° .

[0026] Compared with the prior art, the ultra-slip antifouling coating with the synergistic function of dispersing and killing fouling organisms and its preparation method of the present invention have the following beneficial effects:

[0027] The present invention provides an ultra-slip antifouling coating with the synergistic function of dispersing and killing fouling organisms and its preparation, adopts a simple self-assembly system as the main body of the coating, designs a micro-nano structure to reduce the loss of lubricating oil, introduces D-cysteine ​​and nano-silver particles to synergistically prevent fouling, not only greatly reduces the use of bactericides, but also gives the coating the function of actively dispersing biofilms, solving the problems faced by existing ultra-slip coatings. Thus, PAA and PAH are self-assembled layer by layer as the base, D-cysteine ​​and nano-silver particles synergistically kill bacteria, forming a triple synergistic system of "difficult to adsorb, easy to disperse, and strong bactericidal", which can greatly inhibit the formation of marine biofouling.

[0028] The present invention studies the surface morphology, the wettability of water on the coating surface and the antibacterial effect by adjusting the number of self-assembly layers. The PDDA used in the pretreatment has good universality, so that the coating can be applied on different substrates such as metal and glass. Negatively charged PAA and positively charged PAH attract each other through electrostatic interaction and grow layer by layer on the sample surface. The overall electrical neutrality of the coating reduces the adhesion of microorganisms caused by charge interaction. Silver ions can coordinate with the amino groups on PAH and be firmly fixed on the coating surface. The slowly released silver ions destroy the biofilm of microorganisms, enter the cells to cause the cell contents to overflow, interfere with the cell metabolism process and the action of various enzymes, thereby causing the cells to lose their physiological functions and die. PMHS contains active Si-H bonds in its molecular structure, so it can participate in a variety of chemical reactions and has good film-forming properties, which can make the coating surface have good hydrophobic effect, large contact angle and durability. PMHS is evenly spread on the coating surface by spin coating. Under high temperature, silver ions and Si-H in PMHS undergo redox reaction to generate Si-OH, and then dehydrate and condense to form a spatial structure, which can provide a good coating for silver and achieve a slow-release effect. The coating is hydrophobic as a whole and has a strong self-cleaning function. The oil layer formed on the coating surface effectively blocks the direct contact of microorganisms and reduces the attachment of microorganisms. The S element in D-cysteine ​​can undergo a synergistic coordination reaction with silver, thereby fixing it on the super-slip coating. The presence of D-cysteine ​​can not only participate in the decomposition process of biofilms, such as interfering with the function of bacterial cell walls, regulating protein synthesis, regulating bacterial mobility and adhesion, but also participate in the metabolism of other substances in bacteria. It is often used as a natural synergist to improve the efficacy of fungicides and reduce their dosage for eliminating biofilms. D-cysteine ​​can decompose biofilms well, causing bacteria to change from a fixed state to a free state, making it easier to kill. The synergistic effect with fungicides can not only improve the antifouling effect but also significantly reduce the dosage of fungicides.

[0029] Based on this, this ultra-slip coating that prevents marine biofouling is stable, durable, universal and efficient, providing a way to develop efficient antifouling coatings in marine engineering. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 1 is a graph showing the coating thickness results obtained in different steps of Example 1 of the present invention.

[0031] Figure 2 This is a graph showing the transmittance results of the SLIC-D coating obtained in Example 1 of the present invention.

[0032] Figure 3 It is a schematic diagram of the microstructure of the coating surface obtained in different steps of Example 1 of the present invention.

[0033] Figure 4It is the infrared spectra of the coatings obtained in different steps of Example 1 of the present invention.

[0034] Figure 5 3 is the distribution diagram of Ag, Si and S elements in the SLIC-D coating prepared in Example 1 of the present invention.

[0035] Figure 6 This is a three-dimensional reconstruction of the Ag, Si and S elements in the SLIC-D coating obtained in Example 1 of the present invention.

[0036] Figure 7 Graph showing contact angle and sliding angle results of the coatings obtained in different steps of Example 1 of the present invention.

[0037] Figure 8 This is a microscopic protein-resistant image of the SLIC and SLIC-D coatings prepared in Example 1 of the present invention.

[0038] Fig. 9 It is a graph showing the changes in the colony counts of Escherichia coli and Staphylococcus aureus of the coatings prepared in different steps of Example 1 of the present invention and the comparative example.

[0039] Fig.10 This is a graph showing the effect of the coating prepared in different steps of Example 1 of the present invention on the biofilm thickness of Escherichia coli and Staphylococcus aureus.

[0040] Fig.11 This is a test diagram of the anti-algae performance of the coating prepared in different steps of Example 1 of the present invention.

[0041] Fig.12 This is a contact angle variation diagram of the super-slip antifouling coating obtained in Examples 1 to 4 of the present invention and Comparative Example 1.

[0042] Fig.13 This is a graph showing the sliding angle changes of the super-slip anti-fouling coatings obtained in Examples 1 to 4 of the present invention and Comparative Example 1. DETAILED DESCRIPTION

[0043] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention application are described in detail below in conjunction with the accompanying drawings and preferred embodiments. In the following description, different "one embodiment" or "embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures, or characteristics in one or more embodiments may be combined in any suitable form.

[0044] The experimental methods for which specific conditions are not specified in the examples of the present invention are usually carried out under conventional conditions, such as those described in textbooks and experimental guides, or under conditions recommended by manufacturers, which are well known or easily known to ordinary technicians in the field. The following examples are only preferred embodiments of the present invention and do not limit the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

[0045] The present invention provides a method for preparing an ultra-slip antifouling coating having a synergistic function of dispersing and killing fouling organisms, comprising:

[0046] Step 1. Preparation of LBL coating: The metal sample was surface-polished with 240, 400, 600, 800, and 1000 grit sandpaper, ultrasonically cleaned in a mixed solution of ethanol and acetone for 20 min-40 min, and then dried. It was placed in positively charged polydiallyldimethylammonium chloride (PDDA) for pretreatment, and then immersed in negatively charged polyacrylic acid (PAA) and positively charged polyacrylamine hydrochloride (PAH) in turn, each time for 10 min-30 min. After immersion, it was washed with ultrapure water to remove unreacted residues; the above process was repeated 4 to 10 times, and PAA and PAH reacted with each other due to electrostatic interaction to form an LBL coating, and then it was allowed to stand at 50°C-80°C for 10 min-60 min for drying; wherein, the concentrations of PDDA, PAA, and PAH were all 1 mg·mL -1 -10mg·mL -1 of aqueous solution.

[0047] Step 2. Preparation of LBL-Ag coating with bactericidal function: The metal sample with LBL coating was exposed to a concentration of 1 mmol·L -1 -10mmol·L -1 Soak in silver acetate aqueous solution for 1h-10h; + Introduced into the surface of the LBL coating to form an LBL-Ag coating, and then allowed to stand at 50°C-80°C for 10min-60min.

[0048] Step 3. Prepare a SLIC coating with super-slip function: evenly coat polymethylhydrogensiloxane (PMHS) on the surface of the LBL-Ag coating by spin coating, and then let it stand at 70℃-150℃ for 10min-60min to form a SLIC coating; wherein, the spin coating volume is 1μL-100μL, the spin coating speed is slow at first and then fast, the first stage spin coating speed is 400rpm-800rpm, and the spin coating time is 1s-50s; the second stage spin coating speed is 800rpm-1600rpm, and the spin coating time is 1s-100s.

[0049] Step 4. Preparation of SLIC-D coating with dispersibility: The SLIC coating was placed in a concentration of 1 mmol·L -1 -10mmol·L -1 The mixture is placed in an aqueous solution of D-cysteine ​​(D-Cys) for 1h~10h, a S-Ag coordination reaction occurs, and after drying at 50℃-80℃, it is allowed to stand for 10min-60min to obtain an ultra-slip anti-fouling coating with synergistic functions of dispersing and killing fouling organisms.

[0050] The present invention is based on layer-by-layer self-assembly technology, D-cysteine ​​and nanosilver synergistically kill bacteria, and PMHS is introduced to provide super-slip function, to obtain SLIC-D super-slip transparent coating with triple synergistic effects of difficult adsorption, easy dispersibility, and strong bactericidal effect. The coating has a protein resistance of 67.28%-80.27%, a bacterial resistance of 96.64%-97.87%, and an algae resistance of 82.82%-96.03%, and has excellent resistance to microbial fouling. The water contact angle of the coating is 105.6 ° ~108.2 ° , the water sliding angle is 4.2 ° ~9.57 ° The light transmittance of the coating at a wavelength of 400nm-800nm ​​is 86.7%~88.46%, and the bactericidal rate of the coating is 96.64%~97.87%, which provides a way to develop high-efficiency antifouling coatings in marine engineering.

[0051] In the embodiments and comparative examples of the present invention, the preparation process of the silver acetate aqueous solution is as follows: 0.01 g to 0.1 g of silver acetate is added to ultrapure water, and continuous magnetic stirring is performed for 10 min to 60 min until a concentration of 1 mmol·L is formed. -1 -10mmol·L -1 The preparation method of the PDDA, PAA and PAH aqueous solutions is as follows: 100 μL-1000 μL PDDA, 0.01 g-0.2 g PAA and 0.01 g-0.2 g PAH are added to ultrapure water respectively, and continuous magnetic stirring is performed for 30 min until a concentration of 1 mg·mL is formed. -1 -10mg·mL -1 Homogeneous aqueous solution.

[0052] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments:

[0053] Embodiment 1:

[0054] This embodiment provides a preparation method for a transparent super-slip antifouling coating with a synergistic function of dispersing and killing fouling organisms. Based on the layer-by-layer self-assembly technology, D-cysteine ​​and nanosilver synergistically kill bacteria, and PMHS is introduced to provide a super-slip function, thereby obtaining a SLIC-D super-slip transparent coating with a triple synergistic effect of difficult adsorption, easy dispersibility, and strong bactericidal effect, including the following preparation steps:

[0055] Step 1, preparation of LBL coating: 316L stainless steel was surface-polished with 240, 400, 600, 800, and 1000 grit sandpaper, ultrasonically cleaned in a mixed solution of ethanol and acetone for 20 min-40 min, and then dried to serve as the substrate material. The treated substrate material was placed in a polydiallyldimethylammonium chloride (PDDA) solution (100 mL 1 mg mL -1 -10mg·mL -1 ) for 10-30 min. Then the pretreated substrate material was immersed in polyacrylic acid (PAA) (100 mL 1 mg mL -1 -10mg·mL -1 ) and polyacrylamine hydrochloride (PAH) solution (100 mL 1 mg mL -1 -10mg·mL -1 ) for 10min-30min and repeated six times, wherein the unreacted residue was washed away with ultrapure water after each immersion, PAA and PAH formed a zwitterionic coating LBL coating through electrostatic action, and then stood at 50℃-80℃ for 10min-60min for drying.

[0056] Step 2, preparation of LBL-Ag coating: Place the dried 316L stainless steel with LBL coating in a silver acetate solution (100 mL 1 mmol·L -1 -10mmol·L -1 ) within 1h-10h, the silver ions coordinated with the amine groups in PAH to form a hollow structure to obtain the LBL-Ag coating, which was then allowed to stand at 50℃-80℃ for 10min-60min.

[0057] Step 3, preparation of SLIC coating: Spin coating 10μL-60μL of polymethylhydrogensiloxane (PMHS) liquid evenly on the sample surface, the spin coating speed is slow at first and then fast, the first stage is 400rpm-800rpm for 1s-50s, and the second stage is 800rpm-1600rpm for 1s-100s. The spin-coated sample is placed at 70℃-150℃ for 10min-60min, and the silver ions and Si-H in PMHS undergo redox reaction to generate Si-OH, which then dehydrates and condenses to form a spatial structure to obtain the SLIC coating.

[0058] Step 4, preparation of SLIC-D coating: The SLIC coating was placed in a D-cysteine ​​solution (100 mL 1 mmol·L -1 -10mmol·L -1 ) for 1h-10h, S-Ag coordination reaction occurs, and then it is allowed to stand at 60°C for 10min-60min to obtain an ultra-slip anti-fouling coating SLIC-D coating with synergistic function of dispersing and killing fouling organisms.

[0059] Embodiment 2~4:

[0060] The preparation methods of Examples 2 to 4 are the same as those of Example 1, except that when preparing the LBL coating in step 1 in Examples 2 to 4, the number of repetitions is 4, 8, and 10, respectively.

[0061] Comparative Example 1:

[0062] This comparative example is the same as Example 1, except that: when preparing the LBL coating in step 1 in this comparative example, the number of repetitions is 2 times.

[0063] Comparative Example 2:

[0064] This comparative example is the same as Example 1, except that in step 4, the SLIC coating is placed in L-cysteine ​​of the same concentration to obtain a SLIC-L coating.

[0065] Comparative Example 3:

[0066] This comparative example is the same as Example 1, except that the substrate material is replaced by glass instead of 316L stainless steel.

[0067] In order to solve the existing problems of ultra-slippery coatings, the present invention introduces D-cysteine ​​as a biofilm dispersant, which works synergistically with a bactericide to prepare a SLIC-D coating with triple synergistic effects of difficult adsorption, easy dispersibility, and strong bactericidal properties, giving the ultra-slippery coating a better anti-fouling effect. First, PDDA (100μL-1000μL), PAA (0.01g-0.2g), and PAH (0.01g-0.2g) were dissolved in ultrapure water for 30 minutes under magnetic stirring to form a uniform solution. The sample was pretreated with PDDA solution for 10min-30min, and then the sample was repeatedly immersed in PAA and PAH solutions for six times. PAA and PAH self-assembled layer by layer through electrostatic interactions to prepare an LBL coating. Afterwards, the 316L stainless steel coated with the LBL coating was immersed in 100mL 1mmol·L -1 -10mmol·L -1The excess silver acetate solution was left to stand for 1h-10h to form a coordinated cross-linked structure. Thus, the LBL-Ag coating with bactericidal function was successfully prepared. Silicone oil was evenly spread on the LBL-Ag coating by spin coating. Under high temperature conditions, redox reaction and shrinkage polymerization occurred to prepare the SLIC coating with super-slippery function. Finally, the SLIC coating was immersed in 100mL 1mmol·L -1 -10mmol·L -1 The S-Ag coordination reaction was carried out by using D-cysteine ​​solution to prepare a SLIC-D coating with the function of dispersing biofilm.

[0068] In order to verify the successful coating on the surface of 316L stainless steel, the thickness of the coating prepared in different steps in Example 1 was analyzed by ellipsometer. The results are as follows: Figure 1 As shown in the figure, after layer-by-layer self-assembly, the thickness of the LBL coating is 107nm. After the surface is immersed in silver acetate solution, the coating thickness increases to 154nm. After PMHS treatment, the coating thickness increases by 64nm. The gradual increase in thickness further proves the success of the experiment. The thickness of SLIC-D is determined to be about 351nm using ellipsometry.

[0069] In order to characterize the transparency of the prepared coating, the light transmittance of the coating prepared in Comparative Example 3 was analyzed. Based on the universality of PDDA, SLIC-D has high optical transparency and is suitable for transparent substrates. Figure 2 As shown, the transmittance test results show that the transmittance of the prepared SLIC-D coating in the visible light band is close to that of the glass without modified coating.

[0070] In addition, the surface structure of the coating obtained in different steps of Example 1 was characterized. Figure 3 As shown in the figure. The results show that the surfaces of LBL, LBL-Ag, SLIC and SLIC-D coatings are all flat, among which the root mean square roughness of SLIC coating is lower than that of the other three coatings. This is because PMHS, as a lubricant, fills the surface roughness of the LBL coating. In addition, the lubricant is fixed on the LBL coating with silver ions. The root mean square roughness of SLIC-D is lower than that of SLIC, which may be due to the immobilization of D-amino acids on the coating.

[0071] The chemical structure of the coating in different steps of Example 1 was analyzed, and the results are as follows: Figure 4 shown. Figure 4 The Fourier transform infrared spectroscopy (FTIR) showed that at 800 cm -1 -1200cm -1A broad characteristic peak appeared between the LBL and LBL-Ag, which was attributed to the overlap of Si-N stretching vibration and Si-O stretching vibration. Compared with LBL and LBL-Ag, the broad characteristic peaks of SLIC and SLIC-D shifted significantly, proving that the organic ligands were strongly embedded in the system. Therefore, PMHS formed a gel or reacted with amine groups with silver ions as the reaction center. In summary, the immobilization of the lubricant gel near the surface of the LBL membrane caused the SLIC membrane to exhibit a high degree of slipperiness, even after the non-immobilized lubricant was removed from the membrane. This immobilization can be attributed to the dehydration condensation of Si-OH on the outer surface of the coating, and the oxidation-reduction reaction between Si-H groups and silver ions with NH in the middle of the coating. 2 The groups react.

[0072] The distribution of Ag, Si, and S elements in the SLIC-D coating prepared in Example 1 was analyzed. Figure 5 , Figure 6 As shown. Silver element has slight vacancies on the coating surface, while silicon element maintains high intensity from beginning to end. In contrast, the intensity of S is much lower than that of the other two elements, and with the increase of etching depth, S almost disappears completely. In addition, the sputtering rate of the time-of-flight secondary ion mass spectrometer is about 1nm per second, and the element intensity tends to stabilize after 400s, which is consistent with the data of the ellipsometer.

[0073] The wettability test of the coating obtained in the embodiment and the comparative example was carried out as follows:

[0074] The contact angle of pure water (the contact angle of a 4 μL water droplet) and the sliding angle (the tilt angle required for a 10 μL water droplet to move) were measured by a contact angle meter to evaluate the surface wettability of the coating at different stages of preparation. The sliding properties of the coatings (LBL, LBL-Ag, SLIC, and SLIC-D) obtained at different steps in Example 1 were measured, and the results are shown in Figure 1. Figure 7 As shown in the figure. It can be seen from the figure that the contact angles of the coatings obtained in different steps decrease in the following order: SLIC>SLIC-D>LBL-Ag>LBL. Due to the absence of lubricant, the contact angles of LBL and LBL-Ag films are small, and water droplets will not slide on the films. Due to the effect of D-cysteine, the contact angle of SLIC-D is smaller than that of SLIC, and the sliding angle is larger than that of SLIC. The sliding performance is reduced, but generally it is not much different from SLIC.

[0075] At the same time, the water contact angle and sliding performance of the super-slip antifouling coating obtained by self-assembly preparation of LBL coating were tested for different times. The results are as follows: Fig.12 , Fig.13 As shown in the figure, when the number of repetitions is 4 to 10 times, the water contact angle of the prepared super-slip antifouling coating is 105.6° ~108.2 ° In the range, the sliding angle is 4.2 ° ~9.57 ° When the number of repetitions is 2, although its hydrophobic performance is excellent, its sliding angle reaches 16.7 ° ~21.5 ° , which affects its sliding performance. Therefore, the present application limits the number of repetitions of the LBL coating preparation process to 4 to 10 times, among which the coating with the best performance is obtained by repeating 6 times.

[0076] 18 ° The sliding effect of the SLIC-D coating prepared on different substrates was investigated by adjusting the tilt angle of the droplet. The coatings obtained in Example 1 and Comparative Example 3 showed excellent self-cleaning performance. The results are shown in Table 1. A 10 μL water droplet took 6.97 s and 8.26 s to slide down the inclined surface very quickly on a 316L stainless steel substrate and a glass substrate of the same specification. The tilt angle TA was 18 ° , leaving no trace, indicating that the coating provided by the present invention is applicable to both metal substrates and glass substrates.

[0077] Table 1 Sliding effect of water droplets on SLIC-D coatings prepared on different substrates

[0078] .

[0079] The various stages of biofouling are protein adhesion (film regulation stage), bacterial adhesion (unstable biofilm stage) and algae adhesion (colonization biofilm stage). The antifouling performance of the ultra-slip antifouling coating with the synergistic function of dispersing and killing fouling organisms provided in the embodiments and comparative examples of the present invention was studied to simulate the resistance of the coating to different fouling organisms in various stages of biofouling. Whey, hemoglobin (Hb) and bovine serum albumin (BSA) were used to simulate the film regulation stage; Gram-positive Staphylococcus aureus and Gram-negative Escherichia coli, which are common in marine environments and daily life environments, were used to simulate the unstable bacterial adhesion stage; and Pseudomonas triangularis and Isochrysis chrysotrichum, which are widely distributed in the ocean, were used to simulate the colonization algae adhesion stage. The specific research process is as follows:

[0080] Fouling is a spontaneous process in biological systems, associated with the dynamic adsorption and accumulation of biomolecules on surfaces, which can be directly monitored in real time using a quartz crystal microbalance with dissipation monitoring (QCM-D). The continuous protein resistance of the coating was demonstrated using a fouled SLIC-D coated Au sensor. The adsorption behavior of whey protein (Whey), hemoglobin (Hb), and bovine serum albumin (BSA) on a bare substrate and a SLIC-D coated substrate prepared in Example 1 was quantitatively studied using QCM. The results are shown in Figure 2. Figure 8 As shown, the whey on SLIC-D after washing with water was only 0.17 mg cm -2 , while the whey content on the Au wafer was as high as 0.54 mg cm -2 The Hb on SLIC-D was 1.04 mg cm -2 , while Hb on Au wafer is 5.27 mg·cm -2 The BSA on SLIC-D was 1.04 mg cm -2 , while the dirt on the Au wafer can reach up to 0.34 mg cm -2 This excellent antifouling performance is likely to originate from the surface-anchored PMHS, which provides interfacial hydration and steric hindrance, hindering the initial attachment of foulants on the surface.

[0081] Bacteria play a vital role in the second stage of biofilm construction in marine biofouling. Gram-negative Escherichia coli and Gram-positive Staphylococcus aureus, as typical pathogens or widely present in the marine environment, are used as model bacteria for antimicrobial detection. All materials were sterilized by ultraviolet irradiation for 30 minutes before use. Single colonies of the above bacteria were isolated by the plate streak method, and single colonies of Escherichia coli and Staphylococcus aureus were cultured in LB liquid culture medium at 37°C and 180rpm for 12h-16h to reach the logarithmic growth phase, and the bacterial solution in the logarithmic growth phase was taken for subsequent experiments.

[0082] 316L stainless steel, SLIC-L coating prepared in comparative example 2, and LBL-Ag coating, SLIC coating, and SLIC-D coating in example 1 were co-cultured with bacteria at 37°C for 1 day. After the culture, the sample surface was gently washed with sterile water to remove weakly adhering planktonic bacteria. Bacteria tightly attached to the sample surface were collected, and the antibacterial properties of the samples were evaluated by dilution plate coating method. The results are shown in Fig. 9As shown in the figure, due to the presence of AgNPs, LBL-Ag, SLIC and SLIC-D all showed good bactericidal efficiency (~80%) against static Escherichia coli and Staphylococcus aureus during the 24h immersion process. For both LBL-Ag and SLIC, the slow release of AgNPs will effectively kill the floating bacteria near the metal surface and inhibit their initial reversible adhesion. It can be concluded that the slow-released AgNPs can significantly affect the growth state of floating bacteria in the initial stage. However, after a long period of immersion, the release process of silver nanoparticles is hindered by the consumption of silver and the diffusion of attached dead bacteria, which reduces its release rate. At that time, the still surviving floating bacteria can still easily attach to SLIC and form biofilms. Therefore, both of the above coatings failed to achieve a truly long-term antifouling effect. For the SLIC-D coating, the presence of D-Cys significantly inhibited the formation of biofilms from the root and effectively maintained the floating state of bacterial cells, which will be more conducive to the bactericidal effect of AgNPs. The antibacterial effect of the control group SLIC-L was significantly poor. Therefore, the antibacterial effect of SLIC-D was the best.

[0083] The 316L stainless steel and the SLIC coating and SLIC-D coating samples prepared in Example 1 were co-cultured with bacteria at 37°C for 4 days. After the culture, the sample surface was gently washed with sterile water to remove weakly adhering planktonic bacteria. The cell viability in the biofilm was evaluated using the LIVE / DEAD BacLight bacterial viability kit. The biofilm was stained with SYTO9 and PI dyes for 20 min in the dark and stained with E x / E m =488 / 559nm CLSM visualization. Cell viability was further evaluated by LIVE / DEADBacLight bacterial viability kit. Fig.10 As shown. STYO9 can penetrate all cell membranes and bind to DNA, showing green fluorescence under a confocal laser scanning microscope. Propidium iodide (PI) can only penetrate damaged cell membranes and show red fluorescence. Cell viability is described by analyzing the red / green fluorescence intensity. The SLIC-D coating showed the highest amount of red fluorescence and the lowest biofilm thickness, and was evenly distributed, showing severe cell damage, while almost no red fluorescence was observed on the surface of 316L stainless steel, indicating that the metal sample itself has weak antibacterial ability. In the SLIC coating, red fluorescence exists, but aggregation occurs at the same time, indicating that the presence of D-cysteine ​​effectively disperses the biofilm.

[0084] Algae are a key component of irreversible biofilms in the process of marine pollution. The full wavelength absorption of algae is determined by UV-vis spectroscopy, and all algae have a characteristic absorption peak at 440nm.440 To evaluate the amount of algal cells attached to the sample. All materials were sterilized by ultraviolet irradiation for 30 min before use. Phaeochromis tricornutum and Isochrysis chrysogenum were used as experimental algae. F / 2 medium and F / 2+Si medium were used for cultivation and cultured at 20°C with visible LED irradiation (3000LUX) for 7 days. The algal solution was collected and diluted to 10 5 cell·mL -1 , used in subsequent experiments. The full wavelength absorption of algae was determined by UV-visible spectroscopy. The absorbance of algae at different concentrations at the maximum absorbance of 440nm was measured, and a standard curve was drawn. The sample was soaked in 2mL of diluted algae solution for 7 days, and then gently washed with PBS solution to remove weakly adhered algae. The absorbance at 440nm was measured to characterize the adhesion of algae on the sample surface. The SLIC coating, SLIC-D coating and 316L stainless steel prepared in Example 1 were tested using the above method, and the results are shown in the figure. Fig.11 As shown in the figure, the concentration of algae attached to the SLIC-D coating is lower than that of 316L stainless steel and SLIC coating, indicating that the SLIC-D coating significantly enhances the anti-algae ability through weak adhesion, more stable super-slippery structure, cell damage and content leakage, giving the SLIC-D coating efficient antifouling performance.

[0085] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. Preparation of an ultra-slip antifouling coating with synergistic functions of dispersing and killing fouling organisms, characterized in that: The following steps are involved: Step 1. Preparation of LBL coating: The metal sample is placed in positively charged polydiallyldimethylammonium chloride (PDDA) for pretreatment, and then immersed in negatively charged polyacrylic acid (PAA) and positively charged polyacrylamine hydrochloride (PAH) in sequence. The above process is repeated 4 to 10 times. PAA and PAH react with each other due to electrostatic interaction to form an LBL coating, which is then dried. Step 2. Preparation of LBL-Ag coating with bactericidal function: Place the metal sample with LBL coating after drying in a silver acetate aqueous solution and use the immersion method to + Introduced onto the surface of the LBL coating to form an LBL-Ag coating, and then dried; Step 3. Prepare a SLIC coating with super-slip function: evenly coat polymethylhydrogensiloxane PMHS on the surface of the LBL-Ag coating by spin coating to form a SLIC coating; Step 4. Prepare a SLIC-D coating with a dispersing function: place the SLIC coating in a D-cysteine ​​D-Cys aqueous solution to cause a S-Ag coordination reaction, and then dry it to finally obtain an ultra-slippery antifouling coating SLIC-D coating with a synergistic function of dispersing and killing fouling organisms.

2. The preparation of an ultra-slip antifouling coating having a synergistic function of dispersing and killing fouling organisms according to claim 1, characterized in that: In step 1, the metal sample is surface-polished with 240, 400, 600, 800, and 1000 grit sandpaper, ultrasonically cleaned in a mixed solution of ethanol and acetone for 20 min to 40 min, and then dried; PDDA, PAA, and PAH were all at a concentration of 1 mg mL -1 -10mg·mL -1 Aqueous solution of Soak for 10-30 minutes each time. After soaking, wash with ultrapure water to remove unreacted residues. The metal sample after the LBL coating is formed is allowed to stand at 50°C-80°C for 10min-60min for drying.

3. The preparation of the ultra-slip antifouling coating having the synergistic function of dispersing and killing fouling organisms according to claim 1, characterized in that: In step 2, the concentration of the silver acetate aqueous solution is 1 mmol·L -1 -10mmol·L -1 ; The soaking time is 1h-10h; the drying process is: standing at 50℃-80℃ for 10min-60min.

4. The preparation of an ultra-slip antifouling coating having a synergistic function of dispersing and killing fouling organisms according to claim 1, characterized in that: In step 3, the spin coating volume of PMHS is 1 μL-100 μL; The spin coating speed is slow at first and then fast. The spin coating speed in the first stage is 400rpm-800rpm, and the spin coating time is 1s-50s. The spin coating speed in the second stage is 800rpm-1600rpm, and the spin coating time is 1s-100s.

5. The preparation of the ultra-slip antifouling coating having the synergistic function of dispersing and killing fouling organisms according to claim 1, characterized in that: In step 3, the spin-coated metal sample is placed at 70° C.-150° C. for 10 min-60 min to form a SLIC coating.

6. The preparation of the ultra-slip antifouling coating with the synergistic function of dispersing and killing fouling organisms according to claim 1, characterized in that: In step 4, the D-cysteine ​​aqueous solution has a concentration of 1 mmol·L -1 -10mmol·L -1 Homogeneous aqueous solution.

7. The preparation of the ultra-slip antifouling coating with the synergistic function of dispersing and killing fouling organisms according to claim 1, characterized in that: In step 4, the reaction time is 1 h to 10 h, and the drying process is: standing at 50° C. to 80° C. for 10 min to 60 min.

8. An ultra-slip antifouling coating with a synergistic function of dispersing and killing fouling organisms, prepared by the method according to any one of claims 1 to 7, characterized in that: Based on the layer-by-layer self-assembly technology, D-cysteine ​​and nanosilver synergistically kill bacteria, while PMHS is introduced to provide super-slippery function.

9. The ultra-slip antifouling coating with the synergistic function of dispersing and killing fouling organisms according to claim 8, characterized in that: The coating has a protein resistance of 67.28%-80.27%, a bacteria resistance of 96.64%-97.87%, and an algae resistance of 82.82%-96.03%; the coating has a light transmittance of 86.7%-88.46% at a wavelength of 400nm-800nm, and a bactericidal rate of 96.64%-97.87%; the water contact angle of the coating is 105.6 ° ~108.2 ° , the water sliding angle is 4.2 ° ~9.57 ° .

Citation Information

Patent Citations

  • Method for preparing antifouling surface from organic-inorganic hybrid particle grafted lubricating oil

    CN113512160A

  • Bionic super-lubricity long-acting antifouling coating based on micro-nano porous structure as well as preparation method and application of bionic super-lubricity long-acting antifouling coating

    CN115895310A

  • Bionic coating for preventing marine organism fouling and preparation method thereof

    CN117264470A