Ash removal method of coal-based asphalt and refined asphalt prepared by ash removal method
Coal-based pitch is processed through a two-stage refining method combined with solvents with different hydrogen-to-carbon ratios, achieving efficient deashing under mild conditions, solving the problems of high ash content, low yield and residual impurities in the existing technology, and preparing high-quality Quality refined asphalt and binder asphalt.
Patent Information
- Application Number
- CN202310460945.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-10-29
AI Technical Summary
The existing coal liquefied asphalt deashing process has problems such as high ash content, low yield, high equipment requirements and residual impurities, making it difficult to achieve deep deashing under mild conditions.
A two-stage refining method is adopted. First, the first solvent with a low hydrogen carbon ratio is used to dissolve the coal-based pitch, and then the second solvent with a high hydrogen carbon ratio is used for flocculation reaction and separation. The solvent is recovered through vacuum distillation to achieve an ash content of less than 100 ppm and quinine content. Preparation of refined asphalt with pholine insoluble matter content less than 0.1%, and co-production of binder asphalt with ash content less than 0.1% and quinoline insoluble matter content less than 1%.
It improves the yield and quality of asphalt, reduces ash and impurity residues, has mild process conditions, low equipment requirements, and is suitable for industrial applications.
Smart Images

Figure CN118853218A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of asphalt refining, and in particular relates to a deashing method for coal-based asphalt and refined asphalt obtained therefrom. Background Art
[0002] The residue from direct coal liquefaction is mainly composed of inorganic and organic matter, of which the organic matter includes heavy liquefied oil, asphalt and unconverted coal. Inorganic matter includes minerals in coal and added catalysts. The content of heavy liquefied oil and asphalt in organic matter accounts for about 50% of the residue, unconverted coal accounts for about 30%, and ash accounts for about 20%. Therefore, it is feasible to separate about 50% of the asphalt and heavy oil in the residue for comprehensive processing and utilization, and to extract or prepare more valuable products from them.
[0003] The asphalt substances contained in the direct coal liquefaction residue need to be further deashed before they can be converted into applicable asphalt products. For example,
[0004] Patent document CN109575974A discloses a method for efficient deashing of coal liquefaction residue, which adopts a two-stage static sedimentation method to remove the ash content of coal liquefaction residue to less than 100 ppm; although this method can effectively reduce the ash content in liquefied asphalt, the separation sedimentation temperature is relatively high (up to 200-280°C), and an aqueous solution of flocculants such as polyacrylamide and polyaluminum chloride needs to be added during the second-stage separation, which will cause the operating pressure of the separation device to be relatively high, polyacrylamide and the like are easily decomposed, polyaluminum chloride is easily hydrolyzed, and flocculants are easily left in the deashed asphalt product, thereby affecting the quality of the asphalt product, and the asphalt yield is relatively low.
[0005] Patent document CN103509576A discloses a method for separating unaffected organic matter from coal direct liquefaction residue. A chemical deashing method is used to combine acid washing and alkaline washing to reduce the inorganic matter content in the direct liquefaction residue from 26.1% to 6.2%. Although some surfactants or alcohol substances are added to the acid / alkaline solution to accelerate the sedimentation step, the number of acid / alkaline washings is large during the entire process, the amount of acid / alkaline used is large, the reaction temperature is high and the reaction time is long.
[0006] Patent document CN105754630A discloses a method for preparing coal liquefied asphalt. The method adopts solvent extraction combined with molecular distillation method, and uses solvent extraction method to obtain extracted asphalt light liquid. After recovering the solvent, it is refined by molecular distillation method to prepare refined liquefied asphalt with an ash content of 100 to 500 ppm; however, the molecular distillation process used in this method needs to be carried out under high vacuum and high temperature, so the equipment and process requirements are relatively high, and the ash content in the product is also relatively high.
[0007] Patent document CN108192650A discloses a method for preparing ultra-low ash asphalt. The patent first heat-condenses the asphalt raw material into intermediate spheres, removes the intermediate phase spheres and other insoluble matter by melting or solution filtration, and then evaporates the solvent to obtain purified asphalt with an ash content of less than 20 ppm; although the product obtained by this process has a low ash content, this method has high requirements on the control accuracy of the reaction process conditions, and the product yield is low.
[0008] In view of this, how to further improve the deashing process of coal liquefaction asphalt and produce refined asphalt with high product yield and low ash content is a direction worthy of research. Summary of the invention
[0009] The purpose of the present invention is to provide a deashing method for reducing the ash content and quinoline insoluble matter in coal-based asphalt in response to the problems existing in the existing coal liquefaction asphalt deashing process, so as to obtain refined asphalt with ultra-low ash content for use in the subsequent preparation of carbon materials such as mesophase asphalt, needle coke, carbon fiber, foamed carbon, electrode materials, etc.; the deashing method can perform deep deashing under mild conditions, improve the deashing effect, and increase the yield of the obtained refined asphalt; and, while being able to produce refined asphalt with an ash content of less than 100 ppm and a quinoline insoluble matter content of less than 0.1%, it can also co-produce a binder asphalt with an ash content of less than 0.1% and a quinoline insoluble matter content of less than 1%.
[0010] In a first aspect, a method for deashing coal-based asphalt is provided, comprising the following steps:
[0011] i. Coal-based asphalt is used as the raw material to be treated, and a first solvent is added to the mixture and fully dissolved to obtain an extract; the mass ratio of the first solvent to the coal-based asphalt is (0.5-4):1 (for example, 0.8:1, 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1); the first solvent is a coal tar fraction or a coal direct liquefaction oil fraction, and its distillation range is between 180 and 300° C. (for example, 180-280° C., 190-300° C., 200-250° C., 260-280° C.) and H / C=0.6-1.0 (n / n), for example, 0.7, 0.8, 0.9;
[0012] ii. The extract obtained in step i is mixed with a second solvent in a mass ratio of 1:(1-4) (for example, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5) and then subjected to flocculation reaction to obtain a suspension; the second solvent is one or more of naphtha, coal indirect liquefaction light oil, coal coking light oil, coal direct liquefaction light oil, petroleum ether and mixed benzene, and its distillation range is between 70-160° C. (for example, 80-160° C., 70-140° C., 120-160° C.) and H / C=1.1-2.3 (n / n), for example, 1.2, 1.4, 1.5, 1.6, 1.8, 2.0, 2.2;
[0013] Then, the suspension is centrifuged or subjected to natural sedimentation separation to obtain a heavy phase and a light phase;
[0014] iii. recovering the solvent from the heavy phase obtained in step ii to obtain heavy asphalt, and optionally mixing the recovered solvent into the light phase;
[0015] The second solvent and the first solvent in the light phase are recovered separately to obtain refined asphalt with an ash content of less than 100 ppm (e.g., 1 ppm, 4 ppm, 10 ppm, 20 ppm, 50 ppm, 80 ppm) and a quinoline insoluble matter content of less than 0.1 wt% (e.g., 0.001 wt%, 0.005 wt%, 0.01 wt%, 0.04 wt%, 0.06 wt%, 0.08 wt%).
[0016] The heavy phase obtained in step ii can be subjected to solvent recovery by vacuum distillation; the operation process of recovering the solvent by vacuum distillation is a conventional operation in the art, for example, the mixed solvent (a mixture of the first solvent and the second solvent) is recovered by vacuum distillation at 250°C and -0.08MPa (gauge pressure) for recycling. Also, the second solvent and the first solvent in the obtained light phase are recovered separately, for example, it can be understood that the light phase obtained in step ii is first subjected to atmospheric distillation to recover the second solvent, and the recovered second solvent can be recycled in step ii, and then subjected to vacuum distillation to recover the first solvent, and the recovered first solvent can be recycled in step i; for example, the obtained light phase is first flashed at 180°C and atmospheric pressure to remove the second solvent and reuse it, and then the first solvent is recovered by vacuum distillation at 250°C and -0.08MPa (gauge pressure) and reused, and ultra-low ash refined asphalt is obtained at the bottom of the distillation kettle.
[0017] According to the deashing method provided by the present invention, by adding a step of separating the extract, while being able to produce a refined asphalt with an ash content of less than 100 ppm and a quinoline insoluble content of less than 0.1%, it is also possible to co-produce a binder asphalt with an ash content of less than 0.1% and a quinoline insoluble content of less than 1%. In some embodiments, the deashing method comprises the following steps:
[0018] i. Coal-based asphalt is used as the raw material to be treated, and a first solvent is added to the mixture and fully dissolved to obtain an extract; the mass ratio of the first solvent to the coal-based asphalt is (0.5-4):1 (for example, 0.8:1, 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1); the first solvent is a coal tar fraction or a coal direct liquefaction oil fraction, and its distillation range is between 180 and 300° C. (for example, 180-280° C., 190-300° C., 200-250° C., 260-280° C.) and H / C=0.6-1.0 (n / n), for example, 0.7, 0.8, 0.9;
[0019] The obtained extract is then centrifuged or subjected to natural sedimentation separation to obtain a first heavy phase and a first light phase; the first heavy phase is then subjected to reduced pressure distillation to recover the first solvent to obtain heavy asphalt;
[0020] ii. The first light phase separated in step i is mixed with a second solvent in a mass ratio of 1:(1-4) (for example, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5) and then subjected to flocculation reaction to obtain a suspension; the second solvent is one or more of naphtha, coal indirect liquefaction light oil, coal coking light oil, coal direct liquefaction light oil, petroleum ether and mixed benzene, and its distillation range is between 70-160° C. (for example, 80-160° C., 70-140° C., 120-160° C.) and H / C=1.1-2.3 (n / n), for example, 1.2, 1.4, 1.5, 1.6, 1.8, 2.0, 2.2;
[0021] Then, the suspension is centrifuged or subjected to natural sedimentation separation to obtain a second heavy phase and a second light phase;
[0022] iii. After solvent recovery of the second heavy phase separated in step ii, a binder asphalt having an ash content of less than 0.1wt% (e.g., 0.001wt%, 0.005wt%, 0.01wt%, 0.04wt%, 0.06wt%, 0.08wt%) and a quinoline insoluble content of less than 1wt% (e.g., 0.01wt%, 0.05wt%, 0.1wt%, 0.4wt%, 0.6wt%, 0.8wt%) is obtained, and the recovered solvent is optionally mixed into the second light phase;
[0023] The second solvent and the first solvent in the second light phase are recovered separately to obtain refined asphalt with an ash content of less than 100 ppm (e.g., 1 ppm, 4 ppm, 10 ppm, 20 ppm, 50 ppm, 80 ppm) and a quinoline insoluble matter content of less than 0.1 wt% (e.g., 0.001 wt%, 0.005 wt%, 0.01 wt%, 0.04 wt%, 0.06 wt%, 0.08 wt%).
[0024] In step i of the above method, the operation process of recovering the solvent from the first heavy phase by vacuum distillation is a conventional operation in the art, for example, the first solvent is recovered by vacuum distillation at 250°C and -0.08MPa (gauge pressure) for recycling. The obtained heavy asphalt can be discharged from the system and used as a product.
[0025] In step iii of the above method, the second heavy phase can be subjected to vacuum distillation to recover the solvent, and the operation process is a conventional operation in the art, for example, vacuum distillation is performed at 250°C and -0.08MPa (gauge pressure) to recover the mixture of the first solvent and the second solvent in the second heavy phase. The light liquid phase (i.e., the mixture of the first solvent and the second solvent) obtained after vacuum distillation can be directly mixed into the second light phase (supernatant liquid) separated in step ii, and the binder asphalt is obtained at the bottom of the distillation kettle.
[0026] In step iii of the method described above, the second light phase (supernatant liquid) can first be subjected to atmospheric distillation to recover the second solvent, and the recovered second solvent can be entered into step ii for recycling, and then subjected to reduced pressure distillation to recover the first solvent, and the recovered first solvent can be entered into step i for recycling; for example, the obtained second light phase (supernatant liquid) is first subjected to flash distillation at 180°C and atmospheric pressure to remove the second solvent and reuse it, and then subjected to reduced pressure distillation at 250°C and -0.08MPa (gauge pressure) to recover the first solvent and reuse it, and ultra-low ash refined asphalt is obtained at the bottom of the distillation kettle.
[0027] In some embodiments, in step i, before separating the extract, a mixture of a sedimentation aid and a wetting agent and / or activated clay is added to the extract.
[0028] In some embodiments, the sedimentation aid is an aqueous solution containing 1-10wt% (e.g., 2wt%, 4wt%, 5wt%, 8wt%) of flocculant; preferably, the flocculant is selected from one or more of polyacrylamide, polyaluminum chloride, polyaluminum sulfate, polyferric chloride and polyferric sulfate.
[0029] In some embodiments, the wetting agent is selected from one or more of ethanol, 1-pentanol, 1-octanol, ethylene glycol, and glycerol.
[0030] In some embodiments, before separating the extract, activated clay is added to the extract, and the amount of activated clay added is 0.1-1 wt% (eg, 0.2 wt%, 0.4 wt%, 0.5 wt%, 0.8 wt%) based on the mass of coal-based asphalt.
[0031] In some embodiments, the process conditions for adding activated clay to the extract for mixing include: mixing temperature of 80-140°C (e.g., 90°C, 100°C, 120°C), and mixing time of 10-60 min (e.g., 15 min, 30 min, 40 min, 50 min).
[0032] In some embodiments, before separating the extract, a mixture of a sedimentation aid and a wetting agent is added to the extract and mixed;
[0033] The process conditions for adding the mixture formed by the sedimentation aid and the wetting agent and mixing include: a mixing temperature of 80-140° C. (e.g., 90° C., 100° C., 120° C.), stirring and mixing for 0.2-5 min (e.g., 0.4 min, 1 min, 2 min, 4 min) at a stirring speed of 3000-8000 r / min (e.g., 3500 r / min, 4000 r / min, 5000 r / min, 6000 r / min, 7000 r / min), and then stirring and mixing for 30-180 min (e.g., 40 min, 60 min, 100 min, 120 min, 150 min) at a stirring speed of 50-500 r / min (e.g., 60 r / min, 100 r / min, 200 r / min, 300 r / min, 400 r / min). The mixing process can be carried out in a homogenizer or a colloid mill.
[0034] In some embodiments, the amount of the sedimentation aid added is 2-10% (e.g., 3%, 4%, 5%, 8%) of the extract, and the amount of the wetting agent added is 0.1-0.5% (e.g., 0.2%, 0.3%, 0.4%) of the extract.
[0035] In some embodiments, in step i, the process conditions for centrifugal separation include: placing the material stream to be separated in a centrifuge, centrifuging at a constant temperature of 80 to 140° C. (e.g., 90° C., 100° C., 120° C.) for 0.5 to 10 min (e.g., 0.6 min, 1 min, 2 min, 4 min, 5 min, 8 min), and the separation factor is between 500 and 3000 (e.g., 600, 800, 1000, 1500, 2000, 2500).
[0036] In some embodiments, in step i, the process conditions for natural sedimentation include: constant temperature sedimentation at 80-180°C (e.g., 90°C, 100°C, 120°C, 150°C) for 4-48 hours (e.g., 5 hours, 10 hours, 15 hours, 20 hours, 25 hours, 30 hours, 40 hours).
[0037] In some embodiments, the coal-based pitch is selected from coal tar pitch, coal tar modified pitch or coal liquefaction pitch.
[0038] In some embodiments, based on the total weight of the coal-based asphalt, the ash content in the coal-based asphalt is 0.1 to 5 wt% (e.g., 0.2 wt%, 0.5 wt%, 1 wt%, 2 wt%, 4 wt%), and / or the quinoline insoluble matter content is 1 to 10 wt% (e.g., 2 wt%, 4 wt%, 5 wt%, 6 wt%, 8 wt%).
[0039] In some embodiments, in step i, the conditions for dissolving by the first solvent include: the dissolution temperature is 100-200°C (for example, 120°C, 150°C, 160°C, 180°C), and the dissolution time is 15-60 min (for example, 20 min, 30 min, 40 min, 50 min).
[0040] In some embodiments, in step ii, the conditions of the flocculation reaction include: the reaction temperature is 50-120°C (for example, 60°C, 80°C, 100°C, 110°C), the stirring speed is 80-350r / min (for example, 100r / min, 250r / min, 300r / min), and the stirring time is 10-60min (for example, 15min, 30min, 40min, 50min).
[0041] In some embodiments, in step ii, the conditions for subjecting the suspension to the centrifugal separation include: placing the suspension in a centrifuge, centrifuging at a constant temperature of 50-120°C (e.g., 60°C, 80°C, 100°C, 110°C) for 0.5-10 min (e.g., 1 min, 2 min, 4 min, 8 min), and a separation factor between 500 and 3000 (e.g., 600, 1000, 1500, 2000, 2500).
[0042] In some embodiments, the process conditions for subjecting the suspension to natural sedimentation include: constant temperature sedimentation at 50-120°C (e.g., 60°C, 80°C, 100°C, 110°C) for 6-72 hours (e.g., 8 hours, 12 hours, 20 hours, 40 hours, 60 hours, 70 hours).
[0043] The separation process conditions in step ii may be a separation operation on a suspension formed by mixing the extract and the second solvent, or a separation operation on a suspension formed by mixing the first light phase and the second solvent.
[0044] In a second aspect, a refined asphalt containing low ash and low quinoline insolubles obtained by the deashing method as described above is provided, for example, a refined asphalt having an ash content of less than 100 ppm (e.g., 1 ppm, 4 ppm, 10 ppm, 20 ppm, 50 ppm, 80 ppm) and a quinoline insoluble content of less than 0.1 wt% (e.g., 0.001 wt%, 0.005 wt%, 0.01 wt%, 0.04 wt%, 0.06 wt%, 0.08 wt%).
[0045] In view of the problems of small ash particle size, high asphalt viscosity, high sulfur and nitrogen impurity content, and strong chelating force on inorganic components in coal-based asphalt, the present invention adopts a two-stage refining step. After the first-stage refining, the solvent is not recovered, and the obtained extract is directly mixed with a second solvent with a higher hydrogen-carbon ratio for flocculation reaction to achieve efficient deashing, which not only has a higher yield of asphalt, but also has better quality. The asphalt deashing process of the present invention is simple, the conditions are mild, and the deashing efficiency is high, and the industrial technical feasibility is strong.
[0046] Compared with the prior art, the present invention has the following beneficial effects:
[0047] 1) Two solvents with large differences in hydrogen-to-carbon ratios are used to perform secondary refining treatment on coal-based asphalt. In the first-stage refining process, a first solvent (solvent with strong solubility) with a relatively low hydrogen-to-carbon ratio is used to dissolve the coal-based asphalt to dissolve the asphalt to the maximum extent, so as to improve the yield of low-ash refined asphalt; before the second-stage refining, there is no need to recover the first solvent, but directly add a second solvent (solvent with relatively weak solubility) with a relatively high hydrogen-to-carbon ratio to precipitate some high-molecular-weight substances in the asphalt, so as to adsorb and condense ultrafine ash particles or flocculant residues suspended in the asphalt solution, so as to achieve deep deashing, reduce impurity residues, and improve the quality of asphalt products, and obtain coal-based refined asphalt with an ash content of less than 100 ppm and a quinoline insoluble content of less than 0.1%;
[0048] 2) The obtained asphalt has a low ash content and can be used as a high-quality raw material for preparing carbon materials such as mesophase asphalt, lithium battery negative electrode materials, needle coke, and coated asphalt;
[0049] 3) Both the dissolution process and the refining process are carried out under relatively mild conditions, which has relatively low requirements for separation equipment, is conducive to the use of high-efficiency separation equipment, and accelerates separation efficiency; compared with the existing asphalt deashing process, the process cycle is short, the operation is simple, the reaction conditions are mild, the yield of asphalt products is as high as 70-90%, and the ash content is only 10-100ppm;
[0050] 4) By adding a step of separating the extract before the obtained extract is mixed with the second solvent and subjected to flocculation reaction, it is possible to produce refined asphalt with an ash content of less than 100 ppm and a quinoline insoluble content of less than 0.1%, and at the same time, produce a binder asphalt with an ash content of less than 0.1% and a quinoline insoluble content of less than 1%. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 A schematic diagram of a deashing method process according to an embodiment of the present invention is shown. DETAILED DESCRIPTION
[0052] In order to understand the technical features and contents of the present invention in detail, the preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described in the embodiments, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described here.
[0053] <Source of raw materials>
[0054] Coal liquefaction pitch: softening point is 162°C, ash content is 1.0wt%, quinoline insoluble content is 4.1wt%;
[0055] Coal tar pitch: softening point 92°C, ash content 0.21wt%, quinoline insoluble content 5.2wt%;
[0056] The first solvent: a coal tar fraction having a content of 5-98 wt %, the distillation temperature of the coal tar fraction being 180-300° C. and H / C=0.89;
[0057] Second solvent A: naphtha with a content of 5-98 wt%, the distillation temperature of naphtha is 70-140° C. and H / C=1.98;
[0058] The second solvent B is a coal indirect liquefaction light oil with a content of 5-98 wt %, the coal indirect liquefaction light oil has a distillation temperature of 70-160° C. and H / C=2.03.
[0059] Embodiment 1:
[0060] Deashing methods for coal-based asphalt, such as Figure 1 As shown, the following steps are included:
[0061] i. Add the first solvent to 1 kg of coal liquefaction pitch to be treated, mix the mixture at a mass ratio of 1:2 between the coal liquefaction pitch and the first solvent, and fully dissolve the mixture at 150° C. for 30 minutes to obtain an extract;
[0062] The obtained extract was cooled to 100°C, and then 4 g of activated clay was added to mix, and the mixture was mixed at this temperature for 30 minutes to obtain an extract mixture, which was placed in a high-temperature centrifuge and centrifuged at 100°C for 2 minutes at a constant temperature, with a separation factor of 1800;
[0063] Centrifugal separation obtains a first heavy phase and a first light phase, and the first heavy phase is subjected to reduced pressure distillation at 250° C. and −0.08 MPa (gauge pressure) to recover the first solvent, thereby obtaining heavy asphalt; the first light phase in the centrifuge enters step ii;
[0064] ii. The first light phase separated in step i was mixed with the second solvent A in a mass ratio of 1:2 and subjected to flocculation reaction under the following reaction conditions: stirring at 100° C. and 150 r / min for 30 min to obtain a suspension;
[0065] The suspension was then placed in a high temperature centrifuge and centrifuged at 100°C for 1.5 min with a separation factor of 1800. After the centrifugation, a second light phase (supernatant) and a second heavy phase (heavy phase at the bottom) were obtained.
[0066] iii. After the second heavy phase (bottom heavy phase material) separated in step ii is subjected to reduced pressure distillation at 250° C. and -0.08 MPa (gauge pressure) to recover the solvent (the recovered solvent is a mixture of the first solvent and the second solvent A), the light phase (recovered solvent) obtained at the top of the still is mixed with the second light phase (supernatant liquid) obtained in step ii, and the binder asphalt is obtained at the bottom of the still;
[0067] The second light phase (supernatant) separated in step ii is first flashed at 160°C and normal pressure to remove the second solvent A and reused, and then the first solvent is recovered and reused by reduced pressure distillation at 250°C and -0.08MPa (gauge pressure), and ultra-low ash refined asphalt is obtained at the bottom of the distillation kettle. The test results of the obtained products are shown in Table 1.
[0068] Embodiment 2:
[0069] The deashing method of coal-based asphalt is referred to Example 1, except that: in step i, activated clay is not added to the extract, but a mixture formed by a sedimentation aid and a wetting agent is added to the extract to obtain an extract mixture; that is, before entering the high-temperature centrifuge, the extract is cooled to 100°C, and a sedimentation aid accounting for 5% of the mass fraction of the extract and 0.2% of ethylene glycol are added under constant temperature conditions, and immediately stirred for 1 minute with a homogenizer at a stirring speed of 4000r / min, and then stirred for 60 minutes at a stirring speed of 100r / min. Among them, the sedimentation aid is an aqueous solution containing 2wt% polyaluminum chloride. The remaining steps are the same as in Example 1. The test results of the obtained product are shown in Table 1.
[0070] Embodiment 3:
[0071] The deashing method of coal-based asphalt is referred to Example 2, except that: in step i, the high-temperature centrifugal separation of the extract mixture is replaced by natural sedimentation separation, wherein the conditions for natural sedimentation separation are: standing at a constant temperature of 140°C for 40 hours; and in step ii, the high-temperature centrifugal separation of the suspension is replaced by natural sedimentation separation, wherein the conditions for natural sedimentation separation are: standing at a constant temperature of 100°C for 48 hours. The remaining steps are the same as in Example 2. The test results of the obtained product are shown in Table 1.
[0072] Embodiment 4:
[0073] The deashing method of coal-based asphalt is referred to Example 1, except that: in step i, the coal liquefied asphalt and the first solvent are mixed at a mass ratio of 1:0.5 and fully dissolved at 150° C. for 30 minutes to obtain an extract. The remaining steps are the same as in Example 1. The test results of the obtained product are shown in Table 1.
[0074] Embodiment 5:
[0075] The deashing method of coal-based asphalt is referred to Example 1, except that: in step i, the coal liquefied asphalt and the first solvent are mixed at a mass ratio of 1:4 and fully dissolved at 150° C. for 30 minutes to obtain an extract. The remaining steps are the same as in Example 1. The test results of the obtained product are shown in Table 1.
[0076] Embodiment 6:
[0077] Deashing methods for coal-based asphalt, such as Figure 1 As shown, the following steps are included:
[0078] i. Add the first solvent to 1 kg of coal liquefaction pitch to be treated, mix the mixture at a mass ratio of 1:2.1 between the coal liquefaction pitch and the first solvent, and fully dissolve the mixture at 180° C. for 30 minutes to obtain an extract;
[0079] The obtained extract is kept at a constant temperature of 180° C. for 42 hours for sedimentation separation to obtain a first heavy phase and a first light liquid phase; the first heavy phase is subjected to reduced pressure distillation at 250° C. and -0.08 MPa (gauge pressure) to recover the first solvent to obtain heavy asphalt; the obtained first light phase enters step ii;
[0080] ii. performing a flocculation reaction on the first light phase separated in step i and the second solvent B in a mass ratio of 1:4, under the following reaction conditions: stirring and mixing at 80° C. and 250 r / min for 30 min to obtain a suspension;
[0081] The suspension was then kept at 80°C for 70 hours to obtain a second light phase (supernatant) and a second heavy phase (bottom heavy phase);
[0082] iii. After the second heavy phase (bottom heavy phase material) separated in step ii is subjected to reduced pressure distillation at 250° C. and -0.08 MPa (gauge pressure) to recover the solvent (the recovered solvent is a mixture of the first solvent and the second solvent B), the light phase (recovered solvent) obtained at the top of the still is mixed with the second light phase (supernatant liquid) obtained in step ii, and the binder asphalt is obtained at the bottom of the still;
[0083] The second light phase (supernatant) separated in step ii is first flashed at 180°C and normal pressure to remove the second solvent B and reused, and then the first solvent is recovered and reused by reduced pressure distillation at 250°C and -0.08MPa (gauge pressure), and ultra-low ash refined asphalt is obtained at the bottom of the distillation kettle. The test results of the obtained products are shown in Table 1.
[0084] Embodiment 7:
[0085] The deashing method of coal-based pitch is similar to that of Example 6, except that in step i, the coal-based pitch to be treated is coal tar pitch; the remaining steps are the same as those of Example 6. The test results of the obtained product are shown in Table 1.
[0086] Embodiment 8:
[0087] The deashing method of coal-based asphalt is referred to Example 6, except that in step i, the coal-based asphalt to be treated is coal tar asphalt, and in step ii, the second solvent is the second solvent A; the remaining steps are the same as in Example 6. The test results of the obtained product are shown in Table 1.
[0088] Embodiment 9:
[0089] The deashing method of coal-based asphalt comprises the following steps:
[0090] i. Add the first solvent to 1 kg of coal liquefaction pitch to be treated, mix the mixture at a mass ratio of 1:2.1 between the coal liquefaction pitch and the first solvent, and fully dissolve the mixture at 180° C. for 30 minutes to obtain an extract;
[0091] ii. The extract obtained in step i was subjected to flocculation reaction with the second solvent B in a mass ratio of 1:4, and the reaction conditions were: stirring and mixing at 250 r / min for 30 min at 80° C. to obtain a suspension;
[0092] The suspension was then kept at 80°C for 70 hours to obtain a light phase (supernatant) and a heavy phase (heavy phase at the bottom).
[0093] iii. After the heavy phase (bottom heavy phase material) separated in step ii is subjected to reduced pressure distillation at 250° C. and -0.08 MPa (gauge pressure) to recover the solvent (the recovered solvent is a mixture of the first solvent and the second solvent B), the light liquid (recovered solvent) obtained at the top of the still is mixed with the light phase (supernatant liquid) obtained in the separation step ii, and heavy asphalt is obtained at the bottom of the still;
[0094] The light phase (supernatant) separated in step ii is first flashed at 180°C and normal pressure to remove the second solvent B and reused, then the first solvent is recovered and reused by reduced pressure distillation at 250°C and -0.08MPa (gauge pressure), and ultra-low ash refined asphalt is obtained at the bottom of the distillation kettle. The test results of the obtained products are shown in Table 1.
[0095] Comparative Example 1:
[0096] The deashing method of coal-based asphalt comprises the following steps:
[0097] i. The first solvent and the second solvent A were uniformly mixed at a mass ratio of 0.2:1 to obtain a mixed solvent; 1 kg of coal liquefaction pitch was mixed with the mixed solvent at a mass ratio of 1:2 and fully dissolved at 150° C. for 30 minutes to obtain an extract;
[0098] The extract is then kept at a constant temperature of 140° C. for 60 hours, and the first light phase (supernatant) and the first heavy phase are separated and extracted; the first heavy phase is subjected to reduced pressure distillation at 250° C. and -0.08 MPa (gauge pressure) to recover the mixed solvent, thereby obtaining heavy asphalt;
[0099] ii. Cooling the supernatant obtained in step i to 100° C., adding 5% by mass fraction of the extract of a sedimentation aid and 0.2% by mass of ethylene glycol (wherein the sedimentation aid is an aqueous solution containing 2% polyaluminium chloride) thereto, and stirring at a speed of 80 r / min for 60 min to obtain a suspension;
[0100] The suspension was then kept at a constant temperature of 140° C. for 48 h to separate into a second light phase (supernatant) and a second heavy phase (bottom heavy phase);
[0101] iii. After the second heavy phase (bottom heavy phase material) obtained in step ii is subjected to reduced pressure distillation at 250° C. and -0.08 MPa (gauge pressure) to recover the mixed solvent, the light liquid (recovered solvent) at the top of the still is introduced into the second light phase, and the binder asphalt is obtained at the bottom of the still;
[0102] The second light phase (supernatant) obtained in step ii was subjected to vacuum distillation at 250°C and -0.08 MPa (gauge pressure) to recover the mixed solvent and reuse it, and the refined asphalt was obtained at the bottom of the distillation kettle. The test results of the obtained products are shown in Table 1.
[0103] Comparative Example 2:
[0104] The deashing method of coal-based asphalt comprises the following steps:
[0105] i. The first solvent and the second solvent A are uniformly mixed at a mass ratio of 1:2 to obtain a mixed solvent; 1 kg of coal tar pitch is mixed with the mixed solvent at a mass ratio of 1:2 and fully dissolved at 150° C. for 30 minutes to obtain an extract;
[0106] The obtained extract was placed in a high temperature centrifuge and centrifuged at 100°C for 2 min with a separation factor of 1800.
[0107] Separate to obtain a first heavy phase and a first light phase, and distill the first heavy phase under reduced pressure at 250° C. and -0.08 MPa (gauge pressure) to recover the mixed solvent to obtain heavy asphalt; the first light phase in the centrifuge enters step ii;
[0108] ii. placing the first light phase obtained in step i in a high temperature centrifuge, and centrifuging at 100° C. for 1.5 min at a constant temperature, with a separation factor of 1800; after the centrifugation, a second light phase (supernatant) and a second heavy phase (heavy phase at the bottom) are obtained;
[0109] iii. After the second heavy phase (bottom heavy phase material) obtained in step ii is subjected to reduced pressure distillation at 250° C. and -0.08 MPa (gauge pressure) to recover the mixed solvent (a mixture of the first solvent and the second solvent A), the obtained light phase (mixed solvent) is mixed with the second light phase (supernatant liquid) obtained in step ii, and the binder asphalt is obtained at the bottom of the distillation kettle;
[0110] The second light phase (supernatant) obtained in step ii is first flashed at 160°C and normal pressure to remove the second solvent A and reused, and then the first solvent is recovered and reused by reduced pressure distillation at 250°C and -0.08MPa (gauge pressure), and refined asphalt is obtained at the bottom of the distillation kettle. The test results of the obtained products are shown in Table 1.
[0111] Comparative Example 3:
[0112] 1 kg of coal liquefaction pitch and 4 kg of the first solvent were added to a stirring kettle, and then they were thoroughly mixed; the stirring kettle was filled with N2 to 2.0 MPa (gauge pressure), the temperature was raised to 180°C, and the mixture was stirred at a stirring speed of 200 r / min for 30 minutes to obtain a mixture-I; the mixture-I was then pressurized and hot filtered, and the extract obtained by filtration was subjected to reduced pressure distillation at 250°C and -0.08 MPa (gauge pressure) to recover the first solvent, and 0.89 kg of the extract was obtained.
[0113] The obtained extract and 3 kg of the second solvent A were added to a stirred tank and mixed thoroughly; the stirred tank was filled with N2 to 0.5 MPa (gauge pressure), the temperature was raised to 120° C., and the mixture was stirred at a stirring speed of 250 r / min for 20 minutes to obtain a mixture-II; the mixture-II was then subjected to constant temperature centrifugation at 120° C. for 2 minutes with a separation factor of 1800 to separate the bottom heavy phase and the upper clear liquid;
[0114] The upper clear liquid obtained by centrifugal separation was distilled at 160°C and atmospheric pressure to recover the second solvent A, and 0.27 kg of heavy liquefied oil was obtained; the bottom heavy phase obtained by centrifugal separation was distilled at 160°C and atmospheric pressure to recover the second solvent A, and 0.62 kg of asphalt-like substance was obtained.
[0115] Table 1 Test results of the products obtained in each embodiment and comparative example
[0116]
[0117] Note: In Table 1, Ash represents the ash content in asphalt, and QI represents the quinoline insoluble content in asphalt.
[0118] From the results in Table 1, it can be seen that in each embodiment, two solvents with large solubility differences are used to perform secondary refining treatment on coal-based asphalt. In the primary refining process, the first solvent with stronger solubility is used to dissolve the coal-based asphalt, dissolving the asphalt to the maximum extent to improve the yield of low-ash refined asphalt; before the secondary refining, it is not necessary to recover the first solvent, but directly add the second solvent with relatively weak dissolving ability to achieve deep deashing, reduce impurity residues, improve the quality of asphalt products, and obtain coal-based refined asphalt with an ash content of less than 100ppm and a quinoline insoluble content of less than 0.1%. Compared with Example 9, the method of Examples 1-8 adds a separation step for the extract, so that while obtaining a coal-based refined asphalt with an ash content of less than 100ppm and a quinoline insoluble content of less than 0.1%, it can also co-produce a binder asphalt with low ash and quinoline insoluble content.
[0119] Although the first solvent and the second solvent are also used for extraction and refining in Comparative Examples 1-3, the process steps and process operations adopted are different from those of the present invention. The quality of the obtained asphalt products is poor, and the ash content of the refined asphalt is greater than 100 ppm and the quinoline insoluble content is greater than 0.1%.
[0120] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A method for deashing coal-based asphalt, characterized in that: The steps include: i. Coal-based asphalt is used as the raw material to be treated, and a first solvent is added to the mixture and fully dissolved to obtain an extract; the mass ratio of the first solvent to the coal-based asphalt is (0.5-4):1; the first solvent is a coal tar fraction or a coal direct liquefaction oil fraction, and its distillation range is between 180 and 300° C. and H / C=0.6-1.0; ii. The extract obtained in step i is mixed with a second solvent in a mass ratio of 1:(1-4) and then subjected to flocculation reaction to obtain a suspension; the second solvent is one or more of naphtha, coal indirect liquefaction light oil, coal coking light oil, coal direct liquefaction light oil, petroleum ether and mixed benzene, and the distillation range is between 70-160° C. and H / C=1.1-2.3; Then, the suspension is centrifuged or subjected to natural sedimentation separation to obtain a heavy phase and a light phase; iii. recovering the solvent from the heavy phase obtained in step ii to obtain heavy asphalt, and optionally mixing the recovered solvent into the light phase; The second solvent and the first solvent in the light phase are recovered separately to obtain a refined asphalt with an ash content of less than 100 ppm and a quinoline insoluble content of less than 0.1 wt%.
2. The deashing method according to claim 1, characterized in that The steps include: i. Coal-based asphalt is used as the raw material to be treated, and a first solvent is added to the mixture and fully dissolved to obtain an extract; the mass ratio of the first solvent to the coal-based asphalt is (0.5-4):1; the first solvent is a coal tar fraction or a coal direct liquefaction oil fraction, and its distillation range is between 180 and 300° C. and H / C=0.6-1.0; The obtained extract is then centrifuged or subjected to natural sedimentation separation to obtain a first heavy phase and a first light phase; the first heavy phase is then subjected to reduced pressure distillation to recover the first solvent to obtain heavy asphalt; ii. The first light phase separated in step i is mixed with a second solvent in a mass ratio of 1:(1-4) and subjected to flocculation reaction to obtain a suspension; the second solvent is one or more of naphtha, coal indirect liquefaction light oil, coal coking light oil, coal direct liquefaction light oil, petroleum ether and mixed benzene, and the distillation range is between 70-160° C. and H / C=1.1-2.3; Then, the suspension is centrifuged or subjected to natural sedimentation separation to obtain a second heavy phase and a second light phase; iii. After solvent recovery from the second heavy phase separated in step ii, a binder asphalt having an ash content of less than 0.1 wt% and a quinoline insoluble content of less than 1 wt% is obtained, and the recovered solvent is optionally mixed into the second light phase; The second solvent and the first solvent in the second light phase are recovered separately to obtain a refined asphalt with an ash content of less than 100 ppm and a quinoline insoluble content of less than 0.1 wt%.
3. The deliming method according to claim 2, characterized in that In step i, before separating the extract, a mixture of a sedimentation aid and a wetting agent and / or activated clay is added to the extract; Preferably, the sedimentation aid is an aqueous solution containing 1 to 10 wt% of a flocculant; more preferably, the flocculant is selected from one or more of polyacrylamide, polyaluminium chloride, polyaluminium sulfate, polyferric chloride and polyferric sulfate; Preferably, the wetting agent is selected from one or more of ethanol, 1-pentanol, 1-octanol, ethylene glycol and glycerol.
4. The deliming method according to claim 3, characterized in that Before separating the extract, activated clay is added to the extract, and the amount of the activated clay added is 0.1-1 wt% based on the mass of the coal-based asphalt; and / or The process conditions for adding activated clay into the extract for mixing include: a mixing temperature of 80 to 140° C. and a mixing time of 10 to 60 minutes.
5. The deliming method according to claim 3, characterized in that: Before separating the extract, a mixture formed by a sedimentation aid and a wetting agent is added to the extract and mixed; The mixing process conditions include: a mixing temperature of 80 to 140° C., stirring and mixing for 0.2 to 5 minutes at a stirring speed of 3000 to 8000 r / min, and then stirring and mixing for 30 to 180 minutes at a stirring speed of 50 to 500 r / min; The added amount of the sedimentation aid accounts for 2-10% of the mass fraction of the extract, and the added amount of the wetting agent accounts for 0.1-0.5% of the mass fraction of the extract.
6. The deliming method according to claim 2, characterized in that: In step i, the process conditions of the centrifugal separation include: placing the stream to be separated in a centrifuge, centrifuging at 80 to 140° C. for 0.5 to 10 min at a constant temperature, and the separation factor is between 500 and 3000; and / or The process conditions of natural sedimentation include: constant temperature sedimentation at 80-180° C. for 4-48 hours.
7. The deliming method according to any one of claims 1 to 6, characterized in that The coal-based asphalt is selected from coal tar asphalt, coal tar modified asphalt or coal liquefaction asphalt; Based on the total weight of the coal-based asphalt, the coal-based asphalt has an ash content of 0.1 to 5 wt%, and / or a quinoline insoluble content of 1 to 10 wt%; In step i, the conditions for dissolving by the first solvent include: a dissolving temperature of 100 to 200° C. and a dissolving time of 15 to 60 min.
8. The deliming method according to claim 1 or 2, characterized in that: In step ii, the conditions of the flocculation reaction include: reaction temperature of 50-120° C., stirring speed of 80-350 r / min, and stirring time of 10-60 min.
9. The deliming method according to claim 1 or 2, characterized in that: In step ii, the conditions for centrifuging the suspension include: placing it in a centrifuge, centrifuging it at 50-120° C. for 0.5-10 min, and the separation factor is between 500 and 3000; and / or The process conditions for subjecting the suspension to the natural sedimentation include: constant temperature sedimentation at 50-120° C. for 6-72 hours.
10. A refined asphalt containing low ash content and low quinoline insoluble matter obtained by the deashing method according to any one of claims 1 to 9.