Method for preparing polymethyl substituted benzene from plastic
By mixing plastic with methanol and catalyst, and using molecular sieve catalysts to convert polymethyl-substituted benzene, the problem of high temperature and wide product distribution in polyolefin recycling is solved, the selectivity and conversion rate of polymethyl-substituted benzene are improved, and the polymethyl-substituted benzene is reduced. Reduce production costs and increase the production capacity of high-end chemicals.
Patent Information
- Application Number
- CN202411183318.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-10-29
AI Technical Summary
In the existing polyolefin chemical recycling technology, the reaction temperature is high and the product distribution is wide, resulting in the value of high value-added products that needs to be improved. In particular, the market share of polymethyl-substituted benzene is small and the cost is high, and there is a lack of efficient synthesis routes.
By mixing and reacting plastic or plastic pyrolysis oil with methanol and a catalyst, the plastic is selectively converted into polymethyl-substituted benzene using a molecular sieve catalyst, thereby improving the catalytic cracking conversion rate and product selectivity.
It significantly improves the selectivity and conversion rate of polymethyl-substituted benzene, reduces production costs, increases the production capacity of high-end chemicals, and solves the problem of increasing the economic value of polymethyl-substituted benzene.
Smart Images

Figure CN118853221A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waste plastic conversion, in particular to a method for preparing polymethyl substituted benzene by using plastic. Background Art
[0002] In the past few decades, the global production and consumption of plastics have grown at an alarming rate. Waste plastics, mainly polyolefins, are difficult to degrade naturally, and the environmental pollution they cause is becoming increasingly serious. In addition, the calorific value of polyolefins is similar to that of petroleum, and they contain huge energy that needs to be effectively recycled. The actual recycling efficiency of traditional mechanical recycling and incineration methods is very limited. Chemical recycling and upgrading processes, as one of the most promising alternatives, can convert plastic waste into high-value-added products and can handle low-value, mixed, and contaminated waste plastics. While solving the problem of waste plastics, it also serves as an alternative raw material to petroleum to produce renewable energy. Therefore, it has important research significance in terms of technology, economy, and environmental protection.
[0003] At present, the chemical recovery of polyolefins mainly relies on catalytic cracking to decompose polyolefins into small molecular compounds or monomers, but the reaction temperature of this route is still relatively high, the product distribution is still relatively wide, and the product value needs to be further improved. In previous studies on polyolefin degradation, researchers have made positive attempts to improve the selectivity of specific products. By introducing co-reactants such as hydrogen, carbon dioxide, light normal alkanes, isoalkanes and olefins in the catalytic cracking process, the polyolefin conversion exceeds its own reaction equilibrium, achieving a higher conversion rate at a lower temperature, and selectively converting polyolefins into high-value products such as liquid fuels, aromatics, lubricants, and paraffin.
[0004] Among them, the economic value of pure benzene in aromatics is lower than that of alkylbenzenes, and there is currently an oversupply. In order to solve the overcapacity in the petrochemical industry and increase the production capacity of high-end chemicals, there have been many studies focusing on the alkylation of pure benzene.
[0005] Alkylbenzene is an important chemical raw material, which plays an important role in pillar industries such as fuel, solvent, polyurethane products, medicine, dye, explosive, pesticide, etc., that is, as an important chemical intermediate. At present, benzene, toluene, and xylene (BTX) occupy the largest proportion in the aromatic hydrocarbon industry chain, so they have received more attention from researchers, while polymethyl (methyl number>2) substituted benzene currently has a small market share, so it is easy to be ignored by researchers. However, polymethyl (methyl number>2) substituted benzene can also serve as an important industrial raw material in the above-mentioned pillar industries, and the current market price per ton is higher than that of xylene, and its value cannot be ignored.
[0006] Therefore, developing a synthetic route for polymethyl (methyl number > 2) substituted benzene and reducing its cost has high potential economic value. Summary of the invention
[0007] In view of the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a method for preparing polymethyl substituted benzenes using plastics.
[0008] To achieve the above objectives and other related objectives, the present invention is achieved through the following technical solutions.
[0009] The first aspect of the present invention is to provide a method for preparing polymethyl substituted benzene using plastic, comprising the following steps: mixing plastic or plastic pyrolysis oil, methanol and a catalyst, reacting to obtain polymethyl substituted benzene, wherein the number of methyl groups of the polymethyl substituted benzene is greater than 2.
[0010] The second aspect of the present invention is a polymethyl substituted benzene, which is prepared by the above-mentioned preparation method, and the number of methyl groups of the polymethyl substituted benzene is greater than 2.
[0011] As described above, the present invention provides a method for preparing polymethyl substituted benzene using plastics and polymethyl substituted benzene, which has the following characteristics:
[0012] Beneficial effects:
[0013] The present invention can selectively convert plastic into polymethyl (methyl number>2) substituted benzene by co-reaction of plastic and methanol under the action of molecular sieve catalyst. The addition of methanol can effectively improve the catalytic cracking conversion rate of plastic and significantly improve the selectivity of polymethyl (methyl number>2) substituted benzene. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 Shown is the mass spectrum of pentamethylbenzene of the present invention.
[0015] Figure 2 Shown is the mass spectrum of hexamethylbenzene of the present invention.
[0016] Figure 3 Shown is the gas chromatogram of the liquid product of the present invention.
[0017] Figure 4 Shown is the H NMR spectrum of the liquid phase product of the present invention.
[0018] Figure 5 Shown is a partial enlarged view of the aroma product in the liquid product of the present invention.
[0019] Figure 6 It is a schematic diagram showing the effect of the amount of methanol added on the plastic conversion rate and liquid product selectivity of the present invention.
[0020] Figure 7 It is a schematic diagram showing the effect of the amount of methanol added on the polymethyl-substituted benzene of the present invention.
[0021] Figure 8Shown is a schematic diagram of the effects of different catalysts of the present invention on plastic conversion rate and liquid product selectivity. DETAILED DESCRIPTION
[0022] In order to make the purpose of the invention, technical solutions and beneficial technical effects of the present invention clearer, the present invention is further described in detail below in conjunction with embodiments. People familiar with this technology can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.
[0023] Definition of terms
[0024] The extended part of this application and the effect description of the extended part, including but not limited to subsequent data analysis, mechanism description, etc.
[0025] The first aspect of the present invention is to provide a method for preparing polymethyl substituted benzene using plastic, comprising the following steps: mixing plastic or plastic pyrolysis oil, methanol and a catalyst, reacting to obtain polymethyl substituted benzene, wherein the number of methyl groups of the polymethyl substituted benzene is greater than 2.
[0026] The plastic pyrolysis oil of the present invention can be obtained by heating plastic.
[0027] The present invention can selectively convert plastic into polymethyl (methyl number>2) substituted benzene through the co-reaction of plastic and methanol. The addition of methanol can effectively improve the catalytic cracking conversion rate of plastic and significantly improve the selectivity of polymethyl (methyl number>2) substituted benzene.
[0028] In some embodiments of the present invention, the plastic is selected from one or more of polyesters, polyamides, and polymers whose main chains are alkyl chains.
[0029] In some embodiments of the present invention, the polymer with an alkyl main chain is selected from one or more of polyolefins, copolymers and polymethyl methacrylate; preferably, the polymer with an alkyl main chain is polyolefin.
[0030] Plastics with alkyl chains as the main chain include polyolefins, polymethyl methacrylate and copolymers. The carbon-carbon bonds of the main chain can be broken at the acidic sites of the molecular sieve. The broken molecular fragments undergo subsequent cyclization and react with methanol to form polymethyl-substituted aromatic compounds.
[0031] In some embodiments of the present invention, the polyolefin is selected from any one of polyalphaolefin, polyethylene, polypropylene, polystyrene and poly-4-methyl-1-pentene; preferably, the polyolefin is polyethylene, and the polyethylene is selected from low-density polyethylene, high-density polyethylene and linear low-density polyethylene; further preferably, the polyethylene is linear low-density polyethylene. The weight average molecular weight of the polyethylene is 10,000-6 million; the density of the high-density polyethylene is 0.93-0.97 g / cm3 The density of the linear low-density polyethylene is 0.92-0.935 g / cm 3 ; The density of the low-density polyethylene is 0.91-0.93g / cm 3 .
[0032] In some embodiments of the present invention, the copolymer is ethylene-vinyl acetate copolymer.
[0033] In some embodiments of the present invention, the polyester is selected from one or more of polyethylene terephthalate, polybutylene terephthalate, and polyarylate.
[0034] In some embodiments of the present invention, the polyamide is selected from one or more of nylon 6, nylon 66, nylon 11, nylon 46, and nylon 1010.
[0035] In some embodiments of the present invention, the mass volume ratio of the plastic or plastic pyrolysis oil to the methanol is 1g: (0.1-10)ml.
[0036] In some specific embodiments of the present invention, the mass volume ratio of the plastic or plastic pyrolysis oil to the methanol can be 1g:0.1-0.5ml, 1g:0.5-1ml, 1g:1-2ml, 1g:1-10ml; typically but not limiting, for example, it can be 1g:0.5ml, 1g:1ml, 1g:2ml. When the mass volume ratio of the plastic or plastic pyrolysis oil to the methanol is less than 1g:0.1ml, there is basically no effect, and when it is greater than 1g:10ml, the polyolefin is methylated to saturation, and the excess methanol only reacts by itself.
[0037] In some embodiments of the present invention, the catalyst is added in an amount of 0.1-100 wt % of the plastic.
[0038] In some specific embodiments of the present invention, the amount of the catalyst added is 0.1-3wt%, 3-6wt%, 6-10wt%, 10-100wt% of the plastic; typically but not limiting, for example, it can be 3wt%, 6wt%, 10wt%. If the amount of the catalyst added is less than 0.1wt%, it is basically ineffective, the required reaction temperature is too high, and excessive energy consumption is caused; if it is greater than 100wt%, the catalyst acid reaction sites are excessive, which will cause a waste of reaction sites and introduce unnecessary costs.
[0039] In some embodiments of the present invention, the catalyst is an acidic catalyst, and the acidic catalyst is selected from one or more of a molecular sieve catalyst, alumina, and a supported metal molecular sieve catalyst.
[0040] In some embodiments of the present invention, the particle size of the molecular sieve catalyst is 0.05-15 μm, and the specific surface area is 300-800 m 2 / g.
[0041] In some embodiments of the present invention, the particle size of the supported metal molecular sieve catalyst is 0.05-15 μm, and the specific surface area is 300-800 m 2 / g.
[0042] In some embodiments of the present invention, the catalyst is a molecular sieve catalyst, and the molecular sieve catalyst is selected from any one of β molecular sieve, ZSM-5 molecular sieve, Y-type molecular sieve, SAPO molecular sieve, and MOR molecular sieve; preferably, the molecular sieve is β molecular sieve.
[0043] In some specific embodiments of the present invention, the raw material of the β molecular sieve is selected from H type, NH4 type, and Na type.
[0044] In some specific embodiments of the present invention, the β molecular sieve is an H-type β molecular sieve, and the H-type β molecular sieve can be commercially available or homemade.
[0045] In some specific embodiments of the present invention, the preparation method of the H-type β molecular sieve comprises the following steps: preparing an ammonium chloride solution, wherein the concentration of the ammonium chloride solution is 5-15wt%, mixing the ammonium chloride solution with the Na-type β molecular sieve, performing ion exchange, then washing, and high-temperature drying and activation to remove ammonia to obtain the H-type β molecular sieve. The contact time is 1-10h, the contact temperature is 50-80°C, and the high-temperature drying and activation to remove ammonia is 350-550°C, preferably, the temperature is 400-500°C, and further preferably, the temperature is 450°C.
[0046] In some specific embodiments of the present invention, the preparation method of the H-type β molecular sieve comprises the following steps: subjecting commercially available NH4-type molecular sieve to high-temperature drying, activation and removal of ammonia to obtain the H-type β molecular sieve. The temperature for high-temperature drying, activation and removal of ammonia is 350-550°C, preferably 400-500°C, and more preferably 450°C.
[0047] In some embodiments of the present invention, the β molecular sieve is a pretreated molecular sieve, and the preparation method of the pretreated molecular sieve comprises the following steps: calcining the molecular sieve, taking it out and storing it, to obtain the pretreated molecular sieve.
[0048] In some embodiments of the present invention, the calcination temperature is 300-550°C; specifically, it can be 300-380°C, 380-450°C, 450-550°C; typically but not limiting, for example, 300°C, 380°C, 450°C, 550°C.
[0049] In some embodiments of the present invention, the calcination time is 3-10 h; specifically, it can be 3-8 h, 8-10 h, and typically but not limitedly, for example, 3 h, 8 h, 10 h.
[0050] In some embodiments of the present invention, the removal temperature is >90°C.
[0051] In some embodiments of the present invention, the storage device is selected from any one of a glove box, a glove box, and a drying box.
[0052] In some embodiments of the present invention, the molar ratio of silicon dioxide to aluminum oxide in the molecular sieve is 10-100:1.
[0053] In some specific embodiments of the present invention, the molar ratio of silicon dioxide to aluminum oxide in the molecular sieve may be 10-40:1, 40-70:1, 70-100:1; typically but not limiting, for example, 10:1, 40:1, 70:1, 100:1.
[0054] In some embodiments of the present invention, the catalyst is a loaded metal molecular sieve catalyst, and the preparation method of the loaded metal molecular sieve catalyst comprises the following steps: mixing a metal salt and water to obtain a metal salt solution, immersing the molecular sieve in the metal salt solution, ultrasonically standing, evaporating and drying, and calcining to obtain the loaded metal molecular sieve catalyst.
[0055] In some embodiments of the present invention, the amount of metal salt added is 0.2-2% of the mass of the pretreated molecular sieve; specifically, it can be 0.2-0.8%, 0.8-1.5%, 1.5-2%; typical but non-limiting, for example, 0.2%, 0.8%, 1.5%, 2%.
[0056] In some embodiments of the present invention, the impregnation is selected from equal volume impregnation or excess impregnation. Equal volume impregnation means adding a metal salt solution that can just immerse the molecular sieve.
[0057] In some embodiments of the present invention, the ultrasound duration is 0.5-1 h; the ultrasound power is 150-300 W; and the ultrasound frequency is 30-40 kHz.
[0058] In some embodiments of the present invention, the standing time is greater than 8 hours.
[0059] In some embodiments of the present invention, the drying temperature is 40-80°C; specifically 40-60°C, 60-80°C, typically but not limiting, for example, 40°C, 60°C, 80°C.
[0060] In some embodiments of the present invention, the drying time is 4-8 hours, specifically 4-6 hours, 6-8 hours, typically but not limiting, for example, 4 hours, 6 hours, 8 hours.
[0061] In some embodiments of the present invention, the evaporation pressure is 1-200 mbar.
[0062] In some embodiments of the present invention, the calcination is performed in a reducing gas or a non-reducing gas.
[0063] In some embodiments of the present invention, the calcination degree is divided into the following stages: stage one, heating from room temperature to 400°C-500°C at a heating rate of 3°C-10°C; stage two, maintaining a constant temperature for 1-10 hours; stage three, natural cooling.
[0064] In some embodiments of the present invention, the metal salt is selected from any one of gallium nitrate, ammonium tetrathiomolybdate, platinum nitrate, ruthenium nitrate and rhodium nitrate.
[0065] In some embodiments of the present invention, the metal salt is gallium nitrate, and the calcination is performed in a non-reducing gas atmosphere; preferably, the non-reducing gas is selected from air or nitrogen.
[0066] In some embodiments of the present invention, the metal salt is any one of ammonium tetrathiomolybdate, platinum nitrate, ruthenium nitrate and rhodium nitrate, and the calcination is carried out in a reducing gas atmosphere; the reducing gas is hydrogen.
[0067] In some embodiments of the present invention, the low-pressure evaporation and drying equipment may be selected from a rotary evaporator, a double-row tube plus a magnetic stirring heating plate, a tubular furnace, a vacuum drying oven and the like. Further preferably, the rotary evaporator preliminarily removes the solvent, uniformly loads the metal substance, and then places the vacuum drying oven overnight to dry.
[0068] In some embodiments of the present invention, the molecular sieve in the supported metal molecular sieve catalyst is a pretreated molecular sieve, and the preparation method of the pretreated molecular sieve comprises the following steps: calcining the molecular sieve, taking it out and storing it to obtain the pretreated molecular sieve.
[0069] In some embodiments of the present invention, the calcination temperature is 300-550°C; specifically, it can be 300-380°C, 380-450°C, 450-550°C; typically but not limiting, for example, 300°C, 380°C, 450°C, 550°C.
[0070] In some embodiments of the present invention, the calcination time is 3-10 h; specifically, it can be 3-8 h, 8-10 h, and typically but not limitedly, for example, 3 h, 8 h, 10 h.
[0071] In some embodiments of the present invention, the removal temperature is >90°C.
[0072] In some embodiments of the present invention, the storage device is selected from any one of a glove box, a glove box, and a drying box.
[0073] In some embodiments of the present invention, the molar ratio of silicon dioxide to aluminum oxide in the molecular sieve is 10-100:1.
[0074] In some specific embodiments of the present invention, the molar ratio of silicon dioxide to aluminum oxide in the molecular sieve may be 10-40:1, 40-70:1, 70-100:1; typically but not limiting, for example, 10:1, 40:1, 70:1, 100:1.
[0075] In some embodiments of the present invention, the reaction device is selected from any one of a reactor, a fixed bed reactor, a fluidized bed reactor and a surging bed reactor.
[0076] In some embodiments of the present invention, the reaction temperature is 200-500°C, specifically, 200-250°C; 250-300°C, 300-500°C, typically but not limiting, for example, 200°C, 250°C, 300°C, 500°C.
[0077] In some embodiments of the present invention, the reaction time is 0.1-36 h; specifically, it can be 0.1-2 h, 2-5 h, 5-8 h, 8-12 h, 12-36 h; typical but non-limiting examples include 2 h, 5 h, 8 h, and 12 h.
[0078] In some embodiments of the present invention, the reaction is carried out under an inert gas atmosphere.
[0079] In some specific embodiments of the present invention, the inert gas is selected from nitrogen, argon or helium.
[0080] In some embodiments of the present invention, the reaction pressure is 0.1-15 MPa. Specifically, the reaction pressure may be 0.1-2.5 MPa, 2.5-10 MPa, 10-15 MPa. Typical but non-limiting examples include 0.1 MPa, 2.5 MPa, 10 MPa, and 15 MPa.
[0081] In some embodiments of the present invention, the plastic is a pretreated plastic, and the method for treating the pretreated plastic comprises the following steps: performing a pre-pyrolysis treatment on the plastic to obtain the pretreated plastic.
[0082] In some embodiments of the present invention, the pre-pyrolysis temperature is 100-800°C, specifically 100-200°C, 200-500°C, 500-800°C; typically but not limitatively, for example, 100°C, 200°C, 500°C, 800°C; the pre-pyrolysis time is 0.5-5h; specifically 0.5-1.5h, 1.5-2h, 2-5h; typically but not limitatively, for example, 0.5h, 1.5h, 2h.
[0083] The second aspect of the present invention is to provide a polymethyl substituted benzene, which is prepared by the above-mentioned preparation method, and the number of methyl groups of the polymethyl substituted benzene is greater than 2.
[0084] The present invention is further described below by way of examples, but the scope of the present invention is not limited thereto.
[0085] When the embodiment gives a numerical range, it should be understood that, unless otherwise specified in the present invention, the two endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those generally understood by those skilled in the art. If specific conditions are not specified in the embodiment, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for all reagents or instruments, they are conventional products that can be purchased commercially. In addition to the specific methods, equipment, and materials used in the embodiments, according to the grasp of the prior art by those skilled in the art and the record of the present invention, any method, equipment, and material of the prior art similar or equivalent to the method, equipment, and material in the embodiments of the present invention can also be used to realize the present invention.
[0086] In the following examples, the reagents, materials and instruments used are all commercially available unless otherwise specified.
[0087] Example
[0088] Example 1
[0089] The method of preparing polymethyl substituted benzene using plastic in this embodiment comprises the following steps: mixing plastic, methanol and catalyst, reacting to obtain polymethyl substituted benzene. The reaction temperature is 250°C, the reaction time is 8h, the argon atmosphere pressure is 2.5MPa, the amount of methanol added is 0.7ml, the amount of plastic added is 1g, and the amount of catalyst added is 5wt% of the amount of plastic added. The plastic is polyolefin, the polyolefin is linear low-density polyethylene, the weight average molecular weight of the linear low-density polyethylene is 30W, and the density is 0.93g / cm 3 The catalyst is an H-type β molecular sieve catalyst, the manufacturer of the H-type β molecular sieve catalyst is Tianjin Nanhua Catalyst Co., Ltd., the model is NKF-6-25H, and the specific surface area is 662m 2 / g, the H-type β molecular sieve was calcined, taken out, and stored in a glove box, the calcination temperature was 500°C, the calcination time was 3h, and the take-out temperature was 100°C. SiO in the H-type β molecular sieve catalyst 2 and Al 2 O 3 The molar ratio is 25. The plastic is a pretreated plastic, and the method for treating the pretreated plastic comprises the following steps: pre-pyrolysis the plastic to obtain the pre-treated plastic, the pre-pyrolysis temperature is 150° C., and the pre-pyrolysis time is 1.5 h.
[0090] Example 2
[0091] The method for preparing polymethyl substituted benzene by using plastic in this embodiment is different from that in Embodiment 1 in that the amount of methanol added is 1.4 ml.
[0092] Example 3
[0093] The method for preparing polymethyl substituted benzene using plastic in this embodiment is different from that in embodiment 1 in that the catalyst is a modified molecular sieve, and the modified molecular sieve is Ga 2 O 3 / Hβ molecular sieve, the preparation method of the modified molecular sieve comprises the following steps:
[0094] (1) calcining the molecular sieve, taking it out and storing it in a glove box to obtain a pretreated molecular sieve; the calcination temperature is 400°C, the calcination time is 8h, and the taking-out temperature is 100°C; SiO in the H-type β molecular sieve catalyst 2 and Al 2 O 3 The molar ratio is 25.
[0095] (2) Mixing metal salt and water to obtain metal salt solution, immersing the pretreated molecular sieve in the metal salt solution, ultrasonically standing, evaporating and drying, calcining, and obtaining the modified molecular sieve; wherein the metal salt is gallium nitrate, the calcination is carried out in a non-reducing gas atmosphere; the non-reducing gas is air; the impregnation is equal volume impregnation; the ultrasonic time is 1 hour; the ultrasonic power is 200W; the ultrasonic frequency is 40kHz; the standing time is greater than 8 hours; the calcination degree is divided into the following stages: stage 1, heating from room temperature to 450°C at a heating rate of 6°C; stage 2, constant temperature is maintained for 10 hours; stage 3, natural cooling in air; the evaporation pressure is 100mbar. The evaporation is carried out using a rotary evaporator, the drying is carried out in a vacuum drying oven, the drying temperature is 60°C; the drying time is 6 hours.
[0096] Example 4
[0097] The method for preparing polymethyl substituted benzene using plastic in this embodiment is different from that in embodiment 1 in that the catalyst is a modified molecular sieve, and the modified molecular sieve is MoS 2 / Hβ molecular sieve, the preparation method of the modified molecular sieve comprises the following steps:
[0098] (1) calcining the molecular sieve, taking it out and storing it in a glove box to obtain a pretreated molecular sieve; the calcination temperature is 400°C, the calcination time is 8h, and the taking-out temperature is 100°C; SiO in the H-type β molecular sieve catalyst 2 and Al 2 O 3 The molar ratio is 25;
[0099] (2) Mixing metal salt and water to obtain metal salt solution, immersing the pretreated molecular sieve in the metal salt solution, ultrasonically standing, evaporating and drying, calcining, and obtaining the modified molecular sieve. Wherein, the metal salt is ammonium tetrathiomolybdate, the calcination is carried out in a reducing gas atmosphere; the reducing gas is hydrogen; the impregnation is equal volume impregnation; the ultrasonic time is 1 hour; the ultrasonic power is 200W; the ultrasonic frequency is 40kHz; the standing time is greater than 8 hours; the calcination degree is divided into the following stages: stage one, heating from room temperature to 450°C at a heating rate of 6°C; stage two, constant temperature is maintained for 10 hours; stage three, natural cooling in the air; the evaporation pressure is 100mbar. The evaporation is carried out using a rotary evaporator, and the drying is carried out in a vacuum drying oven, the drying temperature is 60°C; and the drying time is 6 hours.
[0100] Comparative Example
[0101] The method for preparing polymethyl substituted benzene by using plastic in this comparative example is different from that in Example 1 in that no methanol is added.
[0102] Performance Testing
[0103] The mass spectrum was measured by GC-MS, the instrument manufacturer is Thermofisher, model is Trace 1300ISQ. Figure 1 and Figure 2 shown.
[0104] The gas chromatograph was tested using Thermofisher Trace 1300, with a 60m DB-5 column and a FID detector. The temperature of the column was raised from 40°C to 330°C at a rate of 5°C / min and maintained for 5 minutes. The internal standard was n-hexadecane. The spectrum is shown in Figure 3 shown.
[0105] Proton spectrum: manufacturer Bruker Biospin AG, model AVANCE NEO 400, frequency 400 MHz, solvent CD 2 Cl 2 . The spectrum is as follows Figure 4-5 shown.
[0106] Plastic conversion rate test: After the reaction was completed, all the solid residues of each group of Examples 1-4 and Comparative Example were collected, dried under reduced pressure, and the solid residues were weighed to obtain m solid-residue , calculate the plastic conversion rate, the formula is:
[0107]
[0108] m initial =m plastic +m catalyst ;
[0109] Among them, the mass of plastic raw materials used in the reaction is m plastic , the mass of catalyst used is m catalyst .
[0110] Selectivity of aromatic compounds: The selectivity test is based on the gas chromatogram, integrating the peak area to obtain a specific product Y i Liquid product liquid Y i The mass ratio of i represents a specific product, and the formula is:
[0111]
[0112] The aromatic compound selectivity and plastic conversion rate of Examples 1-2 and Comparative Examples are as follows: Figure 6 and Figure 7 shown.
[0113] The aromatic compound selectivity and plastic conversion rate of Example 1 and Examples 3-4 are as follows: Figure 8 shown.
[0114] in, Figure 6-8 The carbon numbers of the substituents in the legends refer to the carbon numbers of the substituents of the corresponding aromatic compounds, and the rest are non-aromatic compounds.
[0115] Results Analysis
[0116] Combined with Example 1-2, and combined with Figure 1 and Figure 2It can be seen that since the mass-to-charge ratios of ordinary pentatoluene and hexatoluene are 148 and 162 respectively, while the mass-to-charge ratios of pentatoluene and hexatoluene whose carbon is entirely carbon 13 isotope are 159 and 174 respectively, the maximum peaks of pentatoluene and hexatoluene molecules obtained by reacting with methanol substituted with carbon 13 isotope are 156 and 171 respectively. Therefore, there are no pentatoluene and hexatoluene whose carbon is entirely carbon 13 isotope. It can be proved that methanol and LDPE co-react, and there is no way for methanol to react alone to produce pentamethylbenzene and hexamethylbenzene.
[0117] Combined with Examples 1-2 and Comparative Examples, and combined with Figure 3-7 It can be seen that the amount of methanol has a certain effect on the reaction. The addition of methanol can improve the LDPE conversion rate and the selectivity of aromatic compounds in the liquid phase product, and mainly improves the selectivity of penta-hexa-toluene. Since the absolute value of toluene and xylene content is too low, the selectivity of tri-toluene and tetra-toluene is incorporated. With the increase of methanol amount, the conversion rate and selectivity are gradually improved.
[0118] Combined with Example 1, Example 3-4, and Figure 8 It can be seen that Ga 2 O 3 / The Hβ catalyst has a high selectivity for penta-hexamethylbenzene, which can reflect the promoting effect of methanol on the production of polymethylbenzenes, but its reaction activity is relatively low compared with that of pure molecular sieve catalysts. 2 / Hβ catalyst can also selectively produce polymethylbenzenes, but the selectivity is reduced.
[0119] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for preparing polymethyl substituted benzene using plastics, It is characterized in that The method comprises the following steps: mixing plastic or plastic pyrolysis oil, methanol and a catalyst, and reacting them to obtain polymethyl substituted benzene, wherein the number of methyl groups of the polymethyl substituted benzene is greater than 2.
2. The method for preparing polymethyl substituted benzene using plastic according to claim 1, Features: Also includes one or more of the following characteristics: 1) The plastic is selected from one or more of polyesters, polyamides, and polymers with an alkyl chain as the main chain; 2) The mass volume ratio of the plastic or plastic pyrolysis oil to the methanol is 1g: (0.1-10)ml; 3) The amount of the catalyst added is 0.1-100wt% of the plastic or plastic pyrolysis oil; 4) The catalyst is an acidic catalyst, and the acidic catalyst is selected from one or more of molecular sieve catalysts, alumina, silica gel, aluminum chloride, and loaded metal molecular sieve catalysts; 5) The reaction temperature is 200-500°C; 6) The reaction time is 0.1-36h; 7) The reaction is carried out under an inert gas atmosphere, preferably, the inert gas is selected from nitrogen, argon or helium; 8) The reaction pressure is 0.1-15MPa; 9) The plastic is a pretreated plastic, and the method for treating the pretreated plastic comprises the following steps: performing a pre-pyrolysis treatment on the plastic to obtain the pretreated plastic.
3. The method for preparing polymethyl substituted benzene using plastic according to claim 2, Features: Also includes one or more of the following characteristics: 11) The polymer with an alkyl main chain is selected from one or more of polyolefins, copolymers and polymethyl methacrylate; preferably, the polymer with an alkyl main chain is a polyolefin, and more preferably, the polyolefin is selected from one or more of polyalphaolefins, polyethylene, polypropylene, polystyrene and poly-4-methyl-1-pentene; 12) The polyester is selected from one or more of polyethylene terephthalate, polybutylene terephthalate, and polyarylate; 13) The polyamide is selected from one or more of nylon 6, nylon 66, nylon 11, nylon 46, and nylon 1010. 91) The pre-pyrolysis temperature is 100-800°C; the pre-pyrolysis time is 0.5-5h.
4. The method for preparing polymethyl substituted benzene using plastic according to claim 2, Features: Also includes any of the following: 41) The catalyst is a molecular sieve, and the molecular sieve catalyst is selected from any one of β molecular sieve, ZSM-5 molecular sieve, Y-type molecular sieve, SAPO molecular sieve, and MOR molecular sieve; preferably, the molecular sieve is β molecular sieve; 42) The catalyst is a loaded metal molecular sieve catalyst. The preparation method of the loaded metal molecular sieve catalyst comprises the following steps: mixing a metal salt and water to obtain a metal salt solution, immersing the molecular sieve in the metal salt solution, ultrasonically standing, evaporating and drying, and calcining to obtain the loaded metal molecular sieve catalyst.
5. The method for preparing polymethyl substituted benzene using plastic according to claim 4, Features: The above 42) also includes one or more of the following features: A1) the amount of the metal salt added is 0.2-2% of the mass of the pretreated molecular sieve; A2) the impregnation is selected from equal volume impregnation or excess impregnation; A3) the ultrasonic time is 0.5-1h; the ultrasonic power is 150-300W; the ultrasonic frequency is 30-40kHz; A4) the standing time is >8h; A5) the drying temperature is 40-80°C; the drying time is 4-8h; A6) the evaporation pressure is 1-200 mbar; A7) the calcination is carried out in a reducing gas or a non-reducing gas; A8) The calcination degree is divided into the following stages: stage 1, heating from room temperature to 400°C-500°C at a heating rate of 3°C-10°C; Stage 2: Maintain constant temperature for 1-10 hours; Stage 3: Natural cooling; A9) The metal salt is selected from any one of gallium nitrate, ammonium tetrathiomolybdate, platinum nitrate, ruthenium nitrate and rhodium nitrate.
6. The method for preparing polymethyl substituted benzene using plastic according to claim 5, Features: Also includes any of the following features: A71) the metal salt is gallium nitrate, and the calcination is carried out in a non-reducing gas atmosphere; A72) The metal salt is any one of ammonium tetrathiomolybdate, platinum nitrate, ruthenium nitrate and rhodium nitrate, and the calcination is carried out in a reducing gas atmosphere.
7. The method for preparing polymethyl substituted benzene using plastic according to claim 6, It is characterized in that Also includes one or more of the following characteristics: A711) the non-reducing gas is selected from air or nitrogen; A721) The reducing gas is hydrogen.
8. The method for preparing polymethyl substituted benzene using plastic according to claim 4, Features: Also includes any of the following features: 411) The β molecular sieve is a pretreated molecular sieve, and the preparation method of the pretreated molecular sieve comprises the following steps: calcining the molecular sieve, taking it out and storing it to obtain the pretreated molecular sieve; 421) The molecular sieve in the loaded metal molecular sieve catalyst is a pretreated molecular sieve, and the preparation method of the pretreated molecular sieve comprises the following steps: calcining the molecular sieve, taking it out and storing it to obtain the pretreated molecular sieve.
9. The method for preparing polymethyl substituted benzene using plastic according to claim 8, Features: Also includes one or more of the following characteristics: S1) the calcination temperature is 300-550°C; S2) the calcination time is 3-10h; S3) the removal temperature is > 90°C; S4) the storage device is selected from any one of a glove box, a glove box, and a drying box; S5) The molar ratio of silicon dioxide to aluminum oxide in the molecular sieve is 10-100:
1.
10. A polymethyl substituted benzene, Features: The polymethyl-substituted benzene is prepared by the preparation method according to any one of claims 1 to 9, wherein the number of methyl groups of the polymethyl-substituted benzene is greater than 2.
Citation Information
Patent Citations
Method for preparing monocyclic aromatic hydrocarbon through selective catalysis of PET waste plastics
CN114835551A
Polystyrene cracking method
CN116272970A
Method for recovering gasoline and diesel from waste plastic
CN1456636A
Process for the preparation of low molecular weight aromatic compounds such as benzene, toluene, and xylenes (BTX) from plastics
EP3744814A1