Preparation method of crystalline-amorphous nickel-lanthanum-based composite compound catalyst

By preparing a crystalline-amorphous nickel lanthanum-based composite compound catalyst, the problem of unsatisfactory electrocatalytic kinetics of nickel-based catalysts in the electrochemical process is solved, the urea oxidation efficiency is improved, and efficient electrolysis of water for hydrogen production and wastewater treatment, demonstrating good photocatalytic performance and industrial applicability.

CN118854346APending Publication Date: 2024-10-29CHONGQING TECH & BUSINESS UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410880277.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Nickel-based catalysts suffer from undesirable electrocatalytic kinetics and slow charge/mass transfer during the electrochemical process, which limits their application efficiency in urea oxidation reactions.

Method used

Using the preparation method of crystalline-amorphous nickel lanthanum-based composite compound catalyst, by reacting lanthanum salt, nickel salt and urea under high temperature and high pressure conditions, a lanthanide series compound with unique electronic configuration and catalytic activity is generated, combined with the nickel element To improve the stability and catalytic activity of the catalyst.

Benefits of technology

It has improved the effect of catalytic urea oxidation, significantly reduced the voltage of electrolyzing water for hydrogen production, and effectively treated urea-containing wastewater. It has good photocatalytic hydrogen evolution potential and industrial applicability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854346A_ABST
    Figure CN118854346A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of nickel-lanthanum-based composite catalysts, and discloses a preparation method of a crystalline-amorphous nickel-lanthanum-based composite compound catalyst, which comprises the following steps: step 1, dissolving lanthanum salt, nickel salt and urea in deionized water, putting foamed nickel as a substrate, and then transferring into a high-pressure reaction kettle with a polytetrafluoroethylene lining for reaction; and 2, washing the mixture obtained in the step 1 until the pH value is neutral, and drying to obtain the crystalline-amorphous nickel-lanthanum-based composite compound catalyst grown on the foamed nickel substrate. By adopting the technical scheme provided by the invention, the crystalline-amorphous nickel-lanthanum-based composite compound catalyst for high-performance treatment of urea wastewater and coupling of electrolyzed water for energy-saving hydrogen production can be obtained, and the process is simple.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nickel-lanthanum-based composite catalysts, and in particular to a method for preparing a crystalline-amorphous nickel-lanthanum-based composite compound catalyst. Background Art

[0002] As an efficient and clean energy carrier, hydrogen has become an ideal choice to replace traditional fossil fuels. Compared with hydrogen production from fossil energy, water electrolysis hydrogen production technology has the advantages of abundant raw material sources, no pollution, simple preparation process and high hydrogen purity. Further coupling with large-scale power generation such as renewable wind energy and solar energy, it is expected to consume the "three abandoned" electricity generated, thereby adjusting and optimizing the energy structure of the power system. Replacing the oxygen evolution reaction at the anode of water electrolysis with the urea oxidation reaction with a low oxidation potential can achieve efficient and energy-saving hydrogen production. Among modern chemical molecules, urea has become one of the most important molecules due to its important role in industry and agriculture. 70%-80% of the nitrogen content in urban sewage is produced by urea. Improper use and uncontrolled discharge of urea pose a potential threat to human health and ecosystem stability. Therefore, the development of highly selective and efficient urea oxidation degradation catalysts can not only achieve efficient treatment of urea-rich wastewater, but also couple with water decomposition cathode hydrogen production to obtain green and clean energy-hydrogen.

[0003] Nickel-based materials are considered to be highly promising bifunctional catalysts and good alternatives to precious metal materials due to their high abundance, low cost and high catalytic activity. However, unsatisfactory electrocatalytic kinetics and slow charge / mass transfer hinder their application in practical electrochemical processes. Therefore, it is urgent to develop a new type of catalyst to achieve better catalytic urea oxidation. Summary of the invention

[0004] The present invention aims to provide a method for preparing a crystalline-amorphous nickel-lanthanum-based composite compound catalyst to achieve a better catalytic effect of urea oxidation.

[0005] To achieve the above object, the present invention adopts the following technical scheme: a method for preparing a crystalline-amorphous nickel-lanthanum-based composite compound catalyst, comprising the following steps:

[0006] Step 1: dissolving lanthanum salt, nickel salt and urea in deionized water, placing nickel foam as a substrate, and then transferring to a polytetrafluoroethylene-lined autoclave for reaction;

[0007] Step 2: Wash the mixture obtained in step 1 until the pH value is neutral, and dry it to obtain a crystalline-amorphous nickel-lanthanum-based composite compound catalyst grown on a nickel foam substrate.

[0008] Preferably, as an improvement, in step 1, the lanthanum salt is at least one of lanthanum nitrate, lanthanum sulfate and lanthanum chloride.

[0009] Preferably, as an improvement, in step 1, the nickel salt is at least one of nickel nitrate, nickel sulfate and nickel chloride.

[0010] Preferably, as an improvement, in step 1, the molar ratio of lanthanum salt, nickel salt and urea is 1:(0.01-1):(0.5-20).

[0011] Preferably, as an improvement, in step 1, the reaction temperature is between 80 and 250°C.

[0012] Preferably, as an improvement, in step 1, the reaction time is 1 to 48 hours.

[0013] Preferably, as an improvement, in step 2, washing is performed with deionized water.

[0014] Preferably, as an improvement, in step 2, the drying temperature is 60-100°C.

[0015] Preferably, as an improvement, in step 1, the molar ratio of lanthanum salt, nickel salt and urea is 1:(0.05-1):(5-20).

[0016] Preferably, as an improvement, in step 1, the molar ratio of lanthanum salt, nickel salt and urea is 1:0.05:5.

[0017] The principle and advantages of this solution are: in practical application, in this technical solution, in view of the undesirable electrocatalytic kinetics and slow charge / mass transfer problems of nickel-based catalysts, the inventor focuses on lanthanide elements, which have catalytic, magnetic and optical properties due to their unique electronic configuration (4f electrons), and constructs morphology-controllable lanthanide compound catalysts to improve their catalytic activity. Compared with 3d transition metal Ni, the rare earth element La with 4f electron orbits is often used as a co-catalyst in oxidation reactions due to its high stability and excellent oxidation activity, and La compounds are almost never used directly as main catalysts in urea oxidation decomposition reactions. This technical solution uses La as the main catalyst and Ni as the co-catalyst. Through the use of nickel and lanthanum elements, not only can the stability of nickel-based catalysts catalyzing urea oxidation be improved, but also through the optimization of the process, a catalyst with a crystalline-amorphous composite structure can be constructed, so that the catalyst surface is rich in a large number of randomly oriented uncoordinated saturated bonds and unsaturated sites, thereby achieving the adsorption of reactants, accelerating the charge transfer between active sites and intermediates, and thus improving the effect of catalyzing urea oxidation.

[0018] The beneficial effects of this technical solution are:

[0019] 1. The raw materials lanthanum salt, nickel salt and urea used in this scheme are dissolved in the hydrothermal medium and enter the solution in the form of ions and molecular clusters. The strong convection under high temperature and high pressure conditions (generated in the solution in the kettle due to the temperature difference between the upper and lower parts of the kettle) transports these ions, molecules or ion clusters to the growth zone (i.e., the low temperature zone) where the seed crystals are placed to form a supersaturated solution, followed by crystallization, and then a chemical reaction occurs to generate lanthanum carbonate precipitate crystals. Due to the incomplete development of the grains and the small particle size, it is easy to form a crystalline-amorphous composite structure. By controlling the reaction conditions, suitable stoichiometric substances and crystal forms can be obtained.

[0020] 2. In this scheme, urea is used as an alkaline regulator to produce OH - Make with Ni 2+ ,La 3+ The reaction generates Ni(OH)2 and La(OH)3, which are then reacted with trace amounts of CO2 to obtain basic carbonate (in addition to being used as a template for synthesizing La2O3 and La(OH)3 morphology control, basic lanthanum carbonate can reduce the recombination rate of photogenerated electrons and holes due to its relatively negative conduction band and positive valence band edge, giving it good photocatalytic hydrogen evolution potential), thus achieving the controllable preparation of hydroxide and basic carbonate catalysts with an amorphous-crystalline composite structure.

[0021] 3. The method for preparing the crystalline-amorphous nickel-lanthanum-based composite compound catalyst of the present invention is simple and easy to operate, safe to operate, applicable to the fields of urea-containing wastewater treatment and hydrogen production by electrolysis of water, and easy to realize industrialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is the XRD pattern of the catalyst in the embodiment of the present invention.

[0023] Figure 2 HR-TEM image of the catalyst in the example of the present invention. DETAILED DESCRIPTION

[0024] The following is further described in detail through specific implementations, but the implementation of the present invention is not limited thereto. Unless otherwise specified, the technical means used in the following implementations are conventional means well known to those skilled in the art; the experimental methods used are all conventional methods; the materials, reagents, etc. used can all be obtained from commercial channels.

[0025] Program Overview:

[0026] A method for preparing a crystalline-amorphous nickel-lanthanum-based composite compound catalyst comprises the following steps:

[0027] Step 1, dissolving lanthanum salt, nickel salt and urea in deionized water in a molar ratio of 1: (0.01-1): (0.5-20), placing nickel foam as a substrate, and then transferring to a polytetrafluoroethylene-lined high-pressure reactor, reacting at 80-250° C. for 1-48 hours; the lanthanum salt is at least one of lanthanum nitrate, lanthanum sulfate and lanthanum chloride; the nickel salt is at least one of nickel nitrate, nickel sulfate and nickel chloride;

[0028] Step 2: After the reaction is completed, the mixture is naturally cooled to room temperature, and the mixture obtained in step 1 is repeatedly rinsed with deionized water until the pH is neutral, and then dried in an oven for use to obtain a crystalline-amorphous nickel-lanthanum-based composite compound catalyst grown on a nickel foam substrate, and the drying temperature is 60-100°C.

[0029] Example 1

[0030] A method for preparing a crystalline-amorphous nickel-lanthanum-based composite compound catalyst comprises the following steps:

[0031] Step 1: dissolving lanthanum nitrate, nickel nitrate and urea in deionized water at a molar ratio of 1:0.05:5, placing nickel foam as a substrate, and then transferring to a polytetrafluoroethylene-lined autoclave for reaction at 150°C for 6 hours;

[0032] Step 2: repeatedly washing the mixture obtained in step 1 with deionized water to remove soluble inorganic salts and impurities, and drying to obtain a crystalline-amorphous nickel-lanthanum-based composite compound catalyst.

[0033] The difference between Example 2-5 and Example 1 is: the selection of raw materials, the addition ratio and the reaction conditions, as shown in Table 1:

[0034] Table 1

[0035]

[0036] Comparative Example 1

[0037] The difference between this comparative example and Example 1 is that in this comparative example, nickel nitrate is not added during the preparation process, and the obtained product is a mixture of lanthanum basic carbonate and lanthanum hydroxide.

[0038] Comparative Example 2

[0039] The difference between this comparative example and Example 1 is that in this comparative example, lanthanum nitrate is not added during the preparation process, and the obtained product is nickel hydroxide.

[0040] Experimental Example 1 Catalyst Structure Analysis

[0041] The catalysts prepared in Example 1 and the comparative example were subjected to X-ray diffraction analysis. The results are as follows: Figure 1As shown in the XRD results, it can be seen that in the crystalline-amorphous nickel-lanthanum-based composite compound prepared in Example 1, La 3+ First, urea hydrolysis provides OH - The reaction generates La(OH)3, which then reacts with a trace amount of CO2 at a lower temperature to produce the La2(CO3)2(OH)2 phase. With the introduction of nickel, the diffraction peak of La(OH)3 disappears. The catalyst prepared in Comparative Example 1 contains not only the La2(CO3)2(OH)2 phase, but also La(OH)3. This is because the introduction of Ni 2+ Can be used with OH - The reaction generates Ni(OH)2, which consumes part of OH - , the alkali concentration decreases, and the generated La(OH)3 reacts with CO2 to generate La2(CO3)2(OH)2, so La(OH)3 disappears. It can also be found that the introduction of nickel does not change the La2(CO3)2(OH)2 structure, and no diffraction peaks of other Ni species are found except for the foam nickel substrate, indicating that Ni exists in the catalyst in an amorphous form. In addition, the crystalline-amorphous nickel-lanthanum-based composite compound was characterized by high-power transmission electron microscopy, such as Figure 2 It can be found that the catalyst obviously contains a crystal structure with lattice fringes and a disordered amorphous structure, which further illustrates that the catalyst is composed of crystalline-amorphous states.

[0042] Experimental Example 2 Catalytic Performance Test of Catalyst

[0043] Experimental method: A three-electrode system was used, including a working electrode, a counter electrode, and a reference electrode. The directly prepared catalyst was used as the working electrode, and the carbon rod and Hg / HgO were used as the counter electrode and reference electrode, respectively. -1 KOH+0.3molL -1 The urea oxidation reaction performance was investigated in urea electrolyte, and all measured electrode potentials were converted to reversible hydrogen electrode (RHE).

[0044] The test results are shown in Table 2: From the comparison between Examples 1 to 5 and the comparative example, it can be seen that the Ni-La2(CO3)2(OH)2 / NF composite compound catalyst prepared in Example 1 has the best electrocatalytic urea oxidation ability, especially at high current density (>100mA cm -2 ), the electrode potential of Ni-La2(CO3)2(OH)2 / NF composite catalyst is lower, which is more conducive to accelerating the oxidation and decomposition of urea. The oxidation state of lanthanum in basic lanthanum carbonate is +3, La 3+The ions gradually occupy the 4f orbital, indicating the corresponding characteristic 4f band energy level. Due to this special electronic structure, when rare earth is used as an electronic modulator for the electrocatalytic application of transition metal-based active materials, the wave functions of the 4f orbital and 5d orbital of the rare earth element can overlap and hybridize, which is conducive to valence band coupling, delocalizing the 4f electrons and promoting covalent interactions with adsorbed intermediates, and is expected to be used to regulate the electrocatalytic performance of transition metal-based materials. Therefore, the crystalline-amorphous nickel-lanthanum-based composite compound catalyst prepared by the present invention can effectively catalyze the oxidative degradation of urea-containing wastewater, thereby being used as an electrolytic water anode for water decomposition and hydrogen production, which can not only significantly reduce the voltage of the electrolytic water hydrogen production cell, but also achieve efficient degradation of urea-containing wastewater, which has important practical value for solving environmental sewage problems and energy-saving hydrogen production by electrolytic water.

[0045] Table 2

[0046]

[0047] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A method for preparing a crystalline-amorphous nickel-lanthanum-based composite compound catalyst, characterized in that: The steps include: Step 1: dissolving lanthanum salt, nickel salt and urea in deionized water, placing nickel foam as a substrate, and then transferring to a polytetrafluoroethylene-lined autoclave for reaction; Step 2: Wash the mixture obtained in step 1 until the pH value is neutral, and dry it to obtain a crystalline-amorphous nickel-lanthanum-based composite compound catalyst grown on a nickel foam substrate.

2. The method for preparing a crystalline-amorphous nickel-lanthanum based composite compound catalyst according to claim 1, characterized in that: In step 1, the lanthanum salt is at least one of lanthanum nitrate, lanthanum sulfate and lanthanum chloride.

3. The method for preparing a crystalline-amorphous nickel-lanthanum based composite compound catalyst according to claim 2, characterized in that: In step 1, the nickel salt is at least one of nickel nitrate, nickel sulfate and nickel chloride.

4. The method for preparing a crystalline-amorphous nickel-lanthanum based composite compound catalyst according to claim 3, characterized in that: In step 1, the molar ratio of lanthanum salt, nickel salt and urea is 1:(0.01-1):(0.5-20).

5. The method for preparing a crystalline-amorphous nickel-lanthanum based composite compound catalyst according to claim 4, characterized in that: In step 1, the reaction temperature is between 80 and 250°C.

6. The method for preparing a crystalline-amorphous nickel-lanthanum based composite compound catalyst according to claim 5, characterized in that: In step 1, the reaction time is 1 to 48 hours.

7. The method for preparing a crystalline-amorphous nickel-lanthanum based composite compound catalyst according to claim 6, characterized in that: In step 2, deionized water is used for washing.

8. The method for preparing a crystalline-amorphous nickel-lanthanum based composite compound catalyst according to claim 7, characterized in that: In step 2, the drying temperature is 60-100°C.

9. The method for preparing a crystalline-amorphous nickel-lanthanum based composite compound catalyst according to claim 8, characterized in that: In step 1, the molar ratio of lanthanum salt, nickel salt and urea is 1:(0.05-1):(5-20).

10. The method for preparing a crystalline-amorphous nickel-lanthanum based composite compound catalyst according to claim 9, characterized in that: In step 1, the molar ratio of lanthanum salt, nickel salt and urea is 1:0.05:5.