Low-contact-angle composite diaphragm for hydrogen production by alkaline electrolysis of water
By designing a composite separator with dense cortex, reinforcement layer and porous layer, the contact angle of the separator for hydrogen production by alkaline electrolysis of water is reduced, the problem of high energy consumption in the technology of hydrogen production by alkaline electrolysis of water is solved, and the electrolysis efficiency and mechanical strength are improved. , achieving lower electricity bills.
Patent Information
- Application Number
- CN202411039382.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-29
AI Technical Summary
The existing alkaline water electrolysis hydrogen production technology consumes high energy, and the main cost is electricity, resulting in low efficiency of the electrolysis process. It is necessary to reduce the water contact angle of the separator to improve the ion permeability and electrolysis efficiency.
Design a composite separator, including a dense cortex, reinforcement layer and porous layer. By adjusting the structure and composition of each layer, the contact angle of the separator is reduced, the ion passage rate and electrolysis efficiency are improved, and the mechanical strength and stability of the membrane are enhanced.
It effectively reduces the surface resistance of the diaphragm, improves the efficiency of hydrogen production by electrolyzing water, significantly reduces the energy consumption of the electrolysis process, increases the current density, and reduces electricity expenses.
Smart Images

Figure CN118854367A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of hydrogen production by alkaline water electrolysis, and in particular to a composite diaphragm for hydrogen production by alkaline water electrolysis with a low contact angle. Background Art
[0002] In the context of global warming and the decreasing fossil energy, hydrogen energy has received more and more attention, prompting the rapid development of water electrolysis hydrogen production technology. As the earliest applied and relatively mature hydrogen production method, alkaline water electrolysis hydrogen production technology plays an important role in the future development of hydrogen energy. In the process of electrolysis hydrogen production in the electrolyzer, the cathode and anode produce hydrogen and oxygen respectively. The mixture of hydrogen and oxygen is prone to explosion. Therefore, a diaphragm is needed to isolate hydrogen and oxygen. At present, the main problem of water electrolysis hydrogen production is high energy consumption. In the production of alkaline water electrolysis hydrogen production, the main cost is electricity. Therefore, how to reduce the energy consumption (power consumption) of water electrolysis hydrogen production is the key to the problem. In the process of alkaline water electrolysis, ions need to move in a directional manner. The poor ion permeability of the diaphragm will lead to a large energy consumption of alkaline water electrolysis hydrogen production. The size of the diaphragm contact angle is highly correlated with the ion permeability of the diaphragm. Therefore, reducing the water contact angle of the diaphragm is of great significance to the development of alkaline water hydrogen production. Summary of the invention
[0003] The technical problem to be solved by the present invention is to overcome the existing defects of the current technology and provide a composite diaphragm for alkaline water electrolysis to produce hydrogen with a low contact angle, so as to solve the high energy consumption problem mentioned in the above background technology and reduce energy consumption (reduce electricity costs) in the production of hydrogen by alkaline water electrolysis.
[0004] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is as follows: a composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle, which reduces the resistance of ions passing through the diaphragm by reducing the contact angle of the diaphragm, thereby achieving the effect of reducing the surface resistance of the diaphragm, thereby reducing the energy consumption of electrolysis and improving the efficiency of producing hydrogen by water electrolysis. The composite diaphragm includes a dense cortex, a reinforcement layer and a porous layer, the porous layers are arranged on both sides of the reinforcement layer, and the dense cortex is arranged on the side of the porous layer away from the support layer. Among them, due to the addition of the reinforcement layer, the tensile strength of the membrane is relatively high and shows good elongation at break; the porous layer improves the alkali absorption rate of the diaphragm and the wettability of the diaphragm to the electrolyte. At the same time, due to the direct interaction between the porous slurry and the support layer, the physical stability is further improved; the dense cortex has a highly three-dimensional cross-linked structure, which can wrap the support layer without basically affecting the ion conduction performance of the diaphragm, thereby improving the overall strength of the diaphragm, and a large number of nano-hydrophilic particles are distributed on the surface of the dense cortex, which effectively reduces the contact angle of the diaphragm, reduces the surface resistance of the diaphragm, and improves the overall electrolysis efficiency of the electrolytic cell.
[0005] A composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle comprises the following steps:
[0006] In a first aspect, the present invention provides a composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle, comprising a dense skin layer, a reinforcement layer and a porous layer, wherein the porous layers are arranged on both sides of the reinforcement layer, and the dense skin layer is arranged on the side of the porous layer away from the support layer.
[0007] According to a composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle provided by the present invention, the average pore sizes of the dense skin layer, the reinforcement layer and the porous layer are 20 to 40 nm, 1 to 500 μm and 50 to 300 nm respectively.
[0008] According to a composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle provided by the present invention, the thicknesses of the dense skin layer, the reinforcement layer and the porous layer are 1-5 μm, 100-150 μm and 200-250 μm respectively.
[0009] According to a composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle provided by the present invention, the porous layer and the dense skin layer both contain 17 to 19 parts of inorganic nanoparticles, 5 to 9 parts of organic high molecular polymers and 0.5 to 0.9 parts of a pore opener, in parts by mass.
[0010] According to a composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle provided by the present invention, the inorganic nanoparticles are one or a combination of strontium titanate, barium titanate, and titanium oxide; and the size is 10 to 200 nm.
[0011] According to a composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle provided by the present invention, the organic high molecular polymer is one or more of polyether sulfone, polysulfone, polyether ether ketone and chitosan.
[0012] According to a composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle provided by the present invention, the pore opening agent is one or more of polyvinyl pyrrolidone, polyoxyethylene ether, polyacrylic acid (salt), polyethylene glycol and polyacrylamide.
[0013] According to a composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle provided by the present invention, the support body is one or more of PP net, PPS net, PP non-woven fabric, and PPS non-woven fabric.
[0014] According to a composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle provided by the present invention, the fiber diameter of the support body is 50 to 150 μm, and the pore size of the support body is 1 to 500 μm.
[0015] According to the present invention, a composite membrane for producing hydrogen by alkaline water electrolysis with a low contact angle has a tensile strength of 16-30 MPa.
[0016] According to the present invention, a composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle has an elongation at break of 28-32%.
[0017] According to the present invention, a composite membrane with low contact angle for producing hydrogen by alkaline water electrolysis is provided, wherein the contact angle of the composite membrane is 45-50°.
[0018] In a second aspect, the present invention provides a method for preparing the above-mentioned composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle.
[0019] (1) Preparation of casting solution:
[0020] The organic high molecular polymer is dissolved in N-methylpyrrolidone and stirred to obtain a uniformly dispersed solution; then a pore opening agent is added and stirred at 300 r / min at room temperature to completely dissolve it; then inorganic nanoparticles are added and stirred for 24 hours until they are completely dispersed, the stirring speed is reduced to 60 r / min, stirred for 24 hours, and degassed to obtain a milky white casting solution;
[0021] (2) Preparation of supported composite membranes:
[0022] The support (mesh) is soaked in the casting liquid obtained in step (1), and the casting liquid is fully immersed in the interior of the support (mesh), and then scraped with a scraper to determine the thickness. The scraped membrane is left to stand in the air for pre-evaporation, and finally, it is placed in deionized water for phase conversion. The supported composite membrane is soaked and cleaned with deionized water for multiple times until the deionized water is not turbid and transparent, thereby obtaining a composite membrane for hydrogen production by alkaline water electrolysis with a low contact angle.
[0023] Preferably, the amount of the pore opening agent added to the solution in step (1) is 1 to 5 wt %.
[0024] Preferably, the amount of the organic high molecular polymer added in step (1) is 10 to 15 wt%.
[0025] Preferably, the amount of the inorganic nanoparticles added in step (1) is 39-70 wt %.
[0026] Preferably, the amount of N-methylpyrrolidone added in step (1) is 50 wt%.
[0027] Preferably, in step (1), the dissolution temperature of the pore opening agent is 0-20°C; and the dissolution time is not less than 1 hour.
[0028] Preferably, in step (1), the dissolution temperature of the organic high molecular polymer is 0-20° C. and the dissolution time is not less than 5 hours.
[0029] Preferably, in step (1), the dispersion temperature of the inorganic nanoparticles is 0-20° C. and the dispersion time is not less than 12 hours.
[0030] Preferably, in step (2), the pre-evaporation time is 5-25 s; preferably 15 s.
[0031] Preferably, in step (2), the temperature of the deionized water is 5-25°C; preferably 15°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 Schematic diagram of the structure of the diaphragm prepared in the embodiment of the present invention. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the embodiment of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0035] In a first aspect, the present invention provides a composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle, comprising a dense skin layer, a porous layer and a reinforcement layer connected in sequence.
[0036] The present invention adopts a special heterogeneous structure design of a dense cortex, a porous layer and a reinforcement layer, which can not only obtain an alkaline water electrolysis diaphragm with an ultra-low contact angle, but also has extremely low surface resistance, high bubble point and ultra-fast wettability. The reinforcement layer can effectively enhance the mechanical strength of the alkaline water electrolysis diaphragm. At the same time, the present invention greatly reduces the contact angle of the diaphragm, which can effectively reduce the interfacial resistance generated by surface penetration in the traditional alkaline water electrolysis process, thereby effectively improving the current density of the water electrolysis process.
[0037] In some embodiments of the present invention, the average pore sizes of the dense skin layer, the reinforcement layer and the porous layer are 20-40 nm, 1-500 μm and 50-300 nm respectively.
[0038] In some embodiments of the present invention, the width of the finger-shaped holes of the finger-shaped porous layer is 2-10 μm.
[0039] The present invention has found that by setting the average pore size of the dense skin layer, the reinforcement layer and the porous layer and the finger pore width of the finger-shaped porous layer within the above range, the gas barrier property can be achieved without hindering ion transmission.
[0040] In some embodiments of the present invention, the thicknesses of the dense skin layer, the reinforcement layer and the porous layer are 1-5 μm, 100-150 μm and 200-250 μm respectively.
[0041] The present invention controls the thickness of the dense skin layer, the reinforcement layer and the porous layer within the above range, thereby controlling the overall thickness of the composite diaphragm within the range of about 400 μm, which is beneficial to reducing the diaphragm resistance.
[0042] In some embodiments of the present invention, the dense skin layer comprises, by weight, 17 to 19 parts of inorganic nanoparticles, 5 to 9 parts of organic high molecular polymers and 0.5 to 0.9 parts of pore openers.
[0043] In some embodiments of the present invention, the porous layer comprises 17 to 19 parts of inorganic nanoparticles, 5 to 9 parts of organic high molecular polymers and 0.5 to 0.9 parts of pore openers.
[0044] It should be noted that, in a specific embodiment, the compositions of the porous layer and the dense skin layer do not have to be completely the same, and can be within the above ranges.
[0045] In some embodiments of the present invention, the inorganic nanoparticles are one or a combination of strontium titanate, barium titanate, and titanium oxide; and have a size of 10 to 200 nm.
[0046] In the prior art, inorganic nanoparticles are generally selected from one or more of aluminum oxide, zirconium oxide, silicon oxide, zinc oxide, and titanium oxide. The present invention selects one or a combination of strontium titanate, barium titanate, and titanium oxide, which has the advantage of longer-term stability.
[0047] In some embodiments of the present invention, the organic high molecular polymer is one or more of polyethersulfone, polysulfone, polyetheretherketone, and chitosan.
[0048] In some embodiments of the present invention, the pore opening agent is one or more of polyvinyl pyrrolidone, polyoxyethylene ether, polyethylene glycol, polyacrylic acid (salt), and polyacrylamide.
[0049] In some embodiments of the present invention, the support body is one or more of PP net, PPS net, PP non-woven fabric, and PPS non-woven fabric.
[0050] The PP net of the present invention is a net woven from polypropylene fibers. Polypropylene fibers are synthetic fibers spun from isotactic polypropylene obtained by polymerization of propylene. Polypropylene fibers have the characteristics of light weight, high strength, good elasticity, corrosion resistance, and electrical insulation.
[0051] The PPS net of the present invention is a net woven from polyphenylene sulfide fibers. The polyphenylene sulfide fibers are made from polyphenylene sulfide by melt spinning. They are amber in color, have a strength of 0.18-0.26 N / tex, an elongation of 25-35%, and an initial modulus of 2.65-3.53 N / tex. They have good heat resistance and can withstand temperatures up to 190°C. The fibers also have excellent resistance to chemical agents and hydrolysis, as well as flame retardant properties.
[0052] In some embodiments of the present invention, the fiber diameter of the support body is 1 to 150 μm, and the pore size of the support body is 1 to 500 μm.
[0053] Furthermore, in some embodiments of the present invention, the support body is in a mesh shape, the fiber diameter thereof is 150 μm, and the pore size of the support body is 400 μm.
[0054] The following are specific examples. Unless otherwise specified, the raw materials used were obtained through regular commercial channels.
[0055] Example 1
[0056] This embodiment provides a composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle, which comprises a dense skin layer, a porous layer, and a reinforcement layer connected in sequence.
[0057] The average pore sizes of the dense cortex and porous layer are 30nm and 70nm respectively; the diameter of the finger-like pores in the finger-like porous layer is 2μm;
[0058] The thickness of the dense cortex and porous layer are 3μm and 200μm respectively;
[0059] The reinforcing layer is a PP mesh, the diameter of the PP fiber is 150 μm, the pore size of the PP mesh is 400 μm, and the reinforcing layer is embedded in the porous layer, and the area of the reinforcing layer is equal to the horizontal cross-sectional area of the porous layer.
[0060] In terms of mass fraction, the dense skin layer contains 18 parts of inorganic nanoparticles (zirconium oxide, particle size 100 nm), 5 parts of organic polymer (polyether sulfone) and 0.5 parts of pore opener (polyvinyl alcohol);
[0061] The porous layer contains 18 parts of inorganic nanoparticles (zirconium oxide, particle size 50 nm), 6 parts of organic high molecular polymer (polyether sulfone) and 0.5 parts of pore opener (polyvinyl alcohol).
[0062] The preparation method is as follows:
[0063] S1. Prepare the casting solution components: polyethersulfone (mass fraction 10%), zirconium oxide (mass fraction 39%), polyacrylamide (mass fraction 1%) and solvent (NMP, mass fraction 50%);
[0064] S2, firstly mix and stir the casting liquid components in S1 for 24 hours, then completely immerse the support in the casting liquid, and then use a membrane manufacturing device (MSK-AFA-L1000 scraper, the same below) to scrape the casting liquid on one side of the support flat with a flat scraper; prepare a composite membrane in a wet state; the slit between the scrapers is set to 400 microns;
[0065] S3. Pre-evaporate the wet composite membrane for 15 seconds and then place it in a phase transition liquid for phase transition; the phase transition temperature is 15°C; the phase transition liquid consists of deionized water and a solvent (NMP); through the phase transition process, a rapid phase transition occurs on the surface to form a dense cortical structure, and a delayed phase separation occurs inside, gradually forming a finger-like porous layer from the surface to the inside, thereby forming a porous structure.
[0066] S4, after the phase inversion, drying the membrane, cutting and storing, and obtaining a diaphragm;
[0067] The structural schematic diagram of the composite diaphragm electrode obtained in this embodiment is as follows Figure 1 shown.
[0068] Example 2
[0069] This embodiment provides a composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle, which comprises a dense skin layer, a porous layer, and a reinforcement layer connected in sequence.
[0070] The average pore sizes of the dense cortex and porous layer are 35nm and 75nm respectively; the diameter of the finger-like pores in the finger-like porous layer is 2μm;
[0071] The thicknesses of the dense cortex and porous layer are 3 μm and 200 μm, respectively;
[0072] The reinforcing layer is a PP mesh, the diameter of the PP fiber is 50 μm, the pore size of the PP mesh is 400 μm, and the reinforcing layer is embedded in the porous layer.
[0073] In terms of mass fraction, the dense skin layer contains 17 parts of inorganic nanoparticles (zirconium oxide, particle size 200 nm), 7 parts of organic polymer (polysulfone) and 0.5 parts of pore opener (polyvinyl pyrrolidone);
[0074] The porous layer contains 17 parts of inorganic nanoparticles (zirconium oxide, particle size 200 nm), 6 parts of organic high molecular polymer (polysulfone) and 0.5 parts of pore opener (polyvinyl pyrrolidone).
[0075] The preparation method is as follows:
[0076] S1. Prepare the casting solution components: polysulfone (mass fraction 14%), zirconium oxide (mass fraction 35%), polyvinyl pyrrolidone (mass fraction 1%) and solvent (NMP, mass fraction 50%);
[0077] S2, firstly mix and stir the casting liquid components in S1 for 24 hours, then completely immerse the support in the casting liquid, and then use a membrane manufacturing device (MSK-AFA-L1000 scraper, the same below) to scrape the casting liquid on one side of the support flat with a flat scraper; prepare a composite membrane in a wet state; the slit between the scrapers is set to 400 microns;
[0078] S3. Pre-evaporate the wet composite membrane for 15 seconds, and then place it in a phase transition liquid for phase transition; the phase transition temperature is 15°C; the phase transition liquid is composed of deionized water; through the phase transition process, a rapid phase transition occurs on the surface to form a dense cortical structure, and a delayed phase separation occurs inside, gradually forming a finger-like porous layer from the surface to the inside, thereby forming a porous structure.
[0079] S4, after the phase inversion, drying the membrane, cutting and storing, and obtaining a diaphragm;
[0080] Example 3
[0081] This embodiment provides a composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle, which comprises a dense skin layer, a porous layer, and a reinforcement layer connected in sequence.
[0082] The average pore sizes of the dense cortex, porous layer and are 40nm and 73nm respectively; the width of the finger-like pores in the finger-like porous layer is 2μm;
[0083] The thicknesses of the dense cortex and porous layer are 3 μm and 200 μm, respectively;
[0084] The reinforcing layer is a PP mesh, the diameter of the PP fiber is 150 μm, the pore size of the PP mesh is 200 μm, and the reinforcing layer is embedded in the porous layer.
[0085] In terms of mass fraction, the dense skin layer contains 19 parts of inorganic nanoparticles (zirconium oxide, particle size 10 nm), 5 parts of organic high molecular polymer (polyetheretherketone) and 0.5 parts of pore opener (polyvinylpyrrolidone);
[0086] The porous layer contains 19 parts of inorganic nanoparticles (zirconium oxide, particle size 10 nm), 5 parts of organic high molecular polymer (polyetheretherketone) and 0.5 parts of pore opener (polyvinyl pyrrolidone).
[0087] The preparation method is as follows:
[0088] S1. Prepare the casting solution components: polyetheretherketone (mass fraction 10%), zirconium oxide (mass fraction 39%), polyvinylpyrrolidone (mass fraction 1%) and solvent (NMP, mass fraction 50%);
[0089] S2, firstly mix and stir the casting liquid components in S1 for 24 hours, then completely immerse the support in the casting liquid, and then use a membrane manufacturing device (MSK-AFA-L1000 scraper, the same below) to scrape the casting liquid on one side of the support flat with a flat scraper; prepare a composite membrane in a wet state; the slit between the scrapers is set to 400 microns;
[0090] S3. Pre-evaporate the wet composite membrane for 15 seconds, and then place it in a phase transition liquid for phase transition; the phase transition temperature is 15°C; the phase transition liquid is composed of deionized water; through the phase transition process, a rapid phase transition occurs on the surface to form a dense cortical structure, and a delayed phase separation occurs inside, gradually forming a finger-like porous layer from the surface to the inside, thereby forming a porous structure.
[0091] S4, after the phase inversion, drying the membrane, cutting and storing, and obtaining a diaphragm;
[0092] Comparative Example 1
[0093] This comparative example provides a composite diaphragm for alkaline water electrolysis, which is PPS purchased from TORAY.
[0094] Comparative Example 2
[0095] This comparative example provides a composite diaphragm for alkaline water electrolysis, which is ZIRFON PERL UTP 500, purchased from Agfa-Gevaert.
[0096] Comparative Example 3
[0097] This comparative example provides a composite diaphragm for alkaline water electrolysis, and its preparation method is as follows:
[0098] S1. Prepare the casting solution components: polyarylethersulfone (mass fraction 2%), nano zirconium oxide (particle size 20 nm, mass fraction 90%), N-methylpyrrolidone (NMP, mass fraction 8%);
[0099] S2, firstly mix and stir the casting liquid components in S1 for 40 hours, then completely immerse the support in the casting liquid, and then use a membrane manufacturing device to scrape the casting liquid on one side of the support using a flat scraper to prepare a wet composite membrane; the slit between the scrapers is set to 500 microns;
[0100] The support body of this embodiment is a polypropylene fiber mesh with a fiber diameter of 30 microns and a mesh width of 800 microns. The area of the support body is consistent with the area of the diaphragm.
[0101] S3, placing the wet composite membrane into a phase inversion liquid for phase inversion; the phase inversion temperature is 40°C; the phase inversion liquid is a mixture of water and NMP (volume ratio 1:1); the phase inversion time is 20s. During this process, the organic polymer resin in the casting liquid solidifies, the solvent dissolves in the water, and the polymer resin and the solvent undergo phase separation, thereby forming a porous structure.
[0102] S4. After the phase inversion, the membrane is dried, cut and preserved to obtain a diaphragm.
[0103] Performance Testing
[0104] (I) The performance of the composite membrane of the embodiment and the composite membrane of the comparative example was tested, and the results are shown in Table 1.
[0105] Among them, the test method of surface resistance is as follows:
[0106] The separator was cut into small pieces and immersed in 30 wt % KOH solution for 1 day, and then the resistance was tested using an electrochemical workstation.
[0107] The contact angle test method is as follows:
[0108] The contact angle reflects the hydrophilicity of the membrane. The static contact angle of the membrane sample surface was measured using a CA100 standard contact angle meter: the membrane sample was glued to a glass slide and placed on a laboratory bench. The sessile drop method was used for measurement. 2 μL of deionized water was dropped on the membrane sample surface each time. Each membrane was measured six times and the average value was taken.
[0109] The breaking strength is tested by conventional methods in the art.
[0110] Table 1
[0111]
[0112] (ii) The diaphragm was evaluated for pore size, tested for thickness, and calculated for porosity. The results are shown in Table 2.
[0113] Pore size evaluation: The average pore size of the membrane is tested using the bubble point method, and high-purity water is used as the infiltration liquid;
[0114] Porosity calculation:
[0115] Porosity (%) = (weight of wet film - weight of dry film) / density of water / volume of wet film × 100.
[0116] Table 2
[0117] sample Pore size (nm) Thickness(μm) Porosity (%) Example 1 70 419 68 Example 2 75 443 65 Example 3 73 432 70 Comparative Example 1 140 520 60 Comparative Example 2 135 496 55 Comparative Example 3 69 490 56
[0118] (III) The composite diaphragm of Example 2 of the present invention was assembled into an alkaline water electrolysis device, and compared with the alkaline water electrolysis device assembled into Comparative Example 1.
[0119] As a result, under the conditions of Example 2 of the present invention, during the electrolysis of alkaline water, when the electrolysis voltage was 2V, the current density was 4400A / m2.
[0120] Under the conditions of Comparative Example 1, during the electrolysis of alkaline water, when the electrolysis voltage was 2V, the current density was 4181A / m2.
[0121] It can be seen that under the same electrolysis voltage, the alkaline water electrolysis diaphragm of the present invention has a higher current density, which means lower energy consumption and higher electrolysis efficiency.
[0122] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle, characterized in that: It includes a dense skin layer, a porous layer and a reinforcement layer connected in sequence; wherein the reinforcement layer is embedded in the porous layer, and the area of the reinforcement layer is equal to the horizontal cross-sectional area of the porous layer.
2. The composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle according to claim 1, characterized in that: The average pore diameters of the dense skin layer, the reinforcement layer and the porous layer are 20-40 nm, 1-500 μm and 50-300 nm respectively; and / or the diameter of the finger-shaped pores of the finger-shaped porous layer is 2-10 μm.
3. A composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle according to claim 2, characterized in that: The thicknesses of the dense skin layer, the reinforcement layer and the porous layer are 1-5 μm, 100-150 μm and 200-250 μm respectively.
4. A composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle according to any one of claims 1 to 3, characterized in that: In parts by mass, the dense skin layer comprises 17 to 19 parts of inorganic nanoparticles, 5 to 9 parts of organic high molecular polymers and 0.5 to 0.9 parts of pore openers; and / or the porous layer comprises 17 to 19 parts of inorganic nanoparticles, 5 to 9 parts of organic high molecular polymers and 0.5 to 0.9 parts of pore openers.
5. A composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle according to claim 4, characterized in that: The inorganic nanoparticles are one or a combination of strontium titanate, barium titanate, titanium oxide and zirconium oxide; the size is 10 to 200 nm; and / or the organic high molecular polymer is one or more of polyether sulfone, polysulfone, polyether ether ketone and chitosan.
6. A composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle according to any one of claims 1 to 3, characterized in that: The support body is one or more of PP net, PPS net, PP non-woven fabric, and PPS non-woven fabric; further, the fiber diameter of the support body is 10 to 150 μm, and the pore size of the support body is 1 to 500 μm.
7. A method for preparing a composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle according to any one of claims 1 to 6, characterized in that: include: Mixing inorganic nanoparticles, organic high molecular polymer, pore opening agent and solvent to prepare a casting solution; The support body is completely immersed in the casting liquid, and the casting liquid on one side of the support body is scraped flat to prepare a wet membrane; the membrane is pre-evaporated, and then the membrane is immersed in a mixed solution of water-organic solvent. Through the phase transformation process, the surface undergoes rapid phase transformation to form a dense cortical structure, and delayed phase separation occurs inside, and a finger-like porous layer is gradually formed from the surface to the inside, thereby forming a porous structure.
8. The method for preparing a composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle according to claim 7, characterized in that: The porous layer slurry is prepared by the following method: an organic high molecular polymer, an inorganic hydrophilic particle, an optional pore opening agent and an organic solvent are mixed to obtain the porous layer slurry; the surface dense skin layer slurry is prepared by the following method: an organic high molecular polymer, an inorganic hydrophilic particle, an optional pore opening agent and an organic solvent are mixed, and a curing reaction is performed to obtain the surface dense skin layer slurry.
9. A composite diaphragm for producing hydrogen by alkaline water electrolysis with a low contact angle according to any one of claims 1 to 7.
Citation Information
Cited By
Diaphragm for electrochemical cell, electrode laminate for alkaline water electrolysis, and alkaline water electrolysis cell
WO2026176843A1