Sliding shoe for coal mining machine and preparation method of sliding shoe
Using bionic technology to design a non-smooth surface bionic sliding shoe with a millimeter-level convex hull, and carrying out boron nitriding modification treatment on the surface of the sliding shoe, the problems of insufficient wear resistance and high friction coefficient of the shearer sliding shoe are solved. Improved service life and work efficiency, reduced maintenance costs.
Patent Information
- Application Number
- CN202410843210.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-29
AI Technical Summary
The existing shearer sliding shoes have insufficient wear resistance under high friction and impact conditions, high friction coefficient, and poor impact resistance, resulting in short service life, increased energy consumption, and high maintenance costs.
A non-smooth surface bionic sliding shoe with millimeter-level convex hull is designed using bionic technology, and the surface of the sliding shoe is modified with boron nitriding to improve hardness, wear resistance, corrosion resistance, thermal stability, and fatigue strength. .
It effectively increases the service life of the sliding shoe, reduces the friction coefficient, improves the working efficiency and overall efficiency of the shearer, and reduces maintenance costs at the same time.
Smart Images

Figure CN118855463A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of mining machinery, and in particular to a sliding shoe for a coal mining machine and a preparation method thereof. Background Art
[0002] Coal is one of the most important energy sources for mankind. It has not only made great contributions to human material civilization, but also provided effective guarantees for the development of social productivity. my country is the world's second largest economy and the world's largest manufacturing country. As my country's main energy source, coal has important strategic significance for my country's economic development. In recent years, with the rapid development of my country's coal mining technology, the degree of automation and production efficiency of underground coal mining machinery have been greatly improved, and coal mining machines have been widely used. The geological conditions of coal seams in my country are complex, and there are large differences in coal seam inclination, coal hardness, etc. The cutting part, walking part and other parts of the coal mining machine with complex forces are prone to premature failure. The slipper is the main component of the coal mining machine's walking mechanism. The stress state varies greatly under different working conditions. The slipper and the track produce greater friction under heavy pressure, which requires its working surface to have good wear resistance. Whether the working surface is wear-resistant directly determines the practical performance and life of the slipper. However, the existing coal mining machine slipper technology still has the following defects:
[0003] 1. Insufficient wear resistance: Traditional sliding shoe materials are prone to wear under high friction and impact conditions, have a short service life, and frequent replacement increases maintenance costs and downtime.
[0004] 2. High friction coefficient: The friction coefficient of the sliding shoe is high when it contacts the coal seam or rock, which leads to increased energy consumption and reduces the overall efficiency of the coal mining machine.
[0005] 3. Poor impact resistance: Existing materials are prone to cracking and breaking under high impact loads, leading to failure of the skid.
[0006] Therefore, developing a high-reliability slipper and increasing its service life can not only ensure the normal mining of the coal mining machine and save the loss of raw materials and accessories in the coal mine, but also reduce the labor intensity of coal miners and improve the production efficiency of coal mines, which is of great significance to the current coal development field. Summary of the invention
[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a sliding shoe for a coal mining machine and a preparation method thereof. The present invention uses bionic technology and studies biological materials and friction behavior to design a non-smooth surface type bionic sliding shoe with a millimeter-level convex hull, which reduces the contact area between the substrate and the external environment, disperses the contact positive pressure, and reduces the friction coefficient. The present invention also performs boron-nitrogen co-diffusion modification on the surface of the sliding shoe, introduces a boron-nitrogen co-diffusion layer on the non-smooth surface of the sliding shoe, successfully improves the hardness and wear resistance, corrosion resistance, thermal stability, and fatigue strength of the sliding shoe, and effectively improves the service life of the sliding shoe, which not only improves the working efficiency of the coal mining machine, but also reduces maintenance costs, and has significant industrial application potential.
[0008] To achieve the above object, the present invention provides the following technical solutions:
[0009] A method for preparing a sliding shoe for a coal mining machine comprises the following steps:
[0010] S1. Shoe pretreatment: First, use sandpaper to evenly polish and remove the oil layer on the surface of the shoe, use 10-20% dilute sulfuric acid to clean the surface oxide, and before laser cladding, the surface of the shoe is shot peened and roughened, and the surface is cleaned with acetone;
[0011] S2. Prepare the wear-resistant layer material: Mix the wear-resistant iron powder and silicon carbide in a mass ratio of 10-15:1-3 to obtain a wear-resistant layer material;
[0012] S3. Cladding wear-resistant layer: Use multi-layer cladding to clad a 3-6mm wear-resistant layer on the surface of the sliding shoe. Pre-set a 0.5-1.5mm powder layer and then perform laser cladding. Cladd a 1-2mm wear-resistant layer each time, layer by layer until the specified thickness is reached. Cool after each cladding to ensure that there are no cracks and pores.
[0013] S4. Cladding convex hull: After cladding the 3-6mm wear-resistant layer, the synchronous powder feeding method is used to laser clad the convex hull. After cladding, it is cooled to ensure that there are no cracks and pores, and the convex hull is polished;
[0014] S5. Boron-nitrogen co-diffusion treatment: the shoe treated in step S4 is mixed with a boron source until the boron source completely covers the shoe, and then placed in a heating furnace, ammonia is introduced under vacuum conditions, and the temperature is raised to 600-800°C, and the temperature is kept for 1-2 hours; the temperature is further raised to 1000-1200°C, and the temperature is kept for 15-28 hours, and the shoe is taken out after cooling in the furnace;
[0015] S6. Annealing treatment: anneal the sliding shoe treated in step S5 at 400-500° C. for 30-60 seconds in an argon atmosphere, take it out while cooling in the furnace, and obtain the sliding shoe for the coal mining machine.
[0016] Preferably, in step S1, the base material of the sliding shoe is 42CrMn; and the sandpaper is P220 sandpaper.
[0017] Preferably, in step S2, the wear-resistant iron powder comprises the following components by mass percentage: Fe 70-75%, Cr 15-18%, Ni 3-4%, O 3-4%, C 2-3%, Si 1-2%.
[0018] Preferably, the wear-resistant iron powder comprises the following components by mass percentage: Fe 71.35%, Cr 17.45%, Ni 3.87%, O 3.43%, C 2.53%, and Si 1.37%.
[0019] Preferably, in step S3, the parameters of the laser cladding are: laser power 1200-1400 W, spot diameter 3-4 mm, scanning speed 5-6 mm / s, overlap rate 40-60%.
[0020] Preferably, in step S4, the parameters of the laser cladding are: laser power 1200-1400 W, spot diameter 3-4 mm, scanning speed 5-6 mm / s, overlap rate 40-60%, and powder feeding rate 10-15 g / min.
[0021] Preferably, in step S4, the diameter of the convex hull is 8 mm-12 mm, the center distance is 12 mm-16 mm, and the height is 3-5 mm; the convex hulls are arranged in a cross manner, with 45-80 convex hulls distributed per 100 square millimeters.
[0022] Preferably, after step S6, the quality of the manufactured sliding shoe for coal mining machine needs to be checked to ensure that there are no cracks or pores on the surface of the sliding shoe.
[0023] Preferably, in step S5, the boron source is selected from one or more of boron carbide and amorphous boron powder.
[0024] A sliding shoe for a coal mining machine is prepared according to the preparation method.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] 1. The present invention uses bionic technology to study biological materials and friction behavior, and designs a non-smooth surface bionic sliding shoe with a millimeter-level convex hull, which reduces the contact area between the substrate and the external environment, disperses the contact positive pressure, and reduces the friction coefficient;
[0027] 2. The present invention also performs boron-nitrogen co-diffusion modification treatment on the surface of the sliding shoe, and introduces a boron-nitrogen co-diffusion layer on the non-smooth surface of the sliding shoe, which successfully improves the hardness and wear resistance, corrosion resistance, thermal stability, and fatigue strength of the sliding shoe, and effectively increases the service life of the sliding shoe. This not only improves the working efficiency of the coal mining machine, but also reduces maintenance costs, and has significant industrial application potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a process flow chart of the preparation of the sliding shoe for the coal mining machine of the present invention;
[0029] Figure 2 This is a bottom view of a sliding shoe for a coal mining machine prepared in Example 1 of the present invention;
[0030] Figure 3 This is a left view of a sliding shoe for a coal mining machine prepared in Example 1 of the present invention;
[0031] In the figure: 100 is the wear-resistant layer; 200 is the convex hull. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] The sliding shoe base material used in the present invention is 42CrMn, and its composition is: C 0.38%-0.45%, Si 0.17%-0.37%, Mn 0.5%-0.8%, Cr 0.9%-1.2%, P≤0.035%, S≤0.035%;
[0034] The components of the wear-resistant iron powder used are: Fe 71.35%, Cr 17.45%, Ni 3.87%, O 3.43%, C 2.53%, and Si 1.37%.
[0035] See also Figure 1-3 , the present invention provides a technical solution:
[0036] Example 1
[0037] A method for preparing a sliding shoe for a coal mining machine:
[0038] S1. Shoe pretreatment: First, use P220 sandpaper to evenly polish and remove the oil layer on the surface of the shoe, use 10% dilute sulfuric acid to clean the surface oxide, and before laser cladding, the surface of the shoe is roughened by shot peening, and the surface is cleaned with acetone;
[0039] S2. Prepare the wear-resistant layer 100 material: Mix the wear-resistant iron powder and silicon carbide in a mass ratio of 10:1 to obtain the wear-resistant layer 100 material;
[0040] S3. Cladding the wear-resistant layer 100: A 3 mm wear-resistant layer 100 is clad on the surface of the sliding shoe by multi-layer cladding. A 1 mm powder layer is pre-set and then laser cladding is performed. A 1 mm wear-resistant layer 100 is clad each time, layer by layer until the specified thickness is reached. Cooling is performed after each cladding to ensure that there are no cracks and pores.
[0041] S4. Cladding convex hull 200: After cladding the 3 mm wear-resistant layer 100, the laser cladding convex hull 200 is performed by synchronous powder feeding method, and the cladding is cooled to ensure that there are no cracks and pores, and the convex hull 200 is polished;
[0042] S5. Boron-nitrogen co-diffusion treatment: the shoe treated in step S4 is mixed with boron carbide until the shoe is completely covered by the boron carbide, and then placed in a heating furnace, ammonia is introduced under vacuum conditions, and the temperature is raised to 600°C, and the temperature is kept for 1 hour; the temperature is further raised to 1000°C, and the temperature is kept for 15 hours, and the shoe is taken out after being cooled in the furnace;
[0043] S6. Annealing treatment: anneal the sliding shoe treated in step S5 at 400° C. for 30 seconds in an argon atmosphere, and take it out while cooling in the furnace to obtain the sliding shoe for the coal mining machine.
[0044] In the above process, in step S3, the laser cladding parameters are: laser power 1200W, spot diameter 3mm, scanning speed 5mm / s, overlap rate 40%;
[0045] In step S4, the laser cladding parameters are: laser power 1200W, spot diameter 3mm, scanning speed 5mm / s, overlap rate 40%, powder feeding rate 10g / min;
[0046] In step S4, the diameter of the convex hull 200 is 8 mm, the center distance is 12 mm, and the height is 3 mm; the convex hull 200 is arranged in a cross manner, with 45 convex hulls 200 distributed on every 100 square millimeters.
[0047] Example 2
[0048] A method for preparing a sliding shoe for a coal mining machine:
[0049] S1. Shoe pretreatment: First, use P220 sandpaper to evenly polish and remove the oil layer on the surface of the shoe, use 10% dilute sulfuric acid to clean the surface oxide, and before laser cladding, the surface of the shoe is roughened by shot peening, and the surface is cleaned with acetone;
[0050] S2. Prepare the wear-resistant layer 100 material: Mix the wear-resistant iron powder and silicon carbide in a mass ratio of 12:2 to obtain the wear-resistant layer 100 material;
[0051] S3. Cladding the wear-resistant layer 100: A 4 mm wear-resistant layer 100 is clad on the surface of the sliding shoe by multi-layer cladding. A 1 mm powder layer is pre-set and then laser cladding is performed. A 1 mm wear-resistant layer 100 is clad each time, and the layers are stacked layer by layer until the specified thickness is reached. Cooling is performed after each cladding to ensure that there are no cracks and pores.
[0052] S4. Cladding convex hull 200: After cladding the 4 mm wear-resistant layer 100, the laser cladding convex hull 200 is performed by synchronous powder feeding method, and the cladding is cooled to ensure that there are no cracks and pores, and the convex hull 200 is polished;
[0053] S5. Boron-nitrogen co-diffusion treatment: the shoe treated in step S4 is mixed with amorphous boron powder until the shoe is completely covered by boron carbide, and then placed in a heating furnace, ammonia is introduced under vacuum conditions, and the temperature is raised to 800° C. and kept at this temperature for 2 h; the temperature is further raised to 1200° C. and kept at this temperature for 18 h, and then taken out of the furnace after cooling;
[0054] S6. Annealing treatment: anneal the sliding shoe treated in step S5 at 500° C. for 60 seconds in an argon atmosphere, take it out while cooling in the furnace, and obtain the sliding shoe for the coal mining machine.
[0055] In the above process, in step S3, the laser cladding parameters are: laser power 1200W, spot diameter 3mm, scanning speed 5mm / s, overlap rate 40%;
[0056] In step S4, the laser cladding parameters are: laser power 1200W, spot diameter 3mm, scanning speed 5mm / s, overlap rate 40%, powder feeding rate 15g / min;
[0057] In step S4, the diameter of the convex hull 200 is 8 mm, the center distance is 12 mm, and the height is 3 mm; the convex hull 200 is arranged in a cross manner, with 60 convex hulls 200 distributed on every 100 square millimeters.
[0058] Example 3
[0059] A method for preparing a sliding shoe for a coal mining machine:
[0060] S1. Shoe pretreatment: First, use P220 sandpaper to evenly polish and remove the oil layer on the surface of the shoe, use 10% dilute sulfuric acid to clean the surface oxide, and before laser cladding, the surface of the shoe is roughened by shot peening, and the surface is cleaned with acetone;
[0061] S2. Prepare the wear-resistant layer 100 material: Mix the wear-resistant iron powder and silicon carbide in a mass ratio of 13:1 to obtain the wear-resistant layer 100 material;
[0062] S3. Cladding the wear-resistant layer 100: A 5 mm wear-resistant layer 100 is clad on the surface of the sliding shoe by multi-layer cladding. A 1 mm powder layer is pre-set and then laser cladding is performed. A 1 mm wear-resistant layer 100 is clad each time, and the layers are stacked layer by layer until the specified thickness is reached. Cooling is performed after each cladding to ensure that there are no cracks and pores.
[0063] S4. Cladding convex hull 200: After cladding the 5 mm wear-resistant layer 100, the laser cladding convex hull 200 is performed by synchronous powder feeding method, and the cladding is cooled to ensure that there are no cracks and pores, and the convex hull 200 is polished;
[0064] S5. Boron-nitrogen co-diffusion treatment: the shoe treated in step S4 is mixed with amorphous boron powder until the shoe is completely covered by boron carbide, and then placed in a heating furnace, ammonia is introduced under vacuum conditions, and the temperature is raised to 700° C. and kept at this temperature for 1.5 hours; the temperature is further raised to 1100° C. and kept at this temperature for 20 hours, and then taken out of the furnace after cooling;
[0065] S6. Annealing treatment: anneal the sliding shoe treated in step S5 at 450° C. for 50 seconds in an argon atmosphere, cool it down in the furnace and take it out to obtain the sliding shoe for the coal mining machine.
[0066] In the above process, in step S3, the laser cladding parameters are: laser power 1200W, spot diameter 3mm, scanning speed 5mm / s, overlap rate 40%;
[0067] In step S4, the laser cladding parameters are: laser power 1200W, spot diameter 3mm, scanning speed 5mm / s, overlap rate 40%, powder feeding rate 13g / min;
[0068] In step S4, the diameter of the convex hull 200 is 8 mm, the center distance is 12 mm, and the height is 3 mm; the convex hull 200 is arranged in a cross manner, with 80 convex hulls 200 distributed on every 100 square millimeters.
[0069] Comparative Example
[0070] Comparative Example 1: There are the following differences between Comparative Example 1 and Example 1. The only difference is that in Comparative Example 1, step S4 originally existing in Example 1 is omitted, and in Comparative Example 1, the convex hump 200 is not clad on the surface of the wear-resistant layer 100. The remaining steps in Comparative Example 1 and Example 1 are exactly the same.
[0071] Comparative Example 2: Comparative Example 2 is different from Example 1 in that step S5 originally existing in Example 1 is omitted in Comparative Example 2, and boronitrification treatment is not performed in Comparative Example 2. The remaining steps are exactly the same in Comparative Example 2 and Example 1.
[0072] Comparative Example 3: Comparative Example 3 is different from Comparative Example 2 in that step S4 originally existing in Comparative Example 2 is omitted in Comparative Example 3, and the convex hump 200 is not clad on the surface of the wear-resistant layer 100 in Comparative Example 3. The remaining steps are exactly the same in Comparative Example 3 and Comparative Example 2.
[0073] The wear resistance of the sliding shoes prepared in Examples 1-3 and Comparative Examples 1-3 was tested. A friction and wear tester was used to simulate the service wear test, and the final wear rate was determined according to the weight loss method. The hardness of the wear-resistant coating was tested using a Vickers hardness tester. The test results are as follows:
[0074] Table 1. Summary of wear resistance test data
[0075]
[0076] Table 2. Summary of hardness performance test data
[0077]
[0078] It can be seen from the test data in Table 1 and Table 2 that the wear rates of Examples 1-3 at room temperature are much lower than those of Comparative Examples 1-3, which proves that the present invention prepares a wear-resistant sliding shoe. The wear rate of Example 1 is compared with the room temperature wear rates of Comparative Examples 1 and 2, respectively. The wear rate of Example 1 is only 76.49% of that of Comparative Example 1 and 66.57% of that of Comparative Example 2, which further proves that the present invention uses bionic technology, studies biological materials and friction behaviors, prepares the millimeter-level convex hull 200, and introduces a boron-nitrogen co-diffusion layer on the non-smooth surface of the sliding shoe by boron-nitrogen co-diffusion modification treatment on the sliding shoe surface, both of which effectively improve the wear resistance of the sliding shoe; and through the hardness tests of Examples 1-3 and Comparative Examples 1-3 and the wear rate test data at different temperatures, it can be seen that the present invention successfully improves the hardness and wear resistance, thermal stability, and fatigue strength of the sliding shoe by introducing a boron-nitrogen co-diffusion layer, and effectively improves the service life of the sliding shoe, which not only improves the working efficiency of the coal mining machine, but also reduces the maintenance cost, and has significant industrial application potential.
[0079] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a sliding shoe for a coal mining machine, characterized in that: The following steps are involved: S1. Shoe pretreatment: First, use sandpaper to evenly polish and remove the oil layer on the surface of the shoe, use 10-20% dilute sulfuric acid to clean the surface oxide, and before laser cladding, the surface of the shoe is shot peened and roughened, and the surface is cleaned with acetone; S2. Prepare the wear-resistant layer material: Mix the wear-resistant iron powder and silicon carbide in a mass ratio of 10-15:1-3 to obtain a wear-resistant layer material; S3. Cladding wear-resistant layer: Use multi-layer cladding to clad a 3-6mm wear-resistant layer on the surface of the sliding shoe. Pre-set a 0.5-1.5mm powder layer and then perform laser cladding. Cladd a 1-2mm wear-resistant layer each time, layer by layer until the specified thickness is reached. Cool after each cladding to ensure that there are no cracks and pores. S4. Cladding convex hull: After cladding the 3-6mm wear-resistant layer, the synchronous powder feeding method is used to laser clad the convex hull. After cladding, it is cooled to ensure that there are no cracks and pores, and the convex hull is polished; S5. Boron-nitrogen co-diffusion treatment: the shoe treated in step S4 is mixed with a boron source until the boron source completely covers the shoe, and then placed in a heating furnace, ammonia is introduced under vacuum conditions, and the temperature is raised to 600-800°C, and the temperature is kept for 1-2 hours; the temperature is further raised to 1000-1200°C, and the temperature is kept for 15-28 hours, and the shoe is taken out after cooling in the furnace; S6. Annealing treatment: anneal the sliding shoe treated in step S5 at 400-500°C for 30-60s in an argon atmosphere, take it out while cooling in the furnace, and obtain the sliding shoe for the coal mining machine.
2. The method for preparing a sliding shoe for a coal mining machine according to claim 1, characterized in that: In step S1, the base material of the sliding shoe is 42CrMn; and the sandpaper is P220 sandpaper.
3. The method for preparing a sliding shoe for a coal mining machine according to claim 1, characterized in that: In step S2, the wear-resistant iron powder comprises the following components by mass percentage: Fe 70-75%, Cr 15-18%, Ni 3-4%, O 3-4%, C 2-3%, and Si 1-2%.
4. The method for preparing a sliding shoe for a coal mining machine according to claim 3, characterized in that: The wear-resistant iron powder comprises the following components by mass percentage: Fe 71.35%, Cr 17.45%, Ni 3.87%, O 3.43%, C 2.53%, and Si 1.37%.
5. The method for preparing a sliding shoe for a coal mining machine according to claim 1, characterized in that: In step S3, the parameters of the laser cladding are: laser power 1200-1400 W, spot diameter 3-4 mm, scanning speed 5-6 mm / s, overlap rate 40-60%.
6. The method for preparing a sliding shoe for a coal mining machine according to claim 1, characterized in that: In step S4, the parameters of the laser cladding are: laser power 1200-1400 W, spot diameter 3-4 mm, scanning speed 5-6 mm / s, overlap rate 40-60%, and powder feeding rate 10-15 g / min.
7. The method for preparing a sliding shoe for a coal mining machine according to claim 1, characterized in that: In step S4, the diameter of the convex hull is 8mm-12mm, the center distance is 12mm-16mm, and the height is 3-5mm; the convex hulls are arranged in a cross manner, with 45-80 convex hulls distributed per 100 square millimeters.
8. The method for preparing a sliding shoe for a coal mining machine according to claim 1, characterized in that: After step S6, the quality of the manufactured shearer skid shoe needs to be checked to ensure that there are no cracks or pores on the skid shoe surface.
9. The method for preparing a sliding shoe for a coal mining machine according to claim 1, characterized in that: In step S5, the boron source is selected from one or more of boron carbide and amorphous boron powder.
10. A sliding shoe for a coal mining machine, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 9.
Citation Information
Cited By
Coal mining machine sliding shoe bionic wear-resistant structure design and service life prediction method
CN120180617A