Catalyst for producing carbon nanotubes and production method thereof
By using boehmite carriers and metal additives in carbon nanotube catalysts, carbon nanotubes with large specific surface areas are prepared, which solves the problem of poor dispersion in aqueous solutions, improves conductivity and dispersion, and enhances the performance of electrodes. Processability and conductive properties.
Patent Information
- Application Number
- CN202380026570.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-10-28
- Filing Date
- 2023-10-26
- Publication Date
- 2024-10-29
AI Technical Summary
Carbon nanotubes are difficult to disperse stably in aqueous solutions, resulting in a decrease in the processability of the dispersion and an increase in the internal resistance of the electrode. Existing mechanical dispersion treatment and dispersant methods are difficult to effectively solve the problems of low solubility and dispersion.
Boehmite carriers are used to load main catalyst components such as Ni, Co, Fe, etc., co-catalyst components such as Mo and V, and Zr metal additives. By preparing the catalyst and drying and calcining it under specific conditions, carbon nanoparticles with a large specific surface area are formed. Tube.
It improves the conductivity and dispersion of carbon nanotubes, enhances its application performance in conductive materials, and avoids the problems of dispersion aggregation and viscosity increase.
Smart Images

Figure BDA0005035510690000091
Abstract
Description
Technical Field
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Korean Patent Application No. 10-2022-0141853, filed on October 28, 2022, the disclosure of which is incorporated herein by reference in its entirety. Technical Field
[0004] The invention relates to a catalyst capable of synthesizing carbon nanotubes with a large specific surface area and a preparation method thereof. Background Art
[0005] Carbon nanomaterials include fullerene, carbon nanotube (CNT), graphene and graphite nanosheet according to the shape of the material. Among them, carbon nanotube is a macromolecule in which a hexagonal honeycomb graphite surface (in which one carbon atom is bonded to three other carbon atoms) is rolled into a nanometer-sized diameter.
[0006] Carbon nanotubes are hollow and lightweight, and have electrical conductivity as good as copper, thermal conductivity as good as diamond, and tensile strength as good as steel. According to the winding form, they are also divided into single-walled carbon nanotubes (SWCNTs), multi-walled carbon nanotubes (MWCNTs), and rope-like carbon nanotubes.
[0007] Recently, the most active field of research on the use of carbon nanotubes is the field of lithium secondary batteries. The ultimate goal of lithium secondary batteries is to store more electrical energy in a smaller size. As one of the methods for manufacturing electrodes with higher energy density per unit volume by increasing the electrode density of lithium secondary batteries, a method of using carbon nanotubes as conductive materials is being studied. Generally, since high-density electrodes are formed by molding electrode active material particles with a size of several microns to tens of microns by a high-pressure press, the particles are easily deformed during the molding process, the space between the particles is reduced, and the electrolyte permeability is reduced. In order to solve this problem, materials with excellent conductivity and strength are used as conductive materials when manufacturing electrodes. Carbon nanotubes are also widely used as conductive materials because of their excellent strength and conductivity. When a conductive material is used in electrode manufacturing, the conductive material is dispersed between the compressed electrode active materials to maintain the micropores between the active material particles, thereby promoting the penetration of the electrolyte and reducing the resistance within the electrode due to excellent conductivity.
[0008] However, when using carbon nanotubes as a conductive material, the biggest problem is the low solubility and dispersibility of the carbon nanotubes themselves. The problem with carbon nanotubes is that they cannot achieve stable dispersion in an aqueous solution due to the strong van der Waals attraction between them, and aggregation occurs. If the carbon nanotubes aggregate in a dispersion, the workability of the dispersion deteriorates and the dispersion cannot be applied uniformly. Therefore, it is preferred to apply the dispersion in a state that minimizes the viscosity of the dispersion.
[0009] As a method for improving the poor dispersibility of carbon nanotube dispersion, various methods are known. For example, a method for dispersing carbon nanotubes in a dispersion medium by mechanical dispersion treatment such as ultrasonic treatment has been proposed. However, in the case of this method, the dispersibility when ultrasonic irradiation is excellent, but the carbon nanotubes begin to gather immediately after the ultrasonic irradiation is terminated, and even when the concentration of the carbon nanotubes is higher than a certain level, there is a problem of rapid aggregation of the carbon nanotubes. In addition, methods for dispersing and stabilizing carbon nanotubes using various dispersants have been proposed, but these methods also have the problem of being difficult to suppress the increase in viscosity that may occur when the carbon nanotubes are dispersed in a dispersion medium at a high concentration.
[0010] Therefore, there is a need to produce a new carbon nanotube in which the dispersibility can be further improved by improving the properties of the carbon nanotube itself rather than by a mechanical dispersion treatment such as ultrasonic treatment or an auxiliary means such as the use of a dispersant.
[0011] Prior art literature
[0012] (Patent Document 1) KR10-2017-0031061A (Publication Date: March 20, 2017) Summary of the invention
[0013] [Technical issues]
[0014] An object of the present invention is to provide a novel catalyst for producing carbon nanotubes and a method for producing the catalyst, wherein the catalyst is capable of preparing carbon nanotubes which are particularly suitable for use as conductive materials due to their large specific surface area and thus excellent conductivity.
[0015] [Technical solution]
[0016] In order to solve the above problems, the present invention provides a catalyst for producing carbon nanotubes and a preparation method thereof.
[0017] Specifically, (1) the present invention provides a catalyst for producing carbon nanotubes, the catalyst comprising: a boehmite carrier; and a main catalyst component, a co-catalyst component and Zr supported on the carrier.
[0018] (2) The present invention provides the catalyst for producing carbon nanotubes according to (1) above, wherein the number average particle size of the boehmite carrier is 20 μm to 100 μm.
[0019] (3) The present invention provides the catalyst for producing carbon nanotubes according to (1) or (2) above, wherein the main catalyst component is at least one selected from the group consisting of Ni, Co and Fe.
[0020] (4) The present invention provides the catalyst for producing carbon nanotubes according to any one of (1) to (3) above, wherein the co-catalyst component is at least one selected from the group consisting of Mo and V.
[0021] (5) The present invention provides a catalyst for producing carbon nanotubes according to any one of (1) to (4) above, wherein the molar ratio of the main catalyst component to the Zr is 1:0.01 to 1:0.1.
[0022] (6) The present invention provides a catalyst for producing carbon nanotubes according to any one of (1) to (5) above, wherein the molar ratio of the main catalyst component to the co-catalyst component is 1:0.01 to 1:0.2.
[0023] (7) The present invention provides a catalyst for producing carbon nanotubes according to any one of (1) to (6) above, wherein the content of the main catalyst component is 5% by weight to 20% by weight based on the total weight of the catalyst.
[0024] (8) The present invention provides a method for preparing a catalyst for producing carbon nanotubes, the method comprising the following steps: preparing a catalyst composition (S1) by adding a main catalyst precursor, a co-catalyst precursor, a Zr precursor and a polycarboxylic acid to a solvent; and adding a boehmite carrier to the catalyst composition, and drying and calcining it to obtain a catalyst (S2).
[0025] (9) The present invention provides a method for preparing a catalyst for producing carbon nanotubes according to (8) above, wherein the molar ratio of the main catalyst precursor to the polycarboxylic acid added in step (S1) is 1:0.01 to 1:0.1.
[0026] (10) The present invention provides the method for preparing a catalyst for producing carbon nanotubes according to (8) or (9) above, wherein the calcination is performed at 300°C to 720°C.
[0027] [Beneficial Effects]
[0028] The carbon nanotubes synthesized using the catalyst of the present invention have a large specific surface area, and therefore can provide better conductivity even at the same content when used as a conductive material. DETAILED DESCRIPTION
[0029] Hereinafter, the present invention will be described in more detail.
[0030] The terms or words used in the specification and claims of the present application should not be construed as limited to their general meanings or dictionary meanings, but should be construed as meanings and concepts consistent with the technical spirit of the present invention based on the principle that the inventor can fully define the concepts of the terms to best describe his invention.
[0031] The term "carbon nanotube" used in the present invention is a secondary structure formed by forming a bundle of carbon nanotube units in whole or in part, wherein the carbon nanotube unit has a graphite sheet in the shape of a cylinder with a nanometer-sized diameter and has an sp2 bond structure. In this case, the characteristics of a conductor or a semiconductor can be manifested according to the angle and structure of the winding of the graphite surface. According to the number of bonds forming the wall, the carbon nanotube unit can be divided into single-walled carbon nanotubes (SWCNT), double-walled carbon nanotubes (DWCNT) and multi-walled carbon nanotubes (MWCNT), wherein the thinner the wall thickness, the lower the resistance.
[0032] The carbon nanotubes of the present invention may include one or more of single-walled, double-walled and multi-walled carbon nanotube units.
[0033] Catalysts for the production of carbon nanotubes
[0034] The present invention relates to a novel catalyst for producing carbon nanotubes, wherein the catalyst is capable of producing carbon nanotubes with a high specific surface area by using boehmite as a carrier and loading Zr together with a main catalyst component and a co-catalyst component. More specifically, the present invention provides a catalyst for producing carbon nanotubes, the catalyst comprising: a boehmite carrier, and a main catalyst component, a co-catalyst component and Zr loaded on the carrier.
[0035] Hereinafter, each component of the catalyst for producing carbon nanotubes according to the present invention will be described separately.
[0036] Carrier
[0037] The catalyst for producing carbon nanotubes of the present invention uses boehmite as a carrier. Boehmite is an aluminum-based carrier expressed as γ-AlO(OH), and allows the main catalyst component and the co-catalyst component to be uniformly loaded through the hydroxyl groups on the surface. In particular, when a boehmite carrier is used as described below and Zr is loaded together with the main catalyst component and the co-catalyst component, the specific surface area of the carbon nanotubes finally prepared can be increased due to the interaction between the boehmite carrier and the Zr component.
[0038] Meanwhile, the number average particle size of boehmite may be 20 μm to 100 μm, and preferably 40 μm to 60 μm. When the number average particle size of boehmite is within the above range, the co-catalyst and main catalyst components to be described below can be effectively loaded, and the carbon nanotubes prepared with the catalyst can have a large specific surface area.
[0039] In addition, the specific surface area of boehmite can be 150m 2 / g to 250m 2 / g, preferably 170m 2 / g to 220m 2 / g. The bulk density of boehmite can be 500kg / m 3 Up to 1200kg / m 3 , preferably 700kg / m 3 Up to 1000kg / m 3 When the properties of boehmite are within the above ranges, there are technical advantages in that the durability of the support is excellent and a large amount of metal components can be supported without difficulty.
[0040] The shape of boehmite is not particularly limited, and may be spherical or potato-shaped. In addition, boehmite may have a porous structure, a molecular sieve structure, a honeycomb structure, etc., to have a relatively high surface area per unit mass or unit volume.
[0041] Main catalyst component
[0042] In the catalyst for producing carbon nanotubes of the present invention, the main catalyst component can be one or more selected from Ni, Co and Fe, preferably Co. The main catalyst component is used to promote the carbon nanotube synthesis reaction by directly reducing the activation energy of the reaction of synthesizing carbon nanotubes from carbon source gas. When using the above-mentioned main catalyst component, it is desired that the manufactured catalyst can have high activity and durability can also be ensured above a certain level.
[0043] In the catalyst for producing carbon nanotubes of the present invention, the content of the main catalyst component can be 5% by weight to 20% by weight, preferably 8% by weight to 15% by weight. As the content of the main catalyst component increases, the amount of carbon nanotubes obtained relative to the weight of the catalyst used may increase. However, even if the amount of the obtained carbon nanotubes is large, the specific surface area of a single carbon nanotube will also decrease. Therefore, if the content of the main catalyst component in the catalyst is too high, carbon nanotubes with desired properties cannot be obtained. On the other hand, if the content of the main catalyst component is too low, the carbon nanotube synthesis reaction itself may not proceed smoothly.
[0044] Co-catalyst component
[0045] In the catalyst for producing carbon nanotubes of the present invention, the co-catalyst component may be one or more selected from Mo and V, preferably V. The co-catalyst component plays a role in further improving the catalytic activity of the main catalyst component. When the above-mentioned co-catalyst component is used, the synergistic effect with the main catalyst component may be excellent, and aggregation between the main catalyst components during the manufacturing process may be prevented.
[0046] In the catalyst for preparing carbon nanotubes of the present invention, the molar ratio between the main catalyst component and the co-catalyst component may be 1: 0.01 to 1: 0.2. By setting the ratio between the main catalyst component and the co-catalyst component within the above range, sufficient catalytic activity can be achieved through the synergistic effect between the main catalyst component and the co-catalyst component without increasing the main catalyst content to more than the required amount, and the yield and specific surface area of carbon nanotubes can be maintained at excellent levels.
[0047] zirconium
[0048] The catalyst for producing carbon nanotubes of the present invention is loaded with Zr as a metal additive together with the above-mentioned main catalyst component and co-catalyst component. In the case of conventional supported catalysts for producing carbon nanotubes, a two-component catalyst system of the above-mentioned main catalyst and co-catalyst components is frequently used. In the case of such a two-component catalyst system, it has the advantages of being relatively easy to manufacture the catalyst and being particularly suitable for large-scale production, but is limited in that it is difficult to improve the performance, especially the specific surface area, of the carbon nanotubes prepared with the catalyst to above a certain level. In the present invention, it is confirmed that when boehmite is used as a catalyst carrier and Zr is used as a metal additive, the specific surface area of the obtained carbon nanotubes can be increased without significant loss in other properties, while maintaining the advantages of the existing two-component catalyst system.
[0049] Zr can be loaded together with the main catalyst and the co-catalyst component in the catalyst manufacturing step, and then subjected to a drying and calcination process, so that it can be present in the catalyst in the form of an oxide. Zr can be contained in the catalyst so that the molar ratio between the main catalyst component and Zr is 1:0.01 to 1:0.1, and particularly preferably 1:0.02 to 1:0.08. When the Zr content in the catalyst is within the above range, the effect of increasing the specific surface area of the carbon nanotubes can be maximized.
[0050] Preparation method of catalyst for producing carbon nanotubes
[0051] The present invention provides a method for producing the above-mentioned catalyst for producing carbon nanotubes. Specifically, the present invention provides a method for preparing a catalyst for producing carbon nanotubes, the method comprising the following steps: preparing a catalyst composition (S1) by adding a main catalyst precursor, a co-catalyst precursor, a Zr precursor and a polycarboxylic acid to a solvent; and adding a boehmite carrier to the catalyst composition, and drying and calcining it to obtain a catalyst (S2).
[0052] Hereinafter, each step of the above-mentioned manufacturing method will be described separately.
[0053] Step of preparing a catalyst composition (S1)
[0054] The main catalyst precursor used in this step is a component for introducing the main catalyst component into the above-mentioned catalyst, and can be a compound containing the main catalyst component. More specifically, the main catalyst precursor can be a salt or oxide of Fe, Ni and Co, or a compound containing the metal component, and particularly preferably, it can be a precursor based on Fe, Ni or Co, such as Fe(NO3)2·6H2O, Fe(NO3)2·9H2O, Fe(NO3)3, Fe(OAc)2, Ni(NO3)2·6H2O, Co(NO3)2·6H2O, Co2(CO)8, [Co2(CO)6(t-BuC=CH)], Co(OAc)2.
[0055] The promoter precursor used in this step is a component for introducing the promoter component into the above-mentioned catalyst, and may be a compound containing the promoter component. The promoter precursor may also be a salt or oxide of V and Mo, or a compound containing the metal component, and particularly preferably, may be such as NH4VO3, (NH4)6Mo7O 24 · Materials of 4H2O, Mo(CO)6 or (NH4)MoS4. When the above-exemplified materials are used as precursors, there is an advantage in that the main catalyst component and the co-catalyst component are stably supported.
[0056] Meanwhile, similar to the molar ratio of the main catalyst component to the co-catalyst component in the catalyst, the ratio between the main catalyst precursor and the co-catalyst precursor in the catalyst composition may be 1:0.01 to 1:0.2.
[0057] The Zr precursor is dissolved in the catalyst composition together with the above-mentioned main catalyst precursor and the co-catalyst precursor, loaded together, and then subjected to a calcination process to form Zr oxide. As the Zr precursor, one or more selected from the group consisting of ZrO(NO3)2·xH2O, Zr(NO3)4, Zr(OH)4 and ZrCl4 can be used. The Zr precursors listed above can be easily dissolved and easily loaded in the boehmite pores.
[0058] The polycarboxylic acid may be, for example, a polycarboxylic acid, which is a compound containing two or more carboxyl groups, and has high solubility as a complexing agent, inhibits precipitation, promotes the synthesis of the catalyst, and acts as an activator to increase the synthesis of carbon nanotubes. The polycarboxylic acid may be one or more selected from dicarboxylic acids, tricarboxylic acids, and tetracarboxylic acids. For example, carboxylic acid compounds such as citric acid, oxalic acid, malonic acid, succinic acid, or tartaric acid, or anhydrides thereof may be used.
[0059] Based on the amount of the main catalyst precursor, the polycarboxylic acid may be added in an amount such that the molar ratio between the main catalyst precursor and the polycarboxylic acid is 1:0.01 to 1:0.1, preferably 1:0.03 to 1:0.05. Within the addition amount range of the polycarboxylic acid as described above, precipitation of the metal components of the main catalyst and the co-catalyst does not occur in the catalyst composition, and the occurrence of cracks during the subsequent calcination process can also be suppressed.
[0060] The solvent of the catalyst composition is not particularly limited as long as it can dissolve the above-mentioned main catalyst precursor and co-catalyst precursor, and for example, water is preferably used.
[0061] In the method for producing a catalyst for producing carbon nanotubes according to the present invention, it may further include the step of mixing the catalyst composition and aging it for a certain period of time before adding boehmite to the prepared catalyst composition. Specifically, the mixing may be performed by rotating or stirring at a temperature of 45° C. to 80° C. The aging may be performed for 3 to 60 minutes.
[0062] Drying and calcining step (S2)
[0063] Boehmite as a carrier can be added to the catalyst composition prepared by the previous step so that the main catalyst, the co-catalyst and the Zr are loaded in the carrier. Then, by drying and calcining processes, the main catalyst precursor, the co-catalyst precursor and the Zr precursor can be converted into the main catalyst oxide, the co-catalyst oxide and the Zr oxide.
[0064] The drying in this step may be performed at 60° C. to 200° C. for 4 to 16 hours, and the drying method may be a conventional drying method used in the art, such as oven drying, reduced pressure drying, and freeze drying.
[0065] The calcination in this step may be performed at a temperature of 300° C. to 720° C., preferably 400° C. to 690° C. When the calcination is performed within the above temperature range, most of the main catalyst precursor and the co-catalyst precursor may be converted into the main catalyst component and the co-catalyst component while minimizing the structural collapse of boehmite as a carrier.
[0066] Hereinafter, the present invention will be described in more detail by examples and experimental examples to specifically illustrate the present invention, but the present invention is not limited to these examples and experimental examples. However, embodiments according to the present invention may be modified in various forms, and the scope of the present invention should not be construed as being limited to the embodiments described in detail below. Embodiments of the present invention are provided in order to more completely explain the present invention to those skilled in the art.
[0067] Example 1
[0068] 13.1 g of Co(NO3)2·6H2O, 0.53 g of NH4VO3 and 0.52 g of ZrO(NO3)2·xH2O were dissolved in 20 g of water, and 0.38 g of anhydrous citric acid and polycarboxylic acid were dissolved to prepare a catalyst composition. The catalyst composition was fully stirred and then added to boehmite as a carrier. Then, it was dried at 120°C for 5 hours using an oven and then calcined at 685°C for 1 hour to obtain a catalyst. The Co content in the catalyst obtained in Example 1 was 11.8% by weight, the molar ratio between Co and V was 1:0.1, and the molar ratio between Co and Zr was 1:0.05.
[0069] Comparative Example 1
[0070] A catalyst was obtained in the same manner as in Example 1, except that 0.58 g of Mg(NO3)2·6H2O was used instead of the Zr precursor. The Co content and the molar ratio between Co and V in Catalyst 1 obtained in Comparative Example 1 were the same as those in Example 1, and the molar ratio between Co and Mg was also 1:0.05.
[0071] Comparative Example 2
[0072] A catalyst was obtained in the same manner as in Example 1, except that 0.67 g of Zn(NO3)2·6H2O was used instead of the Zr precursor. The Co content and the molar ratio between Co and V in Catalyst 1 obtained in Comparative Example 1 were the same as those in Example 1, and the molar ratio between Co and Zn was also 1:0.05.
[0073] Comparative Example 3
[0074] A catalyst was obtained in the same manner as in Example 1, except that 0.53 g of Ca(NO3)2·6H2O was used instead of the Zr precursor. The Co content and the molar ratio between Co and V in Catalyst 1 obtained in Comparative Example 1 were the same as those in Example 1, and the molar ratio between Co and Ca was also 1:0.05.
[0075] Example 2
[0076] Except for using 0.35 g of NH4VO3, 0.13 g of ZrO(NO3)2·xH2O and 0.25 g of anhydrous citric acid, the same procedure as in Example 1 was performed. The Co content in Catalyst 2 obtained in Example 2 was 11.4 wt %, the molar ratio between Co and V was 1:0.066, and the molar ratio between Co and Zr was 1:0.0125.
[0077] Example 3
[0078] Except for using 0.35 g of NH4VO3, 0.26 g of ZrO(NO3)2·xH2O and 0.25 g of anhydrous citric acid, the same procedure as in Example 1 was performed. The Co content in Catalyst 2 obtained in Example 2 was 11.4 wt %, the molar ratio between Co and V was 1:0.066, and the molar ratio between Co and Zr was 1:0.025.
[0079] Example 4
[0080] Except for using 0.35 g of NH4VO3, 0.47 g of ZrO(NO3)2·xH2O and 0.25 g of anhydrous citric acid, the same procedure as in Example 1 was performed. The Co content in Catalyst 2 obtained in Example 2 was 11.4 wt%, the molar ratio between Co and V was 1:0.066, and the molar ratio between Co and Zr was 1:0.045.
[0081] Example 5
[0082] Except for using 0.35 g of NH4VO3, 0.52 g of ZrO(NO3)2·xH2O and 0.25 g of anhydrous citric acid, the same procedure as in Example 1 was performed. The Co content in Catalyst 2 obtained in Example 2 was 11.4 wt %, the molar ratio between Co and V was 1:0.066, and the molar ratio between Co and Zr was 1:0.050.
[0083] Example 6
[0084] Except for using 0.35 g of NH4VO3, 0.62 g of ZrO(NO3)2·xH2O and 0.25 g of anhydrous citric acid, the same procedure as in Example 1 was performed. The Co content in Catalyst 2 obtained in Example 2 was 11.4 wt %, the molar ratio between Co and V was 1:0.066, and the molar ratio between Co and Zr was 1:0.060.
[0085] The types of metal additives, Co contents, Co:V molar ratios, and relationships between Co and metal additives in the catalysts obtained in Examples and Comparative Examples are summarized in the following Table 1. Meanwhile, M in the following Table 1 refers to a metal additive.
[0086] [Table 1]
[0087]
[0088] Experimental Example 1. Confirmation of the properties of carbon nanotubes produced using the catalysts of Examples / Comparative Examples
[0089] The catalyst prepared in the above-mentioned embodiment and the comparative example is used to synthesize carbon nanotubes. Specifically, after filling 0.1g of the prepared catalyst in a fixed bed reactor, nitrogen is injected into the fixed bed reactor at 100sccm, and the temperature in the fixed bed reactor is heated to the reaction temperature. Then, ethylene as a carbon source gas and hydrogen as a reducing gas are injected at 100sccm, and the reaction is continued for 60 minutes to synthesize carbon nanotubes. The yield, specific surface area and bulk density of the synthesized carbon nanotubes are measured, and each property is measured using the following method.
[0090] 1) The yield was calculated by measuring the weight of the carbon nanotubes obtained by the reaction and using the following formula.
[0091] Yield = {(weight of recovered carbon nanotubes - weight of added catalyst) / (weight of added catalyst)}
[0092] 2) The specific surface area was measured by a standard measurement method using Trista 2000 from Microtrac.
[0093] 3) The bulk density was calculated by measuring the weight of the carbon nanotubes contained in the container freely falling using a 25 ml SUS measuring cup and dividing the measured weight by the volume of the container.
[0094] The measurement results are summarized in Table 2 below.
[0095] [Table 2]
[0096] Yield (multiple) <![CDATA[Specific surface area (m 2 / g)]]> <![CDATA[Bulk density (kg / m 3 )]]> Example 1 18.4 315 29 Comparative Example 1 18.4 275 31 Comparative Example 2 23.5 270 35 Comparative Example 3 15.4 275 27 Example 2 19.0 327 30 Example 3 19.1 337 31 Example 4 19.2 345 32 Example 5 18.8 330 30 Example 6 18.5 315 29
[0097] It can be seen from Table 2 that when Zr is used as a metal additive, the specific surface area of the carbon nanotubes produced is 300 m 2 / g or more, it was confirmed that carbon nanotubes with a high specific surface area can be synthesized. On the other hand, in the case of Comparative Examples 1 to 3 using other types of metals as additives, carbon nanotubes with a lower specific surface area than the present invention were synthesized. In particular, in the case of Comparative Example 2 using a Zn additive, it was confirmed that the yield was high, but the specific surface area was the lowest. Thus, it was confirmed that the use of Zr has the effect of increasing the specific surface area of the synthesized carbon nanotubes.
[0098] Furthermore, it was confirmed that in the case of Examples 2 to 6 having different Zr contents, carbon nanotubes having a high specific surface area were produced within almost all Zr content ranges, and in particular, considering only the specific surface area of the carbon nanotubes, carbon nanotubes having a particularly high specific surface area were synthesized within a Co:M molar ratio range of 1:0.02 to 1:0.05.
Claims
1. A catalyst for producing carbon nanotubes, the catalyst comprising: a boehmite support; and The main catalyst component, the co-catalyst component and Zr are supported on the carrier.
2. The catalyst for producing carbon nanotubes according to claim 1, wherein The boehmite carrier has a number average particle size of 20 μm to 100 μm.
3. The catalyst for producing carbon nanotubes according to claim 1, wherein The main catalyst component is at least one selected from the group consisting of Ni, Co and Fe.
4. The catalyst for producing carbon nanotubes according to claim 1, wherein The co-catalyst component is at least one selected from the group consisting of Mo and V.
5. The catalyst for producing carbon nanotubes according to claim 1, wherein The molar ratio of the main catalyst component to the Zr is 1:0.01 to 1:0.
1.
6. The catalyst for producing carbon nanotubes according to claim 1, wherein The molar ratio of the main catalyst component to the co-catalyst component is 1:0.01 to 1:0.
2.
7. The catalyst for producing carbon nanotubes according to claim 1, wherein The main catalyst component may be included in an amount of 5 to 20 wt % based on the total weight of the catalyst.
8. A method for preparing a catalyst for producing carbon nanotubes, the method comprising the following steps: preparing a catalyst composition (S1) by adding a main catalyst precursor, a co-catalyst precursor, a Zr precursor and a polycarboxylic acid to a solvent; as well as A boehmite support is added to the catalyst composition, and it is dried and calcined to obtain a catalyst (S2).
9. The method for preparing a catalyst for producing carbon nanotubes according to claim 8, wherein: The molar ratio of the main catalyst precursor to the polycarboxylic acid added in step S1 is 1:0.01 to 1:0.
1.
10. The method for preparing a catalyst for producing carbon nanotubes according to claim 8, wherein: The calcination is performed at 300°C to 720°C.
Citation Information
Patent Citations
Directly-prepared ultrahigh-purity carbon nanotube and preparation method thereof
CN102145883A
Carbon nanotube having high specific surface area and method for manufacturing same
CN104870363A
Method for producing double wall carbon nanotube and composition containing double wall carbon nanotube
JP2006111458A
Short carbon nanotube for catalyst support, carbon nanatube impregnated catalyst using the carbon nanotube and fuel cell adopting the same
KR1020050072634A
Carbon nanotube having high specific surface area and method for manufacturing same
WO2015047042A1