Thin film transistor and manufacturing method thereof

By introducing a second metal element oxide contact layer into the thin film transistor, the problem of increased conductivity caused by insufficient oxygen in the active layer is solved, the stability and reliability of the thin film transistor are improved, and the friction between the source and drain electrodes is reduced. Contact resistance.

CN118872075APending Publication Date: 2024-10-29JUSUNG ENG
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380026965.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-07
Filing Date
2023-03-10
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

During the manufacturing process of thin film transistors, due to the exposure of the active layer to etching gases, oxygen is insufficient, resulting in increased conductivity, resulting in component short circuits and inability to drive stably.

Method used

A contact layer containing an oxide of a second metal element, such as ruthenium (Ru), is introduced into the thin film transistor to prevent oxygen from moving from the active layer to the source and drain electrodes and improve the stability of the active layer. The contact layer is composed of a variety of metal elements and their oxides, with moderate impurity content and a thickness controlled within a specific range to prevent conductivity from increasing.

Benefits of technology

It effectively prevents the conductivity of the active layer from increasing, improves the switching characteristics and reliability of thin film transistors, reduces the contact resistance between the source and drain, and enhances the stability and characteristics of the component.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118872075A_ABST
    Figure CN118872075A_ABST
Patent Text Reader

Abstract

Provided are a thin film transistor and a method for manufacturing the same, in particular, a thin film transistor having improved characteristics and a method for manufacturing the same. A thin film transistor according to an exemplary embodiment includes a gate electrode, an active layer including an oxide of a first metal element and disposed to be spaced apart from the gate electrode in a vertical direction, a source electrode and a drain electrode disposed to be spaced apart from each other on the active layer, and a contact layer disposed between the active layer and the source electrode and the drain electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a thin film transistor and a method for manufacturing the same, and more particularly to a thin film transistor with improved characteristics and a method for manufacturing the same. Background Art

[0002] Thin-film transistors (TFTs) are used as circuits for independently driving each pixel in devices such as semiconductor devices, liquid crystal displays (LCDs), and organic electroluminescent (EL) displays.

[0003] The thin film transistor is formed on the bottom substrate of the display device together with the gate line and the data line. That is, the thin film transistor is composed of a gate which is part of the gate line, an active layer used as a channel, a source and a drain which are part of the data line, and an insulating layer with the gate.

[0004] In the process of manufacturing a thin film transistor, the active layer is exposed to an etching gas for patterning. When the active layer is exposed to the etching gas, the exposed surface of the active layer is damaged by the etching gas and loses oxygen. In addition, the active layer is connected to the source and drain (i.e., part of the data line). Here, when the thin film transistor is driven, oxygen moves from the active layer to the source and drain, and thus the active layer loses oxygen. As described above, when a deficiency of oxygen is generated in the active layer, the active layer inadvertently increases conductivity to act as a conductor. Therefore, there is a defect that the thin film transistor cannot be stably driven due to a component short circuit.

[0005] (Prior Technical Document)

[0006] Patent Document 1KR10-2004-0013273A Summary of the invention

[0007] Technical issues

[0008] The present invention provides a thin film transistor capable of preventing oxygen deficiency from being generated in an active layer while improving stability, and a method for manufacturing the same.

[0009] Technical Solution

[0010] According to an exemplary embodiment, a thin film transistor includes: a gate, an active layer including an oxide of a first metal element and disposed to be spaced apart from the gate in a vertical direction, a source electrode and a drain electrode disposed to be spaced apart from each other on the active layer, and a contact layer including a second metal element and disposed between the active layer and the source electrode and the drain electrode.

[0011] The contact layer may contain a metal or an alloy containing a second metal element.

[0012] The second metal element may include ruthenium (Ru).

[0013] The contact layer may include an oxide of the second metal element.

[0014] The oxide of the first metal element and the oxide of the second metal element may have different compositions from each other.

[0015] Each of the oxide of the first metal element and the oxide of the second metal element may include zinc oxide doped with a plurality of impurities, and the oxide of the first metal element and the oxide of the second metal element may have different impurity contents from each other.

[0016] The impurity content of the oxide of the second metal element may be greater than the impurity content of the oxide of the first metal element.

[0017] These impurities may include at least one of indium (In), gallium (Ga), tungsten (W), lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), manganese (Mn), technetium (Tc), rhenium (Re), iron (Fe), ruthenium (Ru), osmium (Os), cobalt (Co), rhodium (Rh), iridium (Ir), nickel (Ni), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), boron (B), thallium (Tl), silicon (Si), germanium (Ge), tin (Sn), lead (Pb), phosphorus (P) and arsenic (As).

[0018] The oxide of the first metal element may contain impurities at more than about 20 atomic percent (at%) and less than about 40 at% relative to the entire oxide of the first metal element, and the oxide of the second metal element may contain impurities at more than about 40 at% and less than about 60 at% relative to the entire oxide of the second metal element.

[0019] The oxygen (O) content of the oxide of the second metal element may be less than the oxygen content of the oxide of the first metal element.

[0020] The thickness of the contact layer can be about to about

[0021] The thin film transistor may further include an insulating layer, which is disposed on the active layer and has a contact hole exposing a portion of the surface of the active layer, wherein the contact layer may be disposed on a portion of the surface of the active layer exposed by the contact hole, and the source and drain may contact the contact layer and extend onto the insulating layer.

[0022] According to another exemplary embodiment, a method for manufacturing a thin film transistor includes: preparing a substrate on which a gate is formed and an active layer is disposed to be spaced apart from the gate in a vertical direction; and forming a contact layer on the active layer to connect the active layer to a source electrode and a drain electrode.

[0023] Preparing the substrate may include preparing a substrate having an insulating layer having a contact hole on the active layer exposing a portion of a surface of the active layer, and forming the contact layer may include forming the contact layer on the portion of the surface of the active layer exposed by the contact hole.

[0024] When forming the contact layer, the contact layer may be formed on a portion of the surface of the active layer to be approximately to about Thickness.

[0025] The contact layer may be formed by repeating an atomic layer deposition process several times including a process cycle of supplying a source gas including a metal element onto the active layer and supplying a reaction gas including oxygen onto the active layer.

[0026] When the source gas is supplied, a first source gas containing zinc (Zn) and a second source gas containing at least one of indium (In), gallium (Ga), tungsten (W), lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), manganese (Mn), technetium (Tc), rhenium (Re), iron (Fe), ruthenium (Ru), osmium (Os), cobalt (Co), rhodium (Rh), iridium (Ir), nickel (Ni), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), boron (B), thallium (Tl), silicon (Si), germanium (Ge), tin (Sn), lead (Pb), phosphorus (P) and arsenic (As) may be supplied simultaneously.

[0027] When the source gas is supplied, the supply of the source gas may be controlled such that a supply amount of the second source gas is greater than a supply amount of the first source gas.

[0028] The method of manufacturing a thin film transistor may further include forming a source electrode and a drain electrode on the contact layer.

[0029] According to yet another exemplary embodiment, a thin film transistor includes: a gate, an active layer, a first insulating layer, a second insulating layer, a contact layer, and a source and a drain, wherein the active layer contains an oxide of a first metal element and is arranged to be spaced apart from the gate in a vertical direction; the first insulating layer is arranged on the active layer and has a first contact hole exposing a portion of the surface of the active layer; the second insulating layer is arranged on the first insulating layer and exposes the first contact hole and a portion of the surface of the first insulating layer extending from the first contact hole; the contact layer contains a second metal element and is arranged on a portion of the surface of the active layer exposed by the first insulating layer; the source and the drain are arranged on the contact layer to be spaced apart from each other and extend to a portion of the surface of the first insulating layer exposed by the second insulating layer.

[0030] The first insulating layer may include silicon oxide, and the second insulating layer may include silicon nitride.

[0031] The first metal element may include at least one of indium (In), gallium (Ga), and zinc (Zn), and the second metal element may include at least one of indium (In), gallium (Ga), zinc (Zn), and ruthenium (Ru).

[0032] According to yet another exemplary embodiment, a method for manufacturing a thin film transistor includes: preparing a substrate having a gate and an active layer arranged to be spaced apart from the gate in a vertical direction and a portion of a surface of which is exposed by a contact hole formed in a first insulating layer; and forming a second insulating layer containing silicon nitride on the first insulating layer.

[0033] According to yet another exemplary embodiment, a method for manufacturing a thin film transistor includes: preparing a substrate having a gate and an active layer disposed to be spaced apart from the gate in a vertical direction and having a portion of its surface exposed by a contact hole formed in each of a laminated first insulating layer and a second insulating layer; and forming a contact layer connecting the active layer to a source and a drain on a portion of the exposed surface of the active layer by an area selective-atomic layer deposition method.

[0034] The contact layer may include a metal oxide doped with a plurality of impurities.

[0035] These impurities may include at least one of indium (In), gallium (Ga), tungsten (W), lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), manganese (Mn), technetium (Tc), rhenium (Re), iron (Fe), ruthenium (Ru), osmium (Os), cobalt (Co), rhodium (Rh), iridium (Ir), nickel (Ni), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), boron (B), thallium (Tl), silicon (Si), germanium (Ge), tin (Sn), lead (Pb), phosphorus (P), and arsenic (As).

[0036] The method of manufacturing a thin film transistor may further include etching the metal oxide layer doped with the impurities formed on the second insulating layer after forming the contact layer.

[0037] The metal oxide layer doped with these impurities can be etched with hydrogen bromide (HBr).

[0038] According to yet another exemplary embodiment, a method for manufacturing a thin film transistor includes: preparing a substrate having a gate and an active layer arranged to be spaced apart from the gate in a vertical direction and a portion of a surface of which is exposed by a first contact hole formed in a first insulating layer comprising silicon oxide; forming a second insulating layer comprising silicon nitride on the first insulating layer, in which a second contact hole exposing the first contact hole is formed; and forming a contact layer connecting the active layer to a source and a drain on a portion of the exposed surface of the active layer by an area selective atomic layer deposition method.

[0039] According to yet another exemplary embodiment, a thin film transistor includes: a gate, an active layer, a source and a drain, and a ruthenium oxide layer, wherein the active layer is arranged to be spaced apart from the gate in a vertical direction and contains at least one of indium (In), gallium (Ga) and zinc (Zn); the source and the drain are arranged to be spaced apart from each other on the active layer; and the ruthenium oxide layer is arranged between the active layer and the source and the drain.

[0040] According to yet another exemplary embodiment, a thin film transistor includes: a gate, an active layer, a source and a drain, a high-concentration metal oxide layer and a ruthenium oxide layer, wherein the active layer is arranged to be spaced apart from the gate in a vertical direction and contains at least one of indium (In), gallium (Ga) and zinc (Zn); the source and the drain are arranged to be spaced apart from each other on the active layer; the high-concentration metal oxide layer is arranged between the active layer and the source and the drain and the impurity content of the metal oxide layer is greater than the impurity content of the active layer; and the ruthenium oxide layer is arranged between the high-concentration metal oxide layer and the source and the drain.

[0041] According to yet another exemplary embodiment, a method for manufacturing a thin film transistor includes: preparing a substrate on which a gate is formed and an active layer is arranged to be spaced apart from the gate in a vertical direction; and forming a ruthenium oxide layer on the active layer to connect the active layer to a source and a drain.

[0042] According to yet another exemplary embodiment, a method for manufacturing a thin film transistor includes: preparing a substrate on which a gate is formed and an active layer is arranged to be spaced apart from the gate in a vertical direction; forming a high-concentration metal oxide layer on the active layer and the content of multiple impurities in the metal oxide layer is greater than the content of multiple impurities in the active layer; and forming a ruthenium oxide layer on the high-concentration metal oxide layer to connect the active layer to a source and a drain.

[0043] These impurities of the metal oxide layer or the active layer may include at least one of indium (In), gallium (Ga), tungsten (W), lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), manganese (Mn), technetium (Tc), rhenium (Re), iron (Fe), ruthenium (Ru), osmium (Os), cobalt (Co), rhodium (Rh), iridium (Ir), nickel (Ni), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), boron (B), thallium (Tl), silicon (Si), germanium (Ge), tin (Sn), lead (Pb), phosphorus (P) and arsenic (As).

[0044] Beneficial Effects

[0045] According to this embodiment, a contact layer for preventing oxygen defects in the active layer may be provided between the active layer and the source and drain electrodes to prevent the active layer from conducting electricity and improve switching characteristics.

[0046] In addition, the contact resistance between the active layer and the source and drain electrodes can be effectively reduced, thereby improving the characteristics and reliability of the components. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 is a schematic diagram illustrating a thin film transistor according to an exemplary embodiment.

[0048] Figure 2 is a schematic diagram illustrating a thin film transistor according to another exemplary embodiment.

[0049] Figure 3 is a schematic diagram illustrating a method of manufacturing a thin film transistor according to an exemplary embodiment.

[0050] Figure 4is a schematic diagram illustrating a method of manufacturing a thin film transistor according to another exemplary embodiment.

[0051] Figure 5 is a schematic diagram illustrating a thin film transistor according to still another exemplary embodiment.

[0052] Figure 6 is a schematic diagram illustrating a thin film transistor according to still another exemplary embodiment. DETAILED DESCRIPTION

[0053] Hereinafter, exemplary embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, the present invention may be implemented in different forms and should not be construed as being limited to the exemplary embodiments described herein. Rather, these embodiments are provided so that the present invention will be thorough and complete and fully convey the scope of the present invention to those having ordinary knowledge in the art.

[0054] It will be understood that when a layer, region or substrate is referred to as being “on” another, it can be directly on the other, or one or more intervening layers, regions or substrates may also be present.

[0055] Furthermore, spatially relative terms such as "above" or "top", and "below" or "bottom", etc., may be used herein for ease of description to describe the relationship of one component or feature to another component or feature as shown in the accompanying drawings. It should be understood that these spatially relative terms are intended to cover different orientations of the device in use or operation in addition to the orientation shown in the drawings. In the accompanying drawings, the dimensions of layers and regions may be exaggerated for clarity of illustration. Like reference numerals refer to like components throughout.

[0056] Figure 1 is a schematic diagram illustrating a thin film transistor according to an exemplary embodiment, and Figure 2 is a schematic diagram illustrating a thin film transistor according to another exemplary embodiment.

[0057] refer to Figure 1 and Figure 2 According to an exemplary embodiment, the thin film transistor includes a gate 150, an active layer 130 disposed to be spaced apart from the gate 150 in a vertical direction, a source electrode 180a and a drain electrode 180b disposed to be spaced apart from each other on the active layer 130, and a contact layer 170 disposed between the active layer 130 and the source electrode 180a and the drain electrode 180b.

[0058] like Figure 1As shown, the thin film transistor according to the exemplary embodiment can be a top gate type thin film transistor including the following components: an active layer 130 arranged on a substrate 110, a gate insulating layer 140 arranged on the active layer 130, a gate 150 arranged on the gate insulating layer 140, a source 180a and a drain 180b arranged on the active layer 130 to be spaced apart from each other, and the gate insulating layer 140 and the gate 150 are located between the source 180a and the drain 180b, and a plurality of contact layers 170 respectively arranged between the active layer 130 and the source 180a and between the active layer 130 and the drain 180b.

[0059] A transparent substrate may be used as the substrate 110. For example, when a flexible display is implemented, a silicon substrate, a glass substrate, or a plastic substrate may be used as the substrate 110. In addition, a reflective substrate may be used as the substrate 110, and in this case, a metal substrate may be used. The metal substrate may be made of stainless steel (SUS), titanium (Ti), molybdenum (Mo), or an alloy of the above metals. A buffer layer 120 may be provided on the substrate 110. Here, the buffer layer 120 may be made of a material including silicon oxide (SiO 2 ) insulating material.

[0060] The active layer 130 may be disposed on the buffer layer 120. The active layer 130 may be disposed on a predetermined region of the buffer layer 120, and a gate 150 to be described below may be disposed to be spaced apart from a top side of the active layer 130 to overlap a portion of the active layer 130.

[0061] Here, the active layer 130 may be made of metal oxide. That is, the active layer 130 may be provided as a metal oxide thin film or a plurality of metal oxide thin films having different compositions. For example, the active layer 130 may include an oxide containing at least one of indium (In), gallium (Ga), and zinc (Zn).

[0062] In the related art, the active layer is made of amorphous silicon or crystalline silicon. However, since the substrate of the thin film transistor using silicon must use a glass substrate, such a substrate is not only heavy, but also has the disadvantage of not being used as a flexible display device. Therefore, in order to implement a high-speed device, that is, to improve mobility, a metal oxide film with a high carrier concentration and excellent conductivity can be used as the active layer.

[0063] In addition, the active layer 130 may be made of a material including zinc oxide doped with a plurality of impurities. Here, the impurities may include at least one of indium (In), gallium (Ga), tungsten (W), lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), manganese (Mn), technetium (Tc), rhenium (Re), iron (Fe), ruthenium (Ru), osmium (Os), cobalt (Co), rhodium (Rh), iridium (Ir), nickel (Ni), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), cadmium (Cd), mercury (Hg), boron (B), thallium (Tl), silicon (Si), germanium (Ge), tin (Sn), lead (Pb), phosphorus (P), arsenic (As), antimony (Sb) and bismuth (Bi).

[0064] For example, indium (In) may be a metal having a relatively low energy gap and a relatively high standard electrode potential, and may therefore have the characteristics of increasing charge concentration and improving mobility. On the other hand, gallium (Ga) may be a metal having a relatively high energy gap and a relatively low standard electrode potential, and may have the characteristics of reducing charge concentration and improving stability. Therefore, the conductivity of the active layer 130 may be adjusted by controlling the content of impurities contained in the metal oxide film. As described above, the active layer 130 made of metal oxide has the characteristics that the conductivity decreases when the oxygen content increases, and the conductivity increases when the oxygen content decreases.

[0065] In addition, the active layer 130 may contain magnesium (Mg) as an impurity to form a p-type active layer, and silicon (Si) as an impurity to form an n-type active layer. In addition, the active layer 130 may contain various noble metals such as ruthenium (Ru), platinum (Pt), gold (Au), silver (Ag), rhodium (Rh), palladium (Pd), osmium (Os), iridium (Ir), yttrium (Yi), tungsten (W), molybdenum (Mo), etc.

[0066] The gate insulating layer 140 may be disposed on the active layer 130. As described above, the gate insulating layer 140 may be disposed on a portion of the active layer 130, and the gate insulating layer 140 may be made of silicon oxide (SiO2) having excellent adhesion to metal materials and excellent dielectric strength. 2 ), silicon nitride (SiN), alumina (Al 2 O 3 ) and zirconium oxide (ZrO 2 ) is made of an inorganic insulating layer or multiple insulating materials.

[0067] The gate 150 may be formed on the gate insulating layer 140. The gate 150 may be made of a conductive material, such as at least one of aluminum (Al), neodymium (Nd), silver (Ag), chromium (Cr), titanium (Ti), tantalum (Ta), molybdenum, or alloys thereof. In addition, the gate 150 may be formed not only as a single-layer structure but also as a multilayer structure including a plurality of metal layers. That is, the gate 150 may be formed as a double-layer structure including a metal layer made of chromium (Cr), titanium (Ti), tantalum (Ta), and molybdenum (Mo) and having excellent physical and chemical properties, and a metal layer made of aluminum (Al) series, silver (Ag) series, or copper (Cu) series and having low specific resistance.

[0068] The insulating layer 160 having a contact hole covering the gate 150 may be disposed on the active layer 130, and a portion of the surface of the active layer 130 may be exposed on both sides of the gate 150 through the contact hole. That is, the contact hole may be defined in the insulating layer 160 so that the source electrode 180a and the drain electrode 180b are each electrically connected to the active layer 130 through the contact hole. The insulating layer 160 may be made of a material including silicon oxide (SiO 2 ) insulating material.

[0069] The contact layer 170 is disposed on a portion of the surface of the active layer 130 exposed by the contact hole. The contact layer 170 contains a metal element. That is, the contact layer 170 may be made of a metal or an alloy. Here, the contact layer 170 may be made of ruthenium (Ru) or a ruthenium alloy. Moreover, the contact layer 170 may be made of a metal oxide. That is, the contact layer 170 may contain a metal oxide film. Here, like the active layer 130, the contact layer 170 may be provided as a single-layer metal oxide film or a plurality of metal oxide films having different compositions. For example, the contact layer 170 may contain ruthenium oxide. In addition, the contact layer 170 may be made of a material containing zinc oxide doped with impurities. Here, the impurities may include at least one material of indium (In), gallium (Ga), tungsten (W), lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), manganese (Mn), technetium (Tc), rhenium (Re), iron (Fe), ruthenium (Ru), osmium (Os), cobalt (Co), rhodium (Rh), iridium (Ir), nickel (Ni), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), cadmium (Cd), mercury (Hg), boron (B), thallium (Tl), silicon (Si), germanium (Ge), tin (Sn), lead (Pb), phosphorus (P), arsenic (As), antimony (Sb), and bismuth (Bi).

[0070] The contact layer 170 may be made of a metal oxide having a different composition from the metal oxide forming the active layer 130. That is, when the metal oxide included in the active layer 130 is referred to as an oxide of a first metal element, and the metal oxide included in the contact layer 170 is referred to as an oxide of a second metal element, the oxide of the first metal element and the oxide of the second metal element may have different compositions. Here, when the oxide of each of the first metal element and the second metal element includes zinc oxide doped with impurities, the oxide of the second metal element may have a greater impurity content than the oxide of the first metal element, wherein the impurities include indium (In), gallium (Ga), tungsten (W), lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (T), etc. ), chromium (Cr), molybdenum (Mo), manganese (Mn), technetium (Tc), rhenium (Re), iron (Fe), ruthenium (Ru), osmium (Os), cobalt (Co), rhodium (Rh), iridium (Ir), nickel (Ni), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), cadmium (Cd), mercury (Hg), boron (B), thallium (Tl), silicon (Si), germanium (Ge), tin (Sn), lead (Pb), phosphorus (P), arsenic (As), antimony (Sb) and bismuth (Bi). For example, when the oxide of the first metal element forming the active layer 130 contains about 20at% or more and less than about 40at% of impurities relative to the entire oxide of the first metal element, the oxide of the second metal element may contain about 40at% or more and less than about 60at% of impurities relative to the entire oxide of the second metal element. As described above, the oxide of the second metal element having a high impurity content may have a smaller oxygen content than the oxide of the first metal element.

[0071] If the contact layer 170 is not provided, and the source electrode 180a and the drain electrode 180b are disposed on the active layer 130, the active layer 130 may be exposed to the etching gas in the process of forming the contact hole in the insulating layer 160 to form the source electrode 180a and the drain electrode 180b. When the active layer 130 is exposed to the etching gas, the active layer 130 may be damaged by the etching gas from the surface of the active layer 130 to a predetermined depth and lose oxygen, and then become an oxygen-deficient state. In addition, when the source electrode 180a and the drain electrode 180b are directly disposed on the surface of the active layer 130 damaged by the etching gas as described above, oxygen may move from the active layer 130 to the source electrode 180a and the drain electrode 180b when the thin film transistor is driven. As described above, when the oxygen deficiency is generated in the active layer, the active layer may inadvertently increase the conductivity and thus become conductive, and a component short circuit may occur so that the thin film transistor cannot be stably driven.

[0072] On the other hand, when the contact layer 170 made of a metal, an alloy, or a metal oxide is disposed between the active layer 130 and the source and drain electrodes 180a and 180b as shown in the exemplary embodiment, oxygen or a metal material contained in the contact layer 170 may be filled to a position where oxygen is separated from the active layer 130. That is, the oxygen or the metal material contained in the contact layer 170 may diffuse at a position where oxygen is separated from the active layer 130 to prevent oxygen from moving from the active layer 130 to the source and drain electrodes 180a and 180b and prevent the active layer from becoming conductive.

[0073] In this case, the contact layer 170 may have a thickness of about to about Here, when the contact layer 170 has a thickness less than about When the thickness of the contact layer 170 exceeds about When the thickness is greater than 100 Å, the process time may be excessively increased, resulting in a defect that limits the miniaturization of thin film transistors. Therefore, the contact layer 170 may preferably have a thickness of about 100 Å. to about Thickness.

[0074] The source 180a and the drain 180b are disposed on the contact layer 170. That is, each of the source 180a and the drain 180b may be provided to contact the contact layer 170 disposed in the contact hole, so that the source 180a and the drain 180b are spaced apart from each other and the gate 150 is located between the source 180a and the drain 180b. Here, the source 180a and the drain 180b may be provided to contact the contact layer 170 and extend onto the insulating layer 160. The source 180a and the drain 180b may be formed by the same process using the same material, and may be made of a conductive material, for example, may be made of at least one of aluminum (Al), neodymium (Nd), silver (Ag), chromium (Cr), titanium (Ti), tantalum (Ta), molybdenum (Mo), and alloys of the above metals. That is, the gate 150 may be made of the same material, but may be made of different materials. In addition, each of the source electrode 180a and the drain electrode 180b may be provided as a single-layer structure or a multi-layer structure. Here, these layers may include different metals or alloys, respectively.

[0075] like Figure 2As shown, according to another exemplary embodiment, a thin film transistor may be a bottom gate type thin film transistor including the following components: a gate 150 disposed on a substrate 110, a gate insulating layer 140 disposed on the gate 150, an active layer 130 disposed on the gate insulating layer 140, a source electrode 180a and a drain electrode 180b disposed on the active layer 130 and spaced apart from each other, and a plurality of contact layers 170 disposed between the active layer 130 and the source electrode 180a and between the active layer 130 and the drain electrode 180b, respectively.

[0076] Even in the case of such a bottom gate type thin film transistor, Figure 1 The contents related to the thin film transistor according to the exemplary embodiment can still be applied as before. That is, even in the example of the thin film transistor according to another exemplary embodiment, these contact layers 170 can still be respectively disposed between the active layer 130 and the source electrode 180a and between the active layer 130 and the drain electrode 180b. As described above, even in the example of the thin film transistor according to another exemplary embodiment, except for the stacking sequence of the gate insulating layer 140 and the gate electrode, the contents described in the thin film transistor according to the aforementioned exemplary embodiment can still be applied as before, and therefore repeated descriptions will be omitted.

[0077] Figure 3 is a schematic diagram illustrating a method of manufacturing a thin film transistor according to an exemplary embodiment.

[0078] refer to Figure 3 , a method for manufacturing a thin film transistor according to an exemplary embodiment includes a process of preparing a substrate 110 on which a gate electrode 150 and an active layer 130 disposed to be spaced apart from the gate electrode 150 in a vertical direction are formed, and a process of forming a contact layer 170 connecting the active layer 130 to each of a source electrode 180a and a drain electrode 180b.

[0079] First, in the process of preparing the substrate 110, as Figure 3 As shown in (a), a substrate 110 having a gate electrode 150 and an active layer 130 spaced apart from the gate electrode 150 in a vertical direction formed thereon is prepared. Here, in the process of preparing the substrate 110, in order to manufacture a top gate type thin film transistor, a substrate 110 in which the active layer 130 is formed on the substrate 110, the gate insulating layer 140 is formed on the active layer 130, and the gate electrode 150 is formed on the gate insulating layer 140 may be prepared. In addition, a buffer layer 120 may be further formed between the substrate 110 and the active layer 130, and an insulating layer 160 having a contact hole exposing a portion of the surface of the active layer 130 to form a source electrode 180a and a drain electrode 180b may be further formed on the active layer 130.

[0080] In the process of forming the contact layer 170, as Figure 3As shown in (b), a contact layer 170 connecting the active layer 130 to each of the source electrode 180a and the drain electrode 180b is formed on the active layer 130. Here, the contact layer 170 may be formed on a portion of the surface of the active layer 130 exposed by the contact hole of the insulating layer 160.

[0081] As described above, the contact layer 170 may be formed of a metal, an alloy, or a metal oxide. The contact layer 170 may be formed by various thin film forming processes. For example, in order to form the contact layer 170 using a metal oxide, the process of forming the contact layer 170 may be performed by repeatedly performing several process cycles, wherein the process cycle includes a process of supplying a source gas containing a metal element to the active layer 130 and a process of supplying a reaction gas containing oxygen to the active layer 130. Such an atomic layer deposition process may be performed by repeatedly performing several process cycles, in which a process of supplying a source gas containing a metal element, a process of blowing off the source gas, a process of supplying a reaction gas containing oxygen, and a process of blowing off the reaction gas are sequentially performed.

[0082] Here, in the process of supplying the source gas, a first source gas containing zinc (Zn) and a first source gas containing indium (In), gallium (Ga), tungsten (W), lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), manganese (Mn), technetium (Tc), etc. may be supplied simultaneously. The first source gas containing zinc (Zn) and the second source gas containing impurities such as indium (In), gallium (Ga), and tungsten (W) may be supplied at the same time, and thus, the contact layer 170 may be formed using a material containing zinc oxide doped with impurities such as indium (In), gallium (Ga), and tungsten (W).

[0083] In the process of supplying source gas, the supply of source gas may be controlled such that the supply amount of the second source gas is greater than the supply amount of the first source gas. Therefore, the metal oxide forming the contact layer 170 may be formed to contain impurities at about 40 at % or more and less than about 60 at % relative to the total amount.

[0084] After the process of forming the contact layer 170, as Figure 3 As shown in (c), a process of forming a source electrode 180 a and a drain electrode 180 b on the contact layer 170 may be performed.

[0085] Figure 4 is a schematic diagram illustrating a method of manufacturing a thin film transistor according to another exemplary embodiment.

[0086] In a method for manufacturing a thin film transistor according to another exemplary embodiment, in a process of preparing a substrate 110, in order to manufacture a bottom gate type thin film transistor, a gate 150 may be formed on the substrate 110, a gate insulating layer 140 may be formed on the gate 150, and an active layer 130 may be formed on the gate insulating layer 140 to prepare the substrate 110. In addition, a buffer layer 120 may be further formed between the substrate 110 and the gate 150.

[0087] Furthermore, although these contact layers 170 are Figure 4 1 and 13. Although the contact layer 170 is shown as being formed on different regions to be spaced apart from each other, in a method for manufacturing a thin film transistor according to yet another exemplary embodiment, the contact layer 170 may be formed as a single-layer structure covering the top surface and the side surfaces of the active layer 130. Except for this structure, the contents described in the method for manufacturing a thin film transistor according to the aforementioned exemplary embodiment are still applicable, and thus repeated descriptions will be omitted.

[0088] Figure 5 is a schematic diagram illustrating a thin film transistor according to still another exemplary embodiment.

[0089] refer to Figure 5 According to yet another exemplary embodiment, a thin film transistor includes a gate 150, an active layer 130 disposed to be spaced apart from the gate 150 in a vertical direction, a first insulating layer 160 disposed on the active layer 130 and having a first contact hole (not shown) exposing a portion of a surface of the active layer 130, a second insulating layer 165 disposed on the first insulating layer 160 and exposing the first contact hole and a portion of the surface of the first insulating layer 160 extending from the first contact hole, a contact layer 170 disposed on a portion of the surface of the active layer 130 exposed by the first insulating layer 160, and a source electrode 180a and a drain electrode 180b disposed on the contact layer 170 to be spaced apart from each other and extending to a portion of the surface of the first insulating layer 160 exposed by the second insulating layer 165.

[0090] The thin film transistor according to still another exemplary embodiment may additionally provide a second insulating layer 165 unlike the thin film transistor according to the exemplary embodiment, and therefore, the contents described about the thin film transistor according to the exemplary embodiment may be applied as is. Here, since the first contact hole and the first insulating layer 160 of the thin film transistor according to still another exemplary embodiment have the same configuration as the contact hole and the insulating layer 160 of the thin film transistor according to the aforementioned exemplary embodiment, they will be denoted by the same reference numerals.

[0091] In more detail, a thin film transistor according to yet another exemplary embodiment includes a gate 150, an active layer 130 including an oxide of a first metal element and disposed to be spaced apart from the gate 150 in a vertical direction, a first insulating layer 160 disposed on the active layer 130 and having a first contact hole exposing a portion of a surface of the active layer 130, a second insulating layer 165 disposed on the first insulating layer 160 and exposing the first contact hole and a portion of the surface of the first insulating layer 160 extending from the first contact hole, a contact layer 170 including a second metal element and disposed on a portion of the surface of the active layer 130 exposed by the first insulating layer 160, and a source electrode 180a and a drain electrode 180b disposed on the contact layer 170 to be spaced apart from each other and extending to a portion of the surface of the first insulating layer 160 exposed by the second insulating layer 165.

[0092] Here, the first insulating layer 160 and the second insulating layer 165 may have different compositions. That is, the first insulating layer 160 may include silicon oxide (SiO), and the second insulating layer 165 may include silicon nitride (SiN). Here, the second insulating layer 165 may be formed on the first insulating layer 160 and have a second contact hole larger than the first contact hole at a position overlapping with the first contact hole defined in the first insulating layer 160. Therefore, when the second insulating layer 165 is disposed on the first insulating layer 160, the first contact hole and the surface of the first insulating layer extending from the first contact hole may be exposed. In addition, the active layer 130 may be made of an oxide of a first metal element including at least one of indium (In), gallium (Ga), and zinc (Zn), and the contact layer 170 may include: a second metal element including at least one of indium (In), gallium (Ga), zinc (Zn), and ruthenium (Ru) as described above.

[0093] As described above, when the second insulating layer 165 is additionally disposed on the first insulating layer 160, the contact layer 170 may be formed by an area selective atomic layer deposition (AS-ALD) method. Here, the area selective atomic layer deposition method may refer to a method of selectively depositing a thin film only on a surface of a specific area by an atomic layer deposition method, and various conventional area selective atomic layer deposition methods may be applied to form the contact layer 170. In addition, the contact layer 170 may be selectively formed on a portion of the exposed surface of the active layer 130 using a deposition method using a shield.

[0094] That is, the method for manufacturing a thin film transistor according to still another exemplary embodiment may include a process of preparing a substrate 110 having a gate electrode 150 and an active layer 130 disposed to be spaced apart from the gate electrode 150 in a vertical direction and having a portion of its surface exposed by a first contact hole formed in a first insulating layer 160, and a process of forming a second insulating layer 165 including silicon nitride on the first insulating layer 160. In this case, a portion of the surface of the active layer 130 may be exposed by the first contact hole and the second contact hole, which are respectively formed in the stacked first insulating layer 160 and the second insulating layer 165, and a contact layer 170 connecting the active layer 130 to the source electrode 180a and the drain electrode 180b by an area selective atomic layer deposition method may be formed on a portion of the exposed surface of the active layer 130.

[0095] As described above, even when the contact layer 170 is selectively formed on a portion of the exposed surface of the active layer 130, a residual layer formed during the process of forming the contact layer 170 may be formed on the second insulating layer 165. For example, when the contact layer 170 includes a metal oxide doped with impurities, the metal oxide layer doped with impurities may remain on the second insulating layer 165. Therefore, in an exemplary embodiment, after the process of forming the contact layer 170, a process of etching the metal oxide layer doped with impurities formed on the second insulating layer 165 may be further performed. Here, the metal oxide layer doped with impurities may be etched with hydrogen bromide (HBr).

[0096] Figure 6 is a schematic diagram illustrating a thin film transistor according to still another exemplary embodiment.

[0097] refer to Figure 6 According to yet another exemplary embodiment, a thin film transistor includes a gate 150, an active layer 130 disposed to be spaced apart from the gate 150 in a vertical direction, a source electrode 180a and a drain electrode 180b disposed to be spaced apart from each other on the active layer 130, a ruthenium oxide layer 172 disposed between the active layer 130 and the source electrode 180a and the drain electrode 180b, and a high-concentration metal oxide layer 174.

[0098] A thin film transistor according to yet another exemplary embodiment may be different from the thin film transistor according to yet another exemplary embodiment in that the contact layer 170 is provided as a ruthenium oxide layer 172 and a high-concentration metal oxide layer 174 is disposed on the ruthenium oxide layer 172, and therefore, the contents described about the thin film transistor according to yet another exemplary embodiment may still apply.

[0099] That is, according to yet another exemplary embodiment, the thin film transistor may include a gate 150, an active layer spaced apart from the gate 150 in a vertical direction and including at least one of indium (In), gallium (Ga) and zinc (Zn), a source 180a and a drain 180b spaced apart from each other on the active layer 130, a high-concentration metal oxide layer 174 disposed between the active layer 130 and the source 180a and the drain 180b and having an impurity content higher than that of the active layer 130, and a ruthenium oxide layer 172 disposed between the high-concentration metal oxide layer 174 and the source 180a and the drain 180b.

[0100] As described above, the contact layer 170 may contain a metal element and may be provided as a plurality of metal oxide films having different compositions. Here, in yet another fourth exemplary embodiment, the contact layer 170 may be provided in a film of a plurality of ruthenium oxide layers 172 containing ruthenium (Ru) oxide and a high-concentration metal oxide layer 174 containing a metal oxide having a high impurity concentration. Here, the metal oxide may be an oxide of at least one of indium (In), gallium (Ga) and zinc (Zn), and the impurity content of the metal oxide layer 174 disposed on the ruthenium oxide layer 172 may be greater than the impurity content of the active layer 130. That is, when both the active layer 130 and the high-concentration metal oxide layer 174 contain metal oxide doped with impurities, the impurity content of the high-concentration metal oxide layer 174 may be greater than the impurity content of the active layer 130. Both the ruthenium oxide layer 172 and the high-concentration metal oxide layer 174 may be formed by a regional selective atomic layer deposition method. On the other hand, the ruthenium oxide layer 172 and the high-concentration metal oxide layer 174 may also be sequentially formed on a portion of the exposed surface of the active layer 130 by using a masked deposition method.

[0101] As described above, according to exemplary embodiments, a contact layer for preventing oxygen deficiency in an active layer may be provided between the active layer and the source and drain electrodes to prevent the active layer from having conductivity and improve switching characteristics.

[0102] Furthermore, the contact resistance between the active layer and the source and drain electrodes can be effectively reduced, and the reliability and characteristics of the device can be improved.

[0103] According to exemplary embodiments, a contact layer to prevent oxygen deficiency in an active layer may be provided between the active layer and the source and drain electrodes to prevent the active layer from having conductivity and improve switching characteristics.

[0104] Furthermore, the contact resistance between the active layer and the source and drain electrodes can be effectively reduced, and the reliability and characteristics of the device can be improved.

[0105] Although specific words are used to describe and illustrate specific embodiments, this is only for the purpose of clearly explaining the exemplary embodiments, and therefore, it is obvious to a person of ordinary knowledge that the exemplary embodiments and technical terms can be implemented in other specific forms without changing the technical concepts or essential features. Therefore, it should be understood that simple modifications according to the exemplary embodiments of the present invention may belong to the technical spirit of the present invention.

Claims

1. A thin film transistor, comprising: Gate; an active layer including an oxide of a first metal element and arranged to be spaced apart from the gate in a vertical direction; a source electrode and a drain electrode, arranged on the active layer to be spaced apart from each other; as well as The contact layer includes a second metal element and is disposed between the active layer and the source and drain electrodes.

2. The thin film transistor according to claim 1, wherein: The contact layer includes a metal or an alloy containing the second metal element.

3. The thin film transistor according to claim 2, wherein: The second metal element includes ruthenium (Ru).

4. The thin film transistor according to claim 1, wherein: The contact layer includes an oxide of the second metal element.

5. The thin film transistor according to claim 4, wherein: The oxide of the first metal element and the oxide of the second metal element have compositions different from each other.

6. The thin film transistor according to claim 4, wherein: Each of the oxide of the first metal element and the oxide of the second metal element includes zinc oxide doped with a plurality of impurities, and The oxide of the first metal element and the oxide of the second metal element have different impurity contents from each other.

7. The thin film transistor according to claim 6, wherein: The impurity content of the oxide of the second metal element is greater than the impurity content of the oxide of the first metal element.

8. The thin film transistor according to claim 6 or 7, wherein: The impurities include at least one of indium (In), gallium (Ga), tungsten (W), lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), manganese (Mn), technetium (Tc), rhenium (Re), iron (Fe), ruthenium (Ru), osmium (Os), cobalt (Co), rhodium (Rh), iridium (Ir), nickel (Ni), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), boron (B), thallium (Tl), silicon (Si), germanium (Ge), tin (Sn), lead (Pb), phosphorus (P) and arsenic (As).

9. The thin film transistor according to claim 6, wherein: The oxide of the first metal element includes the impurity in an amount of about 20 at % or more and less than about 40 at % relative to the entire oxide of the first metal element, and The oxide of the second metal element includes the impurity in an amount of about 40 at % or more and less than about 60 at % with respect to the entire oxide of the second metal element.

10. The thin film transistor according to claim 6, wherein: The oxygen (O) content of the oxide of the second metal element is smaller than the oxygen (O) content of the oxide of the first metal element.

11. The thin film transistor according to claim 1, wherein: The contact layer has approximately to about Thickness.

12. The thin film transistor according to claim 1, further comprising an insulating layer, the insulating layer being disposed on the active layer and having a contact hole, a portion of a surface of the active layer being exposed through the contact hole, in, The contact layer is disposed on the portion of the surface of the active layer exposed through the contact hole, and The source electrode and the drain electrode contact the contact layer and extend onto the insulating layer.

13. A method for manufacturing a thin film transistor, comprising: preparing a substrate on which a gate and an active layer are formed, the active layer being arranged to be spaced apart from the gate in a vertical direction; as well as A contact layer connecting the active layer with the source electrode and the drain electrode is formed on the active layer.

14. The method for manufacturing a thin film transistor according to claim 13, wherein: Preparing the substrate includes preparing the substrate in which the insulating layer on the active layer has a contact hole, a portion of the surface of the active layer is exposed through the contact hole, and Forming the contact layer includes forming the contact layer on the portion of the surface of the active layer exposed through the contact hole.

15. The method for manufacturing a thin film transistor according to claim 14, wherein: When forming the contact layer, the contact layer is formed on the portion of the surface of the active layer to be approximately to about Thickness.

16. The method for manufacturing a thin film transistor according to claim 13, wherein: The contact layer is formed by repeating an atomic layer deposition process including supplying a source gas including a metal element onto the active layer and supplying a reaction gas including oxygen onto the active layer for several times.

17. The method for manufacturing a thin film transistor according to claim 16, wherein: When the source gas is supplied, a first source gas containing zinc (Zn) and a second source gas containing at least one of indium (In), gallium (Ga), tungsten (W), lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), manganese (Mn), technetium (Tc), rhenium (Re), iron (Fe), ruthenium (Ru), osmium (Os), cobalt (Co), rhodium (Rh), iridium (Ir), nickel (Ni), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), boron (B), thallium (Tl), silicon (Si), germanium (Ge), tin (Sn), lead (Pb), phosphorus (P), and arsenic (As) are simultaneously supplied.

18. The method for manufacturing a thin film transistor according to claim 17, wherein: In supplying the source gas, supply of the source gas is controlled such that a supply amount of the second source gas is greater than a supply amount of the first source gas. 19 . The method for manufacturing a thin film transistor according to claim 13 , further comprising forming a source electrode and a drain electrode on the contact layer.

20. A thin film transistor, comprising: Gate; an active layer including an oxide of a first metal element and arranged to be spaced apart from the gate in a vertical direction; The first insulating layer is disposed on the active layer and has a first contact hole, through which a portion of the surface of the active layer is exposed. The second insulating layer is disposed on the first insulating layer and exposes the first contact hole and a portion of the surface of the first insulating layer extending from the first contact hole. a contact layer including a second metal element and disposed on the portion of the surface of the active layer exposed through the first insulating layer; as well as A source electrode and a drain electrode are disposed on the contact layer to be spaced apart from each other and extend to the portion of the surface of the first insulating layer exposed through the second insulating layer.

21. The thin film transistor according to claim 20, wherein the first insulating layer comprises silicon oxide, and The second insulating layer includes silicon nitride.

22. The thin film transistor according to claim 20, wherein: The first metal element includes at least one of indium (In), gallium (Ga), and zinc (Zn), and The second metal element includes at least one of indium (In), gallium (Ga), zinc (Zn), and ruthenium (Ru).

23. A method for manufacturing a thin film transistor, comprising: preparing a substrate having a gate and an active layer thereon, the active layer being disposed to be spaced apart from the gate in a vertical direction and a portion of a surface of the active layer being exposed through a contact hole formed in a first insulating layer; as well as A second insulating layer including silicon nitride is formed on the first insulating layer.

24. A method for manufacturing a thin film transistor, comprising: preparing a substrate having a gate electrode and an active layer thereon, the active layer being disposed to be spaced apart from the gate electrode in a vertical direction and a portion of a surface of the active layer being exposed through a contact hole formed in each of a stacked first insulating layer and a second insulating layer; as well as A contact layer connecting the active layer with a source electrode and a drain electrode is formed on the portion of the exposed surface of the active layer by an area selective atomic layer deposition method.

25. The method for manufacturing a thin film transistor according to claim 24, wherein: The contact layer includes a metal oxide doped with impurities.

26. The method for manufacturing a thin film transistor according to claim 25, wherein: The impurities include at least one of indium (In), gallium (Ga), tungsten (W), lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), manganese (Mn), technetium (Tc), rhenium (Re), iron (Fe), ruthenium (Ru), osmium (Os), cobalt (Co), rhodium (Rh), iridium (Ir), nickel (Ni), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), boron (B), thallium (Tl), silicon (Si), germanium (Ge), tin (Sn), lead (Pb), phosphorus (P) and arsenic (As). 27 . The method for manufacturing a thin film transistor according to claim 25 , further comprising etching the metal oxide layer doped with the impurities formed on the second insulating layer after forming the contact layer.

28. The method for manufacturing a thin film transistor according to claim 27, wherein: The metal oxide layer doped with the impurities is etched using hydrogen bromide (HBr).

29. A method for manufacturing a thin film transistor, comprising: preparing a substrate having a gate and an active layer thereon, the active layer being disposed to be spaced apart from the gate in a vertical direction and a portion of a surface of the active layer being exposed through a first contact hole formed in a first insulating layer including silicon oxide; forming a second insulating layer on the first insulating layer, wherein a second contact hole exposing the first contact hole is formed in the second insulating layer and the second insulating layer comprises silicon nitride; as well as A contact layer connecting the active layer with a source electrode and a drain electrode is formed on the portion of the exposed surface of the active layer by an area selective atomic layer deposition method.

30. A thin film transistor comprising: Gate; an active layer disposed to be spaced apart from the gate in a vertical direction and comprising at least one of indium (In), gallium (Ga), and zinc (Zn); a source electrode and a drain electrode, arranged on the active layer to be spaced apart from each other; as well as The ruthenium oxide layer is disposed between the active layer and the source electrode and the drain electrode.

31. A thin film transistor comprising: Gate; an active layer disposed to be spaced apart from the gate in a vertical direction and containing at least one of indium (In), gallium (Ga), and zinc (Zn); a source electrode and a drain electrode, arranged on the active layer to be spaced apart from each other; A high-concentration metal oxide layer is disposed between the active layer and the source electrode and the drain electrode, and the impurity content of the high-concentration metal oxide layer is greater than the impurity content of the active layer; as well as The ruthenium oxide layer is disposed between the high-concentration metal oxide layer and the source electrode and the drain electrode.

32. A method for manufacturing a thin film transistor, comprising: preparing a substrate on which a gate electrode and an active layer disposed to be spaced apart from the gate electrode in a vertical direction are formed; as well as A ruthenium oxide layer is formed on the active layer to connect the active layer with the source electrode and the drain electrode.

33. A method for manufacturing a thin film transistor, comprising: preparing a substrate on which a gate and an active layer are formed, the active layer being arranged to be spaced apart from the gate in a vertical direction; forming a high-concentration metal oxide layer on the active layer, wherein the content of multiple impurities in the metal oxide layer is greater than the content of multiple impurities in the active layer; as well as A ruthenium oxide layer is formed on the high-concentration metal oxide layer to connect the active layer with the source electrode and the drain electrode.

34. The method for manufacturing a thin film transistor according to claim 33, wherein: The impurities include at least one of indium (In), gallium (Ga), tungsten (W), lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), manganese (Mn), technetium (Tc), rhenium (Re), iron (Fe), ruthenium (Ru), osmium (Os), cobalt (Co), rhodium (Rh), iridium (Ir), nickel (Ni), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), boron (B), thallium (Tl), silicon (Si), germanium (Ge), tin (Sn), lead (Pb), phosphorus (P) and arsenic (As).

Citation Information

Patent Citations

  • Thin Film Transistor and the same method

    KR1020040013273A