Negative electrode, power storage element, and power storage apparatus
By adding a rubber-based adhesive and carbon nanotubes to the negative active material layer, the bonding state and conductivity of the silicon-based negative active material are improved, and the capacity maintenance rate and high rate caused by the expansion and contraction of the silicon-based negative active material are solved. The problem of reduced discharge performance is achieved, and higher discharge capacity and more stable electrochemical performance are achieved.
Patent Information
- Application Number
- CN202380026346.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-10
- Filing Date
- 2023-03-10
- Publication Date
- 2024-10-29
AI Technical Summary
The silicon-based negative active material expands and contracts greatly during the charge and discharge process, causing damage to the bonding state and reducing the capacity maintenance rate and high-rate discharge performance of the storage element.
Add rubber binder and carbon nanotubes to the negative active material layer. The silicon negative active material content is more than 68%, the rubber binder content is more than 3.0%, and the carbon nanotube content is 0.4×(n2+4 )/(2n+3) mass % or less, these components improve the bonding state and conductivity, and suppress the isolation of the silicon-based negative electrode active material.
The discharge capacity of the electric storage element is increased, and the decrease in capacity maintenance rate and high-rate discharge performance after charge and discharge cycles are suppressed.
Smart Images

Figure BDA0005033665500000061 
Figure BDA0005033665500000301 
Figure BDA0005033665500000341
Abstract
Description
Technical Field
[0001] The present invention relates to a negative electrode, an electricity storage element, and an electricity storage device. Background Art
[0002] Non-aqueous electrolyte secondary batteries represented by lithium ion secondary batteries are mostly used in electronic devices such as personal computers, communication terminals, and automobiles due to their high energy density. Non-aqueous electrolyte secondary batteries are usually composed of a pair of electrodes electrically isolated by a diaphragm and a non-aqueous electrolyte between the electrodes, and are charged and discharged by transferring charge transport ions between the two electrodes. In addition, as storage elements other than non-aqueous electrolyte secondary batteries, capacitors such as lithium ion capacitors and double electric layer capacitors, storage elements using electrolytes other than non-aqueous electrolytes, etc. have also been widely popularized.
[0003] As described in Patent Documents 1 to 3, it is known that there are storage elements using silicon-based negative electrode active materials (e.g., negative electrode active materials containing silicon elements such as silicon alone or silicon oxide) as negative electrode active materials. Silicon-based negative electrode active materials have a larger capacity than carbon-based negative electrode active materials (carbon-based materials) such as graphite, and are therefore expected to be promising negative electrode active materials. Prior art literature Patent Literature
[0004] Patent Document 1: Japanese Patent Application Publication No. 2015-053152 Patent Document 2: Japanese Patent Application Publication No. 2010-212228 Patent Document 3: Japanese Patent Application Publication No. 2004-356078 Summary of the invention Problems to be solved by the invention
[0005] On the other hand, the above-mentioned silicon-based negative electrode active material has large expansion and contraction accompanying charge and discharge. In addition, the greater the content of silicon-based negative electrode active material in the negative electrode active material layer, the greater the impact of the expansion and contraction of the silicon-based negative electrode active material, and the bonding state between the silicon-based negative electrode active materials is easily damaged in the case of repeated charge and discharge. Therefore, sometimes the isolation of the silicon-based negative electrode active material occurs, which reduces the capacity retention rate of the storage element after charge and discharge cycles. In response to this, it is proposed to mix carbon-based materials in the negative electrode active material layer to reduce the content ratio of the silicon-based negative electrode active material. However, when the content ratio of the silicon-based negative electrode active material in the negative electrode active material layer is reduced, the discharge capacity density of the negative electrode will be reduced, so that a high-capacity storage element cannot be made. In addition, it is proposed to use high-strength adhesives such as polyimide and acrylic resin. However, in order to obtain sufficient adhesion, polyimide-based adhesives have practical problems such as heating to a high temperature in an inactive atmosphere in the manufacturing process of the negative electrode. In addition, the effect of acrylic resin on reducing the capacity retention rate of silicon-based negative electrode active materials after charge and discharge cycles is not sufficient. In addition, it has been proposed to use carbon nanotubes as a conductive agent, but when a large amount of carbon nanotubes is used, a tendency is observed to reduce the high rate discharge performance.
[0006] The object of the present invention is to provide a negative electrode, a storage element having such a negative electrode, and a storage device, which can improve the discharge capacity of the storage element and suppress the decrease in capacity retention rate after charge and discharge cycles and the decrease in high-rate discharge performance when using a silicon-based negative electrode active material. Means for solving problems
[0007] The negative electrode of one aspect of the present invention comprises a negative electrode active material layer, wherein the negative electrode active material layer comprises a silicon-based negative electrode active material, a rubber-based binder and carbon nanotubes, wherein the content of the silicon-based negative electrode active material in the negative electrode active material layer is 68% by mass or more, the content of the rubber-based binder in the negative electrode active material layer is 3.0% by mass or more, and the content of the carbon nanotubes in the negative electrode active material layer is 0.4×(n 2 +4) / (2n+3) mass % or less (wherein n is the number of graphene layers forming the carbon nanotube).
[0008] A power storage device according to another aspect of the present invention includes the negative electrode according to one aspect of the present invention.
[0009] A power storage device according to another aspect of the present invention includes two or more power storage elements and includes one or more power storage elements according to the one aspect of the present invention described above. Effects of the Invention
[0010] According to one aspect of the present invention, a negative electrode, a storage element having such a negative electrode, and a storage device can be provided, which can increase the discharge capacity of the storage element and suppress the decrease in capacity retention rate after charge and discharge cycles and the decrease in high-rate discharge performance when using a silicon-based negative electrode active material. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] [ Figure 1 ] Figure 1 This is a perspective view showing an embodiment of an electric storage element. [ Figure 2 ] Figure 2 This is a schematic diagram showing one embodiment of an electric storage device constituted by combining a plurality of electric storage elements. [ Figure 3 ] Figure 3 This is a diagram showing a state where the surface of a silicon-based negative electrode active material is covered with carbon nanotubes. DETAILED DESCRIPTION
[0012] [1] In one aspect of the present invention, a negative electrode comprises a negative electrode active material layer, wherein the negative electrode active material layer comprises a silicon-based negative electrode active material, a rubber-based binder and carbon nanotubes, wherein the content of the silicon-based negative electrode active material in the negative electrode active material layer is 68% by mass or more, the content of the rubber-based binder in the negative electrode active material layer is 3.0% by mass or more, and the content of the carbon nanotubes in the negative electrode active material layer is 0.4×(n 2 +4) / (2n+3) mass % or less (wherein n is the number of graphene layers forming the carbon nanotube).
[0013] The negative electrode described in [1] above can improve the discharge capacity of the storage element and suppress the decrease in capacity retention rate after charge and discharge cycles and the decrease in high-rate discharge performance even if it contains a silicon-based negative electrode active material. The reason for this is not yet clear, but it is presumed to be the following. As described above, in the existing storage element using silicon-based negative electrode active materials, one of the reasons for the low capacity retention rate after charge and discharge cycles is that the silicon-based negative electrode active materials expand and contract greatly with charge and discharge. In addition, the greater the content of silicon-based negative electrode active materials in the negative electrode active material layer, the greater the impact of the expansion and contraction of the silicon-based negative electrode active materials, and the bonding state between the silicon-based negative electrode active materials is easily damaged in the case of repeated charge and discharge. As a result, the silicon-based negative electrode active materials will be isolated, and the capacity retention rate after charge and discharge cycles in the storage element will be significantly reduced. In view of this, in the negative electrode described in [1], the negative electrode active material layer contains a rubber-based binder and carbon nanotubes, the content of the silicon-based negative electrode active material in the negative electrode active material layer is 68% by mass or more, the content of the rubber-based binder in the negative electrode active material layer is 3.0% by mass or more, and the content of the carbon nanotubes in the negative electrode active material layer is 0.4×(n 2 +4) / (2n+3)% by mass or less (where n is the number of graphene layers forming the carbon nanotubes). The rubber-based binder is considered to be an elastomer and is concentrated near the contact points with the silicon-based negative electrode active material, the conductive agent described later, etc., so that the bonding state between the silicon-based negative electrode active materials that expand and contract greatly with charge and discharge can be improved. Here, it is further considered that by using carbon nanotubes as conductive agents, the number of contact points between the silicon-based negative electrode active materials and the conductive agent is increased, and the isolation between the silicon-based negative electrode active materials is suppressed. In addition, in addition to the above-mentioned structure, by setting the content of the silicon-based negative electrode active material to 68% by mass or more, the silicon-based negative electrode active materials are more appropriately arranged with each other, and the contact with the carbon nanotubes as the conductive agent is better maintained. It is speculated that the negative electrode described in [1] above can still improve the discharge capacity of the storage element despite the high content of the silicon-based negative electrode active material, and suppress the reduction of the capacity retention rate after the charge and discharge cycle and the reduction of the high-rate discharge performance. In addition, the negative electrode described in [1] can improve the effect of suppressing the decrease in capacity retention rate and high-rate discharge performance after charge and discharge cycles of the storage element by making the content of the rubber-based binder 3.0% by mass or more. On the other hand, if the negative electrode active material layer contains excessive carbon nanotubes as a conductive agent, the carbon nanotubes cover the silicon-based negative electrode active material excessively, and the high-rate discharge performance is reduced. It is speculated that the negative electrode described in [1] can improve the effect of suppressing the decrease in capacity retention rate and high-rate discharge performance after charge and discharge cycles of the storage element by making the content of the rubber-based binder 3.0% by mass or more. On the other hand, if the negative electrode active material layer contains excessive carbon nanotubes as a conductive agent, the carbon nanotubes cover the silicon-based negative electrode active material excessively, and the high-rate discharge performance is reduced. 2 +4) / (2n+3) mass % or less (where n is the number of graphene layers forming the carbon nanotubes), so that the carbon nanotubes cover the silicon-based negative electrode active material appropriately, and the reduction in high-rate discharge performance is suppressed. For example, when the carbon nanotubes are single-walled carbon nanotubes (the number of graphene layers is 1), it is speculated that by making the content of the carbon nanotubes 0.4×(1 2 +4) / (2×1+3) mass % or less, that is, 0.4 mass % or less, the coating of the silicon-based negative electrode active material with the carbon nanotubes becomes appropriate, and the reduction in high-rate discharge performance is suppressed. Here, the content of carbon nanotubes is 0.4×(n 2 +4) / (2n+3) mass % or less (wherein n is the number of graphene layers forming the above-mentioned carbon nanotube) will be described. Figure 3Indicates the state of the surface of the silicon-based negative electrode active material being coated with carbon nanotubes. Table 1 shows the number of graphene layers forming the carbon nanotubes, the diameter of the carbon nanotubes, the coverage area of the silicon-based negative electrode active material per unit length of the carbon nanotubes, the mass of the carbon nanotubes per unit length, and the carbon nanotube content in the negative electrode active material layer required to form the same silicon-based negative electrode active material coverage area as when the content of the single-walled carbon nanotubes in the negative electrode active material layer is 0.4 mass %. Figure 3 As shown, assuming that the length of the carbon nanotube is constant, the area of the surface of the silicon-based negative electrode active material covered by the carbon nanotube is proportional to the diameter of the carbon nanotube. Assuming that the diameter of a single-walled carbon nanotube (the number of graphene layers is 1) is 1.7nm, and the distance between graphene layers is 0.34nm, the diameter of the carbon nanotube formed by n layers of graphene is 0.34×(2n+3)[nm]. Here, assuming that the coverage area of a single-walled carbon nanotube per unit length is 1.7, the coverage area of a carbon nanotube formed by n layers of graphene per unit length can be estimated to be 0.34×(2n+3). In addition, assuming that the mass of a single-walled carbon nanotube per unit length is 1.7, the mass of the kth (k is a natural number less than n) layer of graphene from the center of a carbon nanotube formed by n layers of graphene per unit length is correlated with the diameter of the kth layer, which can be expressed as 0.34×(2k+3). Therefore, the mass of the carbon nanotube consisting of n-layer graphene per unit length can be expressed as 0.34×(n 2 Therefore, the content of carbon nanotubes composed of n-layer graphene in the negative electrode active material layer required to form the same silicon-based negative electrode active material coating area as when the content of single-walled carbon nanotubes in the negative electrode active material layer is 0.4 mass % can be expressed as 0.4×(n 2 +4n) / (2n+3)mass%.
[0014] [Table 1]
[0015] [2] In the negative electrode described in [1] above, the content of the carbon nanotubes in the negative electrode active material layer may be 0.4 mass % or less. It is speculated that in the negative electrode described in [2] above, by making the content of the carbon nanotubes in the negative electrode active material layer 0.4 mass % or less, the coating of the silicon-based negative electrode active material particles by the carbon nanotubes becomes appropriate, and the reduction in high-rate discharge performance is further suppressed.
[0016] [3] In the negative electrode described in [1] or [2] above, the negative electrode active material layer may further contain a carbon-based material, and the total content of the carbon nanotubes and the carbon-based material in the negative electrode active material layer may be 22% by mass or less. The negative electrode described in [3] above can further improve the effect of suppressing the reduction of the capacity retention rate after charge and discharge cycles of the storage element and the reduction of the high-rate discharge performance by making the total content of the carbon nanotubes and the carbon-based material below the above upper limit. In the prior art, it is disclosed that in order to suppress the influence of expansion and contraction of silicon-based active materials, or to improve the capacity retention rate (charge and discharge cycle characteristics), it is preferred to set the proportion of carbon-based materials such as graphite to above a certain level (Japanese Patent Gazette No. 2006-196338, Japanese Patent Gazette No. 2013-101921, Japanese Patent Gazette No. 2017-188334, International Publication No. WO2012 / 026462). In particular, Japanese Patent Publication No. 2017-188334 states that "the graphite material is preferably 20% by mass or more and 80% by mass or less relative to the total active material mass (100% by mass). When it is less than 20% by mass, the negative electrode is easily separated from the collector due to the volume change of the silicon-based active material." (Paragraph 0022). In contrast, in the negative electrode described in [3] above, it is believed that by making the total content of carbon nanotubes and carbon-based materials in the above-mentioned negative electrode active material layer less than 22% by mass, the silicon-based negative electrode active materials can be more appropriately arranged to better maintain contact with the carbon nanotubes as a conductive agent. It is speculated that despite the low content of carbon-based materials in the negative electrode, the discharge capacity of the storage element can be improved, and the reduction in capacity retention rate after charge and discharge cycles and the reduction in high-rate discharge performance can be suppressed. The above-mentioned "total content of carbon nanotubes and carbon-based materials" refers to the total content of carbon nanotubes and carbon-based materials contained in the negative electrode active material layer as negative electrode active materials, conductive agents, etc., including the coated carbon when the surface of the negative electrode active material is coated with carbon.
[0017] [4] In the negative electrode described in any one of [1] to [3] above, the content of the rubber-based binder in the negative electrode active material layer may be 6.0% by mass or more. The negative electrode described in [4] above can further improve the effect of suppressing the reduction of the capacity retention rate after charge and discharge cycles of the storage element and the reduction of the high-rate discharge performance by making the content of the rubber-based binder be greater than the above lower limit.
[0018] [5] In the negative electrode described in any one of [1] to [4] above, the carbon nanotubes may include single-walled carbon nanotubes. Even when the content of the single-walled carbon nanotubes in the negative electrode active material layer is small, the single-walled carbon nanotubes are densely distributed in the negative electrode active material layer, and can appropriately maintain the contact between the silicon-based negative electrode active material in the entire negative electrode active material layer and the single-walled carbon nanotubes as a conductive agent. Therefore, the negative electrode described in [5] above can further improve the effect of suppressing the reduction of the capacity retention rate after the charge and discharge cycle of the storage element and the reduction of the high-rate discharge performance by making the carbon nanotubes include single-walled carbon nanotubes.
[0019] [6] Another aspect of the present invention is an electric storage device comprising the negative electrode described in any one of [1] to [5]. The electric storage device described in [6] comprises the negative electrode described in any one of [1] to [5], and thus can suppress a decrease in capacity retention rate after charge and discharge cycles and a decrease in high rate discharge performance.
[0020] [7] Another aspect of the present invention is a power storage device having two or more power storage elements and having one or more power storage elements described in [6]. Since the power storage device described in [7] has one or more power storage elements described in [6], it is possible to suppress a decrease in capacity retention rate after charge and discharge cycles and a decrease in high-rate discharge performance.
[0021] The structure of the negative electrode, the structure of the storage element, the structure of the storage device, and the manufacturing method of the storage element according to one embodiment of the present invention are described in detail, as well as other embodiments. In addition, the names of the components (components) used in each embodiment are sometimes different from the names of the components (components) used in the background art.
[0022] <Negative electrode> A negative electrode according to one embodiment of the present invention comprises a negative electrode substrate and a negative electrode active material layer disposed on the negative electrode substrate directly or via an intermediate layer. The negative electrode is used in a storage element such as a secondary battery.
[0023] The negative electrode substrate has electrical conductivity. Whether it has "electrical conductivity" is determined by measuring the volume resistivity in accordance with JIS-H-0505 (1975) with a value of 10 -2 Ω·cm is the threshold value for determination. As the material of the negative electrode substrate, metals such as copper, nickel, stainless steel, nickel-plated steel, or their alloys, carbonaceous materials, etc. can be used. Among them, copper or copper alloys are preferred. As the negative electrode substrate, foil, vapor-deposited film, mesh, porous material, etc. can be cited. From the perspective of cost, foil is preferred. Therefore, as the negative electrode substrate, copper foil or copper alloy foil is preferred. As examples of copper foil, rolled copper foil, electrolytic copper foil, etc. can be cited.
[0024] The average thickness of the negative electrode substrate is preferably 2 μm or more and 35 μm or less, more preferably 3 μm or more and 30 μm or less, further preferably 4 μm or more and 25 μm or less, and particularly preferably 5 μm or more and 20 μm or less. By setting the average thickness of the negative electrode substrate to the above range, the strength of the negative electrode substrate can be improved while increasing the energy density of the storage element.
[0025] The intermediate layer is a layer disposed between the negative electrode substrate and the negative electrode active material layer. The intermediate layer reduces the contact resistance between the negative electrode substrate and the negative electrode active material layer by including a conductive agent such as carbon particles. The composition of the intermediate layer is not particularly limited, and for example, includes a binder and a conductive agent.
[0026] The negative electrode active material layer contains a silicon-based negative electrode active material, a rubber-based binder and carbon nanotubes. The negative electrode active material layer may contain any components such as carbon-based materials other than carbon nanotubes, other conductive agents other than carbon-based materials and carbon nanotubes, other binders other than rubber-based binders, thickeners, fillers, etc. as needed.
[0027] The negative electrode active material layer may contain typical non-metallic elements such as B, N, P, F, Cl, Br, I, typical metal elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, Ba, and transition metal elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Ta, Hf, Nb, and W as components other than silicon-based negative electrode active materials, carbon nanotubes, rubber-based binders, carbon-based materials, other conductive agents, other binders, thickeners, and fillers.
[0028] The negative electrode active material contains a silicon-based negative electrode active material. A silicon-based negative electrode active material refers to an active material containing silicon. Examples of silicon-based negative electrode active materials include silicon alone or compounds containing silicon. Examples of compounds containing silicon include silicon oxide (SiO x: 0 < x < 2, preferably 0.8 ≤ x ≤ 1.2), silicon nitride, silicon carbide, metal silicon compounds, etc. As the metal silicon compound, compounds containing metal elements such as aluminum element, tin element, zinc element, nickel element, copper element, titanium element, vanadium element, magnesium element and silicon element can be cited. In addition, as the silicon-based negative electrode active material, it can also be a composite material such as a SiO / Si / SiO2 composite material containing elemental silicon or a compound containing silicon element. The silicon-based negative electrode active material can also use a material pre-doped with charge transfer ions or metal ions of the energy storage element. That is, for example, the silicon-based negative electrode active material can further contain alkali metal elements such as lithium element and magnesium element, alkaline earth metal elements, etc. The silicon-based negative electrode active material can be used singly or in combination of two or more. Among the silicon-based negative electrode active materials, elemental silicon and silicon oxide are preferred, silicon oxide is more preferred, and silicon oxide pre-doped with charge transfer ions or metal ions of the energy storage element is further preferred.
[0029] The surface of the silicon-based negative electrode active material can be coated with a conductive material such as carbon. By using such a form of the silicon-based negative electrode active material, the electron conductivity of the negative electrode active material layer can be improved. In the case where the silicon-based negative electrode active material is coated with a conductive material, as the mass ratio of the conductive material to the total amount of the silicon-based negative electrode active material and the conductive material coating it, for example, it is preferably 1% by mass or more and 10% by mass or less, more preferably 2% by mass or more and 5% by mass or less.
[0030] The shape of the silicon-based negative electrode active material is not particularly limited, and particle shape is preferred. The average particle size of the silicon-based negative electrode active material is, for example, preferably 1 nm or more and 50 μm or less, more preferably 1 μm or more and 40 μm or less, further preferably 3 μm or more and 30 μm or less, and even more preferably 5 μm or more and 20 μm or less. By setting the average particle size of the silicon-based negative electrode active material to be above the above lower limit, the manufacture or treatment of the silicon-based negative electrode active material becomes easy. By setting the average particle size of the silicon-based negative electrode active material to be below the above upper limit, the silicon-based negative electrode active material can react sufficiently during charge and discharge. Here, the "average particle size" means the value when the volume-based cumulative distribution calculated based on JIS-Z-8819-2 (2001) for the particle size distribution measured by the laser diffraction-scattering method on the dilution obtained by diluting the particles with a solvent is 50% according to JIS-Z-8825 (2013).
[0031] The lower limit of the content of the silicon-based negative electrode active material in the negative electrode active material layer is 68 mass %, preferably 80 mass %, and more preferably 85 mass %. On the other hand, the upper limit of the content of the silicon-based negative electrode active material in the negative electrode active material layer is 96.6 mass %, which may be 96 mass %, 95 mass %, or 93 mass %. By setting the content of the silicon-based negative electrode active material to above the above lower limit, a higher capacity can be achieved, and the effect of suppressing the decrease in the capacity retention rate after the charge and discharge cycle is excellent.
[0032] In the negative electrode active material layer, other negative electrode active materials other than silicon-based negative electrode active materials may be further included. As such other negative electrode active materials, known negative electrode active materials commonly used in lithium secondary batteries, etc. may be cited, for example, carbon-based materials, Sn or Sn oxides, titanium-containing oxides, polyphosphate compounds, etc. may be cited. Among these materials, preferably a carbon-based material is contained. As carbon-based materials, graphite, non-graphite carbon, etc. may be cited. One of these materials may be used alone, or two or more may be mixed and used.
[0033] “Graphite” refers to the average lattice spacing (d) of the (002) plane determined by X-ray diffraction before charge or discharge or in the discharged state. 002 ) is a carbon-based material having a diameter of 0.33 nm or more and less than 0.34 nm. Examples of graphite include natural graphite and artificial graphite. From the perspective of obtaining a material with stable physical properties, artificial graphite is preferred.
[0034] “Non-graphite carbon” refers to the average lattice spacing (d ) of the (002) plane determined by X-ray diffraction before charge / discharge or in a discharged state. 002 ) is a carbon-based material having a diameter of 0.34 nm or more and 0.42 nm or less. Examples of non-graphite carbon include difficult-graphitizable carbon and easily-graphitizable carbon. Examples of non-graphite carbon include materials derived from resins, petroleum asphalt or materials derived from petroleum asphalt, petroleum coke or materials derived from petroleum coke, materials derived from plants, materials derived from alcohols, and the like.
[0035] Here, the "discharge state" refers to a state in which lithium ions that can be stored and released during charge and discharge are fully released from the carbon-based material as the negative electrode active material. For example, in a half-cell in which a negative electrode containing a carbon-based material as a negative electrode active material is used as a working electrode and metal Li is used as a counter electrode, the open circuit voltage is 0.7 V or more.
[0036] "Difficult to graphitize carbon" refers to the above-mentioned 002 A carbon-based material having a diameter of 0.36 nm or more and 0.42 nm or less.
[0037] "Easily graphitizable carbon" refers to the above-mentioned 002A carbon-based material having a diameter of 0.34 nm or more and less than 0.36 nm.
[0038] The above-mentioned other negative electrode active materials are usually particles (powders). When the above-mentioned other negative electrode active materials are carbon-based materials, titanium-containing oxides or polyphosphate compounds, the average particle size thereof may be greater than 1 μm and less than 100 μm. When the above-mentioned other negative electrode active materials are Sn or Sn oxides, etc., the average particle size thereof may be greater than 1 nm and less than 1 μm. By making the average particle size of the above-mentioned other negative electrode active materials greater than the above-mentioned lower limit, the manufacture or handling of the above-mentioned negative electrode active materials becomes easy. By setting the average particle size of the above-mentioned other negative electrode active materials to less than the above-mentioned upper limit, the electronic conductivity of the negative electrode active material layer is improved. In order to obtain a powder with a predetermined particle size, a pulverizer, a classifier, etc. are used. As a pulverization method, for example, a method using a mortar, a ball mill, a sand mill, a vibrating ball mill, a planetary ball mill, a jet mill, a reverse jet mill, a rotating airflow jet mill, or a sieve can be cited. When pulverizing, wet pulverization in which an organic solvent such as water or hexane coexists can also be used. As a classification method, a sieve, a wind classifier, etc. can be used together with a dry method or a wet method as needed.
[0039] The content of all negative electrode active materials in the negative electrode active material layer is 68% by mass or more and 96.6% by mass or less, preferably 68% by mass or more and 96% by mass or less, more preferably 80% by mass or more and 95% by mass or less, more preferably 85% by mass or more and 93% by mass or less. By setting the content of the negative electrode active material to the above range, it is possible to achieve a balance between the high energy density of the negative electrode active material layer and the effect of improving the reduction of the capacity retention rate after the charge and discharge cycle. In addition, as the upper limit of the content of the silicon-based negative electrode active material in the negative electrode active material layer relative to the total negative electrode active material, there is no particular limitation, for example, it can be 100% by mass.
[0040] The negative electrode active material layer contains carbon nanotubes (CNT). Carbon nanotubes are graphene-based carbon and are components that function as a conductive agent in the negative electrode active material layer. It is believed that by containing carbon nanotubes in the negative electrode active material layer, the number of contact points between the silicon-based negative electrode active material and the conductive agent in the negative electrode is increased, and the isolation between the silicon-based negative electrode active materials is suppressed. As carbon nanotubes, for example, single-walled carbon nanotubes (SWCNTs) formed by one layer of graphene, multi-walled carbon nanotubes (MWCNTs) formed by two or more layers (for example, 2 to 20 layers, typically 2 to 60 layers) of graphene, etc. can be cited. Among them, even when the content of SWCNT in the negative electrode active material layer is a small amount, it is densely distributed in the negative electrode active material layer, and the contact between the silicon-based negative electrode active material of the entire negative electrode active material layer and the single-walled carbon nanotubes as a conductive agent can be appropriately maintained, so it is particularly preferred. Therefore, from the viewpoint of being able to further improve the effect of suppressing the decrease in capacity retention rate and high-rate discharge performance after charge and discharge cycles of the storage element, it is preferred that the above-mentioned carbon nanotubes include single-walled carbon nanotubes, and it is more preferred that the above-mentioned carbon nanotubes consist only of single-walled carbon nanotubes. The structure of graphene-based carbon is not particularly limited, and can be any type of chiral (spiral), zigzag, and armchair. In addition, catalyst metal elements (for example, iron, cobalt, and platinum group elements (ruthenium, rhodium, palladium, osmium, iridium, platinum)) used in the synthesis of carbon nanotubes may also be included. The presence of carbon nanotubes in the negative electrode active material layer can be confirmed by observation using an electron microscope. In addition, the presence of single-walled carbon nanotubes in the negative electrode active material layer can be confirmed by observation using a transmission electron microscope (TEM) and observation of the peak corresponding to RBM (radial breathing mode) in Raman spectroscopy. In addition, the number of layers of carbon nanotubes can be confirmed by observation using a transmission electron microscope (TEM).
[0041] The lower limit of the content of carbon nanotubes in the negative electrode active material layer is preferably 0.025×(n 2 +4) / (2n+3) mass % (where n is the number of graphene layers forming the carbon nanotubes), and more preferably 0.05×(n 2 +4) / (2n+3) mass%, and more preferably 0.10×(n 2 +4) / (2n+3) mass%. By making the content of carbon nanotubes above the above lower limit, the discharge capacity of the storage element, the capacity retention rate after charge and discharge cycles, and the effect of suppressing the reduction of high-rate discharge performance can be improved. On the other hand, the upper limit of the content of carbon nanotubes in the negative electrode active material layer is 0.4×(n 2 +4) / (2n+3) mass%, preferably 0.3×(n 2+4) / (2n+3) mass %. By setting the carbon nanotube content to be less than the upper limit, the cost can be reduced, and the content of the negative electrode active material in the negative electrode active material layer can be increased to achieve a high capacity, thereby suppressing a decrease in high rate discharge performance.
[0042] The content of single-walled carbon nanotubes in the negative electrode active material layer is preferably 0.025% by mass or more, more preferably 0.05% by mass or more, and further preferably 0.10% by mass or more. By setting the content of single-walled carbon nanotubes to above the above lower limit, the discharge capacity of the storage element, the capacity retention rate after charge and discharge cycles, and the effect of suppressing the reduction of high-rate discharge performance can be improved. On the other hand, the content of single-walled carbon nanotubes in the negative electrode active material layer is 0.4% by mass or less, preferably 0.3% by mass or less, and more preferably 0.2% by mass or less. By setting the content of single-walled carbon nanotubes to below the above upper limit, the cost can be reduced, and the content of the negative electrode active material in the negative electrode active material layer is increased to become a high capacity, which can suppress the reduction of high-rate discharge performance.
[0043] The average diameter of the carbon nanotubes is not particularly limited, but is preferably 100 nm or less, more preferably 50 nm or less, further preferably 20 nm or less, and further preferably 10 nm or less from the viewpoint of appropriately forming a conductive path throughout the negative electrode active material layer. The average length of the carbon nanotubes is preferably 1 μm to 500 μm, more preferably 1 μm to 100 μm, and even more preferably 1 μm to 20 μm, from the viewpoint of easy handling and better conductivity.
[0044] It should be noted that the above average diameter and average length refer to the average values of any 10 carbon nanotubes observed with an electron microscope.
[0045] The negative electrode active material layer contains a rubber-based binder. It is believed that if the negative electrode active material layer contains a rubber-based binder, the rubber-based binder is an elastomer and is concentrated near the contact points with the silicon-based negative electrode active material, the conductive agent, etc., so that the bonding state between the silicon-based negative electrode active materials with large expansion and contraction accompanying charge and discharge can be good. As the rubber-based binder in the negative electrode active material layer, styrene butadiene rubber (SBR), ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, fluororubber, gum arabic, etc. can be cited. Among them, from the viewpoint of adhesion, SBR is preferred.
[0046] Regarding the above-mentioned SBR, one or more SBRs can be used as a binder. SBR is a copolymer of styrene and butadiene. Monomers other than styrene and butadiene can also be copolymerized in SBR. For example, carboxyl-modified SBR, acrylic acid-modified SBR (including fluorine-containing SBR), methyl methacrylate-modified SBR, etc. can be used. As the monomer composition of SBR, the mixing ratio of styrene to butadiene (styrene: butadiene) is preferably about 1:2 to 2:1. In addition, the total amount of styrene and butadiene preferably accounts for more than 50% by mass (typically more than 75% by mass, for example, more than 90% by mass) of the total amount of monomers. In the preparation of the negative electrode, SBR can preferably be used in the form of an aqueous emulsion (latex) dispersed in an aqueous solvent (typically water). As the SBR of this mode, an SBR in which a carboxyl group is introduced into the polymer can be preferably used. Alternatively, SBR containing substantially no copolymerized monomers other than polystyrene and butadiene (the content of monomers other than styrene and butadiene is 5% by mass or less, and further 1% by mass or less, based on the total amount of monomers) may be used.
[0047] When the rubber-based binder has a functional group that reacts with lithium or the like, the functional group may be inactivated in advance by methylation or the like.
[0048] The lower limit of the content of the rubber-based binder in the negative electrode active material layer is 3.0 mass %, preferably 5.0 mass %, more preferably 6.0 mass %, and further preferably 8.0 mass %. By making the content of the rubber-based binder above the above lower limit, the effect of suppressing the reduction of the capacity retention rate after the charge and discharge cycle of the storage element and the reduction of the high rate discharge performance can be further improved. On the other hand, as the upper limit of the content of the rubber-based binder, it is preferably 15.0 mass %, more preferably 10.0 mass %, and further preferably 9.0 mass %. By making the content of the rubber-based binder below the above upper limit, the content of the negative electrode active material in the negative electrode active material layer can be increased to become a high capacity.
[0049] The negative electrode active material layer may contain other binders other than the rubber-based binder. Examples of other binders include polyacrylates, polymethacrylates, and the like. When the negative electrode active material layer contains other binders other than the rubber-based binder, it is preferred that the rubber-based binder be contained as the main component of the binder. Here, the "main component" refers to the component with the largest content, which refers to the component that exceeds 50% by mass relative to the total mass of the binder.
[0050] The negative electrode active material layer may contain other conductive agents other than carbon nanotubes. Examples of other conductive agents include carbon-based materials other than carbon nanotubes, metals, conductive ceramics, and the like. Examples of carbon-based materials include non-graphite carbon, graphene-based carbon, and the like. Examples of non-graphite carbon include carbon nanofibers, pitch-based carbon fibers, and carbon black. Examples of carbon black include furnace black, acetylene black, and Ketjen black. Examples of graphene-based carbon include graphene and fullerene. Examples of the shape of other conductive agents include powdered and fibrous forms. Examples of other conductive agents include one of these materials, or a mixture of two or more thereof. In addition, these materials may be composited and used.
[0051] Examples of the thickener include polysaccharide polymers such as carboxymethyl cellulose (CMC) and methyl cellulose. When the thickener has a functional group that reacts with lithium or the like, the functional group may be inactivated in advance by methylation or the like. The content of the thickener in the negative electrode active material layer is preferably 0.3% by mass or more and 4% by mass or less, and more preferably 0.5% by mass or more and 2% by mass or less.
[0052] The filler is not particularly limited. As the filler, there can be mentioned polyolefins such as polypropylene and polyethylene, inorganic oxides such as silicon dioxide, aluminum oxide, titanium dioxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicate, hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide, carbonates such as calcium carbonate, insoluble ionic crystals such as calcium fluoride, barium fluoride, and barium sulfate, nitrides such as aluminum nitride and silicon nitride, talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, mica, and other materials from mineral resources or their artificial products.
[0053] In the case where the negative electrode active material layer further contains a carbon-based material, the upper limit of the total content of the carbon nanotubes and the carbon-based material in the negative electrode active material layer is preferably 22% by mass, and more preferably 10% by mass. It is believed that by setting the total content of the carbon nanotubes and the carbon-based material in the negative electrode active material layer to less than 22% by mass, the silicon-based negative electrode active materials can be more appropriately arranged to better maintain contact with the carbon nanotubes as a conductive agent. It is inferred that the negative electrode can improve the discharge capacity of the storage element despite the low content of the carbon-based material, and suppress the reduction of the capacity retention rate after the charge and discharge cycle and the reduction of the high-rate discharge performance.
[0054] The production of the negative electrode can be carried out, for example, by applying the negative electrode mixture paste directly or through an intermediate layer on the negative electrode substrate and drying it. After drying, it can be pressed as needed. The negative electrode mixture paste contains silicon-based negative electrode active materials, rubber-based binders, carbon nanotubes, and other negative electrode active materials as arbitrary components, other conductive agents, other binders, thickeners, fillers, and other components that constitute the negative electrode active material layer. The negative electrode mixture paste usually also contains a dispersion medium.
[0055] <Electrical storage element> The storage element of one embodiment of the present invention comprises: an electrode body having a positive electrode, a negative electrode and a separator; a non-aqueous electrolyte; and a container for accommodating the electrode body and the non-aqueous electrolyte. The electrode body is usually a stacked type in which a plurality of positive electrodes and a plurality of negative electrodes are stacked with a separator therebetween, or a wound type in which a positive electrode and a negative electrode are wound with a separator therebetween. The non-aqueous electrolyte exists in a state contained in the positive electrode, the negative electrode and the separator. As an example of a storage element, a non-aqueous electrolyte secondary battery (hereinafter also referred to as a "secondary battery") is described.
[0056] (positive electrode) The positive electrode comprises a positive electrode substrate and a positive electrode active material layer disposed on the positive electrode substrate directly or via an intermediate layer. The structure of the intermediate layer is not particularly limited, and can be selected from the structures exemplified for the negative electrode described above.
[0057] The positive electrode substrate has conductivity. As the material of the positive electrode substrate, metals such as aluminum, titanium, tantalum, stainless steel, or their alloys can be used. Among them, from the viewpoints of potential resistance, high conductivity and cost, aluminum or aluminum alloys are preferred. As the positive electrode substrate, foil, vapor-deposited film, net, porous material, etc. can be cited, and from the viewpoint of cost, foil is preferred. Therefore, as the positive electrode substrate, aluminum foil or aluminum alloy foil is preferred. As aluminum or aluminum alloy, A1085, A3003, A1N30, etc. specified in JIS-H-4000 (2014) or JIS-H-4160 (2006) can be exemplified.
[0058] The average thickness of the positive electrode substrate is preferably 3 μm or more and 50 μm or less, more preferably 5 μm or more and 40 μm or less, further preferably 8 μm or more and 30 μm or less, and particularly preferably 10 μm or more and 25 μm or less. By setting the average thickness of the positive electrode substrate to the above range, the energy density of the secondary battery can be increased while improving the strength of the positive electrode substrate.
[0059] The positive electrode active material layer contains a positive electrode active material and optionally contains a conductive agent, a binder, a thickener, a filler, and other optional components.
[0060] As the positive electrode active material, it can be appropriately selected from known positive electrode active materials. As the positive electrode active material for lithium ion secondary batteries, materials that can absorb and release lithium ions are generally used. As the positive electrode active material, for example, lithium transition metal composite oxides having an α-NaFeO2 type crystal structure, lithium transition metal composite oxides having a spinel type crystal structure, polyanion compounds, chalcogen compounds, sulfur, etc. can be cited. As the lithium transition metal composite oxide having an α-NaFeO2 type crystal structure, for example, Li[Li x Ni (1-x) ]O2(0≤x<0.5), Li[Li x Ni γ Co (1-x-γ) ]O2(0≤x<0.5, 0<γ<1), Li[Li x Co (1-x) ]O2(0≤x<0.5), Li[Li x Ni γ Mn (1-x-γ) ]O2(0≤x<0.5, 0<γ<1), Li[Li x Ni γ Mn β Co (1-x-γ-β) ]O2(0≤x<0.5, 0<γ, 0<β, 0.5<γ+β<1), Li[Li x Ni γ Co β Al (1-x-γ-β) ]O2 (0≤x<0.5, 0<γ, 0<β, 0.5<γ+β<1), etc. Examples of lithium transition metal composite oxides having a spinel crystal structure include Li x Mn2O4、Li x Ni γ Mn (2-γ) O4, etc. As polyanion compounds, LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4, Li3V2(PO4)3, Li2MnSiO4, Li2CoPO4F, etc. can be mentioned. As chalcogen compounds, titanium disulfide, molybdenum disulfide, molybdenum dioxide, etc. can be mentioned. Atoms or part of polyanions in these materials can be replaced by atoms or anions composed of other elements. The surfaces of these materials can also be coated with other materials. As positive electrode active materials, one of these materials can be used alone, or two or more can be mixed and used.
[0061] The positive electrode active material is usually a particle (powder). The average particle size of the positive electrode active material is preferably set to be greater than 0.1 μm and less than 20 μm, for example. In addition, the lower limit of the average particle size of the positive electrode active material is preferably greater than 1 μm, more preferably greater than 4 μm, and sometimes further preferably greater than 8 μm. By making the average particle size of the positive electrode active material greater than the above lower limit, the manufacture or handling of the positive electrode active material becomes easy. By making the average particle size of the positive electrode active material less than the above upper limit, the positive electrode active material fully reacts during charging and discharging. It should be noted that when a composite of the positive electrode active material and other materials is used, the average particle size of the composite is used as the average particle size of the positive electrode active material.
[0062] In order to obtain a powder with a predetermined particle size, a pulverizer, a classifier, etc. can be used. As a pulverization method, for example, a method using a mortar, a ball mill, a sand mill, a vibrating ball mill, a planetary ball mill, a jet mill, a reverse jet mill, a rotating airflow jet mill, or a sieve can be cited. When pulverizing, wet pulverization in which an organic solvent such as water or hexane coexists can also be used. As a classification method, a sieve, a wind classifier, etc. can be used together with a dry method or a wet method as needed.
[0063] As the lower limit of the content of the positive electrode active material in the positive electrode active material layer, it is preferably 50% by mass or more, more preferably 70% by mass or more, and further preferably 80% by mass or more. As the upper limit of the content of the positive electrode active material in the positive electrode active material layer, it is preferably 99.5% by mass, more preferably 99% by mass. By setting the content of the positive electrode active material to the above range, it is possible to take into account the high capacity and manufacturability of the positive electrode.
[0064] The conductive agent is not particularly limited as long as it is a material with conductivity. As such a conductive agent, for example, carbonaceous materials, metals, conductive ceramics, etc. can be cited. As carbonaceous materials, graphite, non-graphite carbon, graphene-based carbon, etc. can be cited. As non-graphite carbon, carbon nanofibers, pitch-based carbon fibers, carbon black, etc. can be cited. As carbon black, furnace black, acetylene black, Ketjen black, etc. can be cited. As graphene-based carbon, graphene, CNT, fullerene, etc. can be cited. As the shape of the conductive agent, powder, fiber, etc. can be cited. As a conductive agent, one of these materials can be used alone, or two or more can be mixed and used. In addition, these materials can also be used in a composite. For example, a material that composites carbon black and CNT can also be used. Among them, from the viewpoint of electronic conductivity and coating properties, carbon black or CNT is preferred, and carbon black and CNT are more preferably used in combination, and carbon black and SWCNT are further preferably used in combination.
[0065] The content of the conductive agent in the positive electrode active material layer is preferably 0.1 mass % to 10 mass %, more preferably 0.2 mass % to 5 mass %. By setting the content of the conductive agent to the above range, the energy density of the secondary battery can be increased while ensuring the conductivity of the positive electrode.
[0066] As adhesives, for example, there can be mentioned thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyacrylic acid, polyimide, etc.; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, etc.; polysaccharide polymers, etc.
[0067] The content of the binder in the positive electrode active material layer is preferably 0.4 mass % or more and 10 mass % or less, more preferably 0.8 mass % or more and 5 mass % or less. By setting the content of the binder to the above range, the positive electrode active material can be stably maintained. In addition, when SWCNT is used as a conductive agent, the content of the binder can be further reduced, and its upper limit can be 2 mass % or less.
[0068] The thickener and the filler can be selected from the materials exemplified in the above-mentioned negative electrode.
[0069] The positive electrode active material layer may contain typical non-metallic elements such as B, N, P, F, Cl, Br, I, typical metal elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, Ba, and transition metal elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, and W as components other than the positive electrode active material, conductive agent, binder, thickener, and filler.
[0070] (negative electrode) The negative electrode of the storage element is the negative electrode of one embodiment of the present invention. In the storage element having the negative electrode, in order to further improve the energy density of the storage element, the discharge capacity per unit area can be increased by increasing the mass per unit area of the positive electrode active material layer and the negative electrode active material layer. From the viewpoint of further improving the energy density of the storage element, the discharge capacity per unit area of the positive electrode is preferably 3.5 mAh / cm 2 More preferably 4.0 mAh / cm 2 Above, more preferably 4.5 mAh / cm 2Here, the area of the positive electrode refers to the area of the positive electrode active material layer arranged opposite to the negative electrode active material layer. When the positive electrode active material layer is arranged on both sides of the positive electrode substrate, the area XA of the positive electrode active material layer arranged opposite to the negative electrode active material layer on one side and the area XB of the positive electrode active material layer arranged opposite to the negative electrode active material layer on the other side (XA+XB) are taken as the area of the positive electrode.
[0071] (Diaphragm) The separator can be appropriately selected from known separators. As the separator, for example, a separator consisting only of a substrate layer, a separator having a heat-resistant layer containing heat-resistant particles and a binder formed on one or both sides of the substrate layer, etc. can be used. As the shape of the substrate layer of the separator, for example, woven fabrics, non-woven fabrics, porous resin films, etc. can be cited. Among these shapes, porous resin films are preferred from the viewpoint of strength, and non-woven fabrics are preferred from the viewpoint of liquid retention of non-aqueous electrolytes. As the material of the substrate layer of the separator, from the viewpoint of shutdown function, polyolefins such as polyethylene and polypropylene are preferred, and from the viewpoint of resistance to oxidative decomposition, for example, polyimides, aromatic polyamides, etc. are preferred. As the substrate layer of the separator, a material composited with these resins can also be used.
[0072] The heat-resistant particles contained in the heat-resistant layer preferably have a mass reduction of 5% or less when the temperature is raised from room temperature to 500°C in an air atmosphere of 1 atmosphere, and more preferably have a mass reduction of 5% or less when the temperature is raised from room temperature to 800°C. As materials whose mass reduction is less than the prescribed value, inorganic compounds can be cited. As inorganic compounds, for example, oxides such as iron oxide, silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminum silicate; nitrides such as aluminum nitride and silicon nitride; carbonates such as calcium carbonate; sulfates such as barium sulfate; insoluble ionic crystals such as calcium fluoride, barium fluoride, and barium titanate; covalently bonded crystals such as silicon and diamond; talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, mica, and other mineral resources or their artificial products. As inorganic compounds, monomers or composites of these substances can be used alone, or two or more can be mixed and used. Among these inorganic compounds, silicon oxide, aluminum oxide, or aluminosilicate is preferred from the viewpoint of safety of the electric storage element.
[0073] The porosity of the separator is preferably 80% by volume or less from the viewpoint of strength, and is preferably 20% by volume or more from the viewpoint of discharge performance. Here, the “porosity” is a value based on volume, and refers to a value measured by a mercury porosimeter.
[0074] As a separator, a polymer gel consisting of a polymer and a non-aqueous electrolyte can be used. As a polymer, polyacrylonitrile, polyethylene oxide, polypropylene oxide, polymethyl methacrylate, polyvinyl acetate, polyvinyl pyrrolidone and polyvinylidene fluoride can be cited. If a polymer gel is used, it has the effect of suppressing leakage. As a separator, a porous resin film or a nonwoven fabric as described above can be used together with a polymer gel.
[0075] (Non-aqueous electrolyte) The non-aqueous electrolyte can be appropriately selected from known non-aqueous electrolytes. A non-aqueous electrolyte solution can be used. The non-aqueous electrolyte solution contains a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent.
[0076] As nonaqueous solvent, it can be suitably selected from known nonaqueous solvents. As nonaqueous solvent, cyclic carbonate, linear carbonate, carboxylate, phosphoric acid ester, sulfonic acid ester, ether, amides, nitrile etc. can be enumerated. As nonaqueous solvent, it can be used that the part of hydrogen atom contained in these compounds is replaced by halogen.
[0077] Examples of the cyclic carbonate include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), vinyl ethylene carbonate (VEC), chloroethylene carbonate, fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), styrene carbonate, 1-phenylvinylene carbonate, 1,2-diphenylvinylene carbonate, etc. Among them, FEC is preferred.
[0078] Examples of the linear carbonate include diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diphenyl carbonate, 2-fluoroethyl methyl carbonate, 2,2-difluoroethyl methyl carbonate, 2,2,2-trifluoroethyl methyl carbonate, bis(trifluoroethyl) carbonate, etc. Among them, 2,2,2-trifluoroethyl methyl carbonate (TFEMC) or ethyl methyl carbonate (EMC) is preferred.
[0079] As nonaqueous solvent, preferably use cyclic carbonate or linear carbonate, more preferably use cyclic carbonate and linear carbonate.By using cyclic carbonate, can promote the dissociation of electrolyte salt and improve the ionic conductivity of nonaqueous electrolyte.By using linear carbonate, can the viscosity of nonaqueous electrolyte be suppressed to be lower.When using cyclic carbonate and linear carbonate, as the volume ratio (cyclic carbonate: linear carbonate) of cyclic carbonate and linear carbonate, for example, preferably be set to the scope of 5:95 to 50:50.
[0080] The electrolyte salt may be appropriately selected from known electrolyte salts. Examples of the electrolyte salt include lithium salts, sodium salts, potassium salts, magnesium salts, and onium salts. Among them, lithium salts are preferred.
[0081] As lithium salts, inorganic lithium salts such as LiPF6, LiPO2F2, LiBF4, LiClO4, LiN(SO2F)2, lithium oxalate salts such as lithium bis(oxalate)borate (LiBOB), lithium difluorooxalate borate (LiFOB), lithium bis(oxalate)difluorophosphate (LiFOP), lithium salts such as LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), LiC(SO2CF3)3, LiC(SO2C2F5)3, etc. having halogenated hydrocarbon groups can be cited. Among them, inorganic lithium salts are preferred, and LiPF6 is more preferred. One or more electrolyte salts can be used.
[0082] The content of the electrolyte salt in the non-aqueous electrolyte is preferably 0.1 mol / dm 3 Above and 2.5 mol / dm 3 Below, more preferably 0.4 mol / dm 3 Above and 2.0 mol / dm 3 Below, more preferably 0.7 mol / dm 3 Above 1.7 mol / dm 3 By setting the content of the electrolyte salt to the above range, the ion conductivity of the non-aqueous electrolyte can be improved.
[0083] The non-aqueous electrolyte solution may contain additives in addition to the non-aqueous solvent and the electrolyte salt. Examples of the additive include oxalates such as lithium bis(oxalato)borate (LiBOB), lithium difluorooxalatoborate (LiFOB), and lithium bis(oxalato)difluorophosphate (LiFOP); imide salts such as lithium bis(fluorosulfonyl)imide (LiFSI); aromatic compounds such as biphenyl, alkylbiphenyl, terphenyl, partial hydride of terphenyl, cyclohexylbenzene, tert-butylbenzene, tert-amylbenzene, diphenyl ether, and dibenzofuran; partial halides of the above aromatic compounds such as 2-fluorobiphenyl, o-cyclohexylfluorobenzene, and p-cyclohexylfluorobenzene; halogenated anisole compounds such as 2,4-difluoroanisole, 2,5-difluoroanisole, 2,6-difluoroanisole, and 3,5-difluoroanisole; vinylene carbonate, methyl vinylene carbonate, ethyl vinylene carbonate, succinic anhydride, glutaric anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, and itaconic acid. anhydride, cyclohexanedicarboxylic anhydride; vinyl sulfite, propylene sulfite, dimethyl sulfite, methyl methanesulfonate, busulfan, methyl toluenesulfonate, dimethyl sulfate, vinyl sulfate, sulfolane, dimethyl sulfone, diethyl sulfone, dimethyl sulfoxide, diethyl sulfoxide, tetramethylene sulfoxide, diphenyl sulfide, 4,4'-bis(2,2-dioxo-1,3,2-dioxathiolane), 4-methylsulfonyloxymethyl- 2,2-dioxo-1,3,2-dioxathiolane, thioanisole, diphenyl disulfide, dipyridine disulfide, 1,3-propylene sultone, 1,3-propane sultone, 1,4-butane sultone, 1,4-butene sultone, perfluorooctane, tris(trimethylsilyl)borate, tris(trimethylsilyl)phosphate, tetrakis(trimethylsilyl)titanate, monofluorolithium phosphate, difluorolithium phosphate, etc. These additives may be used alone or in combination of two or more.
[0084] The content of the additive contained in the nonaqueous electrolyte is preferably 0.01% by mass or more and 10% by mass or less relative to the overall mass of the nonaqueous electrolyte, more preferably 0.1% by mass or more and 7% by mass or less, and further preferably 0.2% by mass or more and 5% by mass or less. By setting the content of the additive to the above range, it is possible to improve the capacity maintenance performance or cycle performance after high temperature storage, or further improve safety.
[0085] A solid electrolyte may be used as the non-aqueous electrolyte, or a non-aqueous electrolyte solution and a solid electrolyte may be used in combination.
[0086] As a solid electrolyte, it can be selected from any material that has ion conductivity and is solid at room temperature (e.g., 15° C. to 25° C.), such as lithium, sodium, and calcium. Examples of the solid electrolyte include sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, polymer solid electrolytes, and gel polymer electrolytes.
[0087] In the case of lithium ion secondary batteries, examples of sulfide solid electrolytes include Li2S-P2S5, LiI-Li2S-P2S5, Li 10 Ge-P2S 12 wait.
[0088] The shape of the electric storage element of the present embodiment is not particularly limited, and examples thereof include cylindrical batteries, pouch batteries, square batteries, flat batteries, coin batteries, and button batteries. Figure 1 A non-aqueous electrolyte storage element 1 is shown as an example of a square battery. It should be noted that the figure is a perspective view of the inside of the container. An electrode body 2 having a positive electrode and a negative electrode wound with a separator sandwiched therebetween is housed in a square container 3. The positive electrode is electrically connected to a positive terminal 4 via a positive electrode lead 41. The negative electrode is electrically connected to a negative terminal 5 via a negative electrode lead 51.
[0089] <Configuration of Power Storage Device> The storage element of this embodiment can be installed in the form of a storage unit (battery module) composed of a plurality of storage elements, such as an electric vehicle (EV), a hybrid electric vehicle (HEV), a plug-in hybrid electric vehicle (PHEV) and other automotive power supplies, personal computers, communication terminals and other electronic equipment power supplies, or power storage power supplies, etc. In this case, it is sufficient to apply the technology of the present invention to at least one storage element included in the storage unit. An electric storage device according to an embodiment of the present invention includes two or more electric storage elements and includes one or more electric storage elements according to the above-mentioned embodiment of the present invention (hereinafter referred to as the "second embodiment"). As long as the technology according to the one embodiment of the present invention is applied to at least one electric storage element included in the electric storage device according to the second embodiment, the electric storage device may include one electric storage element according to the above-mentioned embodiment of the present invention and one or more electric storage elements not according to the above-mentioned embodiment of the present invention, or may include two or more electric storage elements according to the above-mentioned embodiment of the present invention. Figure 2 An example of an electric storage device 30 is shown in which an electric storage unit 20 formed by combining two or more electrically connected electric storage elements 1 is further combined. The electric storage device 30 of the second embodiment may also include a bus bar (not shown) that electrically connects the two or more electric storage elements 1, a bus bar (not shown) that electrically connects the two or more electric storage units 20, etc. The electric storage unit 20 or the electric storage device 30 may also include a state monitoring device (not shown) that monitors the state of one or more electric storage elements 1.
[0090] <Method for Manufacturing Electric Storage Element> The manufacturing method of the storage element of this embodiment can be appropriately selected from known methods. The manufacturing method includes, for example, preparing an electrode body; preparing a non-aqueous electrolyte; and storing the electrode body and the non-aqueous electrolyte in a container. Preparing the electrode body includes: preparing a positive electrode and a negative electrode; and forming the electrode body by stacking or winding the positive electrode and the negative electrode through a separator. As the preparation of the above-mentioned negative electrode, the negative electrode of one embodiment of the present invention is prepared.
[0091] The non-aqueous electrolyte may be stored in the container by appropriately selecting from known methods. For example, when a non-aqueous electrolyte solution is used as the non-aqueous electrolyte, the non-aqueous electrolyte solution may be injected from an injection port formed in the container and then the injection port may be sealed.
[0092] <Other Implementation Methods> In addition, the storage element of the present invention is not limited to the above-mentioned embodiment, and various changes may be made within the scope of the main purpose of the present invention. For example, the structure of another embodiment may be added to the structure of a certain embodiment, and a part of the structure of a certain embodiment may be replaced with the structure of another embodiment or a known technology. In addition, a part of the structure of a certain embodiment may be deleted. In addition, a known technology may be added to the structure of a certain embodiment.
[0093] In the above embodiment, the case where the storage element is used as a non-aqueous electrolyte secondary battery (e.g., a lithium ion secondary battery) capable of charge and discharge is described, but the type, shape, size, capacity, etc. of the storage element are arbitrary. The present invention can also be applied to capacitors such as various secondary batteries, double-layer capacitors, or lithium ion capacitors. In the above embodiment, an electrode body formed by stacking or winding a positive electrode and a negative electrode with a separator is described, but the electrode body may not have a separator. For example, the positive electrode and the negative electrode may be in direct contact with each other in a state where a non-conductive layer is formed on the active material layer of the positive electrode or the negative electrode. Example
[0094] The present invention will be described in more detail below by way of examples, but the present invention is not limited to the following examples.
[0095] [Example 1] (Production of negative electrode) A negative electrode mixture paste is prepared which contains silicon oxide (SiO) as a negative electrode active material, carbon covering its surface, graphite (Gr) as a negative electrode active material, single-walled carbon nanotubes (SWCNT) as a conductive agent, styrene-butadiene rubber (SBR) as a rubber-based binder, and carboxymethyl cellulose (CMC) as a thickener in a mass ratio of 72.8:2.2:14.9:0.1:8.8:1.2 (converted to solid content), and contains water as a dispersion medium. The above-mentioned negative electrode mixture paste is applied to one side of a copper foil as a negative electrode substrate, and pressed after drying to prepare a negative electrode having a negative electrode active material layer arranged on one side of the negative electrode substrate. Silicon oxide (SiO) used is silicon oxide pre-doped with lithium ions. In addition, the average particle size of silicon oxide (SiO) is 7μm.
[0096] (Production of positive electrode) As the positive electrode active material, LiNi 0.5 Co 0.2 Mn 0.3 A lithium transition metal composite oxide represented by O2. A positive electrode mixture paste containing the above-mentioned positive electrode active material, acetylene black (AB) and SWCNT as conductive agents, and polyvinylidene fluoride (PVDF) as a binder at a mass ratio of 97.72:1.00:0.09:1.19 (converted to solid content), and containing N-methylpyrrolidone (NMP) as a dispersion medium is prepared. The above-mentioned positive electrode mixture paste is applied to one side of an aluminum foil as a positive electrode substrate, and pressed after drying to prepare a positive electrode having a positive electrode active material layer arranged on one side of the positive electrode substrate.
[0097] (Preparation of non-aqueous electrolyte) Make LiPF6 at 1.6 mol / dm 3 The concentration was dissolved in a mixed solvent of FEC and TFEMC in a volume ratio of 30:70 to prepare a non-aqueous electrolyte.
[0098] (Production of energy storage elements) The positive electrode and the negative electrode are stacked with a polyolefin microporous film as a separator to produce an electrode body. The separator has a heat-resistant layer on the positive electrode side, and the heat-resistant layer contains heat-resistant particles of aluminosilicate. The electrode body is housed in a container made of a metal-resin composite film, and after the non-aqueous electrolyte is injected into the container, it is sealed by heat welding to obtain the storage element of Example 1.
[0099] [Example 2, Example 3, Example 5 to Example 7 and Comparative Example 2, Comparative Example 10] Except that the contents of silicon oxide and graphite as negative electrode active materials and SBR as rubber-based binder were set as shown in Table 2, the same operation as in Example 1 was carried out to obtain storage elements of Examples 2, 3, 5 to 7 and Comparative Examples 2 and 10.
[0100] [Example 4] An electric storage device of Example 4 was obtained in the same manner as in Example 1 except that graphite was not used as the negative electrode active material and the contents of silicon oxide as the negative electrode active material and single-walled carbon nanotubes as the conductive agent were as shown in Table 2.
[0101] [Comparative Example 1] The storage element of Comparative Example 1 was obtained in the same manner as in Example 1, except that single-walled carbon nanotubes were not used as the conductive agent, and the contents of silicon oxide and graphite as the negative electrode active material, acetylene black as the conductive agent, and styrene-butadiene rubber as the rubber-based binder were as shown in Table 2.
[0102] [Comparative Example 3] An electric storage device of Comparative Example 3 was obtained in the same manner as in Example 1 except that single-walled carbon nanotubes were not used as a conductive agent and the contents of silicon oxide and graphite as negative electrode active materials and acetylene black as a conductive agent were as shown in Table 2.
[0103] [Comparative Example 4] A storage element of Comparative Example 4 was obtained in the same manner as in Comparative Example 1, except that acetylene black was used as a conductive agent instead of single-walled carbon nanotubes, sodium polyacrylate (PAANa) was used as a binder instead of SBR as a rubber-based binder and CMC as a thickener, and the contents of silicon oxide and graphite as negative electrode active materials, acetylene black as a conductive agent, and sodium polyacrylate as a binder were as shown in Table 2.
[0104] [Comparative Examples 5 to 9] The storage elements of Comparative Examples 5 to 9 were obtained by following the same procedure as in Comparative Example 4, except that single-walled carbon nanotubes were used as the conductive agent, and the contents of silicon oxide and graphite as the negative electrode active material, single-walled carbon nanotubes as the conductive agent, and sodium polyacrylate as the binder were as shown in Table 2.
[0105] (Initial charge and discharge 1) For each of the obtained storage elements of Examples 1 to 7 and Comparative Examples 1 to 9, initial charge and discharge 1 was performed according to the following steps (1) and (2) at 25°C. It should be noted that the storage element in the initial (first cycle or second cycle) fully charged state (the state after constant current constant voltage charging to a set charge termination voltage in the storage element. In the later-described Examples 1 to 7, Examples 12 to 15, and Comparative Examples 1 to 11, the charge termination voltage is 4.5V. In the later-described Examples 8 to 11, Examples 16 to 18, and Comparative Example 7-1, the charge termination voltage is 4.25V) is subjected to constant current discharge, and the current that becomes a fully discharged state (the state after constant current discharge to a set discharge termination voltage in the storage element. In the later-described Examples and Comparative Examples, the discharge termination voltage is 2.5V) within 10 hours is set to 0.1C. The current of 0.1C can be calculated and estimated based on the positive electrode capacity, negative electrode capacity, design of the storage element, etc. During the initial charge and discharge of the storage element, when constant current discharge is performed at a current of 0.1C, the appropriateness of the current of 0.1C can be confirmed by confirming that the discharge time is approximately 10 hours. (1) Perform constant current charging with a charging current of 0.1C and a charging time of 3 hours. After a rest period of 12 hours, perform constant current and constant voltage charging with a charging current of 0.1C and a charging end voltage of 4.5V. The charging end condition is set to when the charging current reaches 0.05C. Then, set a rest period of 10 minutes. Then, perform constant current discharge with a discharge current of 0.1C and a discharge end voltage of 2.5V, and then set a rest period of 10 minutes. (2) Then, constant current and constant voltage charging is performed with a charging current of 0.2C and a charging end voltage of 4.5V. The end condition of charging is set when the charging current reaches 0.05C. Then, a rest period of 10 minutes is set. Then, constant current discharge is performed with a discharge current of 0.1C and a discharge end voltage of 2.5V, and then a rest period of 10 minutes is set.
[0106] (Charge and discharge cycle test 1) Next, the following charge and discharge cycle test 1 was performed under an environment of 25°C. Constant current and constant voltage charging was performed with a charging current of 0.5C and a charge end voltage of 4.5V. The end condition of charging was set until the charging current reached 0.05C. Then, a 10-minute rest period was set. Then, constant current discharge was performed with a discharge current of 0.5C and a discharge end voltage of 2.5V, and then a 10-minute rest period was set. These charging, discharging and resting steps were regarded as one cycle, and 500 cycles were implemented.
[0107] (Capacity confirmation test 1) After the above-mentioned charge and discharge cycle test 1 has been completed for 300 cycles and 500 cycles, the following capacity confirmation test 1 is performed under a 25°C environment. Constant current and constant voltage charging is performed with a charging current of 0.2C and a charge end voltage of 4.5V. The end condition of charging is set until the charging current reaches 0.05C. Then, a rest period of 10 minutes is set. Then, constant current discharge is performed with a discharge current of 0.1C and a discharge end voltage of 2.5V, and then a rest period of 10 minutes is set.
[0108] (Capacity maintenance rate) The ratio of the discharge capacity after 300 cycles and 500 cycles obtained in the above capacity confirmation test 1 to the discharge capacity obtained in the above initial charge and discharge (2) was determined as the capacity retention rate [%). The results are shown in Table 2.
[0109] (Discharge capacity per unit of negative electrode active material) Table 2 shows the discharge capacity per unit negative electrode active material obtained by dividing the discharge capacity obtained in the initial charge and discharge (2) by the mass of the negative electrode active material contained in the region of the negative electrode facing the positive electrode.
[0110] (Discharge capacity per unit area of positive electrode) Table 2 shows the value obtained by dividing the discharge capacity obtained in the initial charge and discharge (2) by the area of the positive electrode as the discharge capacity per unit area of the positive electrode.
[0111] [Table 2]
[0112] As shown in Table 2, the content of the silicon-based negative electrode active material in the negative electrode active material layer is 68 mass % or more, the content of the rubber-based binder in the negative electrode active material layer is 3.0 mass % or more, and the content of the carbon nanotubes in the negative electrode active material layer is 0.4 (0.4 × (n 2 In the storage elements of Examples 1 to 7 in which the content of the negative electrode is less than 2n+4) / (2n+3) by mass%, the discharge capacity per unit of the negative electrode active material is high, and the decrease in the capacity retention rate after the charge and discharge cycle is suppressed. In addition, in Example 4 in which the content of the silicon-based negative electrode active material is large, the discharge capacity per unit of the negative electrode active material is particularly high, and the effect of suppressing the decrease in the capacity retention rate after the charge and discharge cycle is excellent. On the other hand, in Comparative Examples 1, 2, 4 and 5, in which the content of the silicon-based negative electrode active material is less than 68% by mass, Comparative Example 3, in which the content of the silicon-based negative electrode active material is 68% by mass or more but does not contain carbon nanotubes as a conductive agent, and Comparative Examples 6 to 9, in which the content of the silicon-based negative electrode active material is 68% by mass or more but contains sodium polyacrylate as a binder other than a rubber-based binder, the discharge capacity per unit of the negative electrode active material is lowered, or the effect of suppressing the decrease in the capacity retention rate after charge and discharge cycles is lowered compared to Examples 1 to 7. In addition, in Comparative Example 10, in which the content of the silicon-based negative electrode active material is 68% by mass or more but the content of the rubber-based binder in the negative electrode active material layer is less than 3.0% by mass, the effect of suppressing the decrease in the capacity retention rate after charge and discharge cycles is lowered.
[0113] [Example 8 to Example 11] Hard carbon (HC) was used as the negative electrode active material instead of graphite, the average particle size of silicon oxide as the negative electrode active material was changed to 11 μm, the contents of silicon oxide, HC and SBR as the rubber-based binder as the negative electrode active material were set as shown in Table 3, and the non-aqueous electrolyte was changed to make LiPF6 at 1.5 mol / dm 3 Each of the energy storage devices of Examples 8 to 11 was obtained in the same manner as in Example 1, except that a nonaqueous electrolyte was dissolved in a mixed solvent in which FEC and EMC were mixed in a volume ratio of 30:70.
[0114] (Initial charge and discharge 2) The obtained energy storage devices of Examples 8 to 11 were initially charged and discharged in an environment of 25° C. according to the following procedures (3) and (4). (3) Perform constant current charging with a charging current of 0.1C and a charging time of 3 hours. After a rest period of 12 hours, perform constant current and constant voltage charging with a charging current of 0.1C and a charging end voltage of 4.25V. The end condition of charging is set to when the charging current reaches 0.05C. Then, set a rest period of 10 minutes. Then, perform constant current discharge with a discharge current of 0.1C and a discharge end voltage of 2.5V, and then set a rest period of 10 minutes. (4) Then, constant current and constant voltage charging is performed with a charging current of 0.2C and a charging end voltage of 4.25V. The end condition of charging is set when the charging current reaches 0.05C. Then, a rest period of 10 minutes is set. Then, constant current discharge is performed with a discharge current of 0.1C and a discharge end voltage of 2.5V, and then a rest period of 10 minutes is set. Furthermore, initial charge and discharge were performed in an environment of 45° C. according to the following procedure (5). (5) Perform constant current and constant voltage charging with a charging current of 1.0C and a charging end voltage of 4.25V. The end condition of charging is set to when the charging current reaches 0.05C. Then, a rest period of 10 minutes is set. Then, perform constant current discharge with a discharge current of 0.2C and a discharge end voltage of 2.5V, and then a rest period of 10 minutes is set. (Charge and discharge cycle test 2) Next, the following charge and discharge cycle test 2 was performed under an environment of 45°C. Constant current and constant voltage charging was performed with a charging current of 2.0C and a charge end voltage of 4.25V. The end condition of charging was set until the charging current reached 0.05C. Then, a rest period of 10 minutes was set. Then, constant current discharge was performed with a discharge current of 2.0C and a discharge end voltage of 2.5V, and then a rest period of 10 minutes was set. These charging, discharging and resting steps were regarded as one cycle, and 500 cycles were implemented. (Capacity confirmation test 2) After the above-mentioned charge and discharge cycle test 2 was completed for 300 cycles and 500 cycles, the following capacity confirmation test 2 was performed in an environment of 45°C. Constant current and constant voltage charging was performed with a charging current of 1.0C and a charge end voltage of 4.25V. The end condition of charging was set until the charging current reached 0.05C. Then, a rest period of 10 minutes was set. Then, constant current discharge was performed with a discharge current of 0.2C and a discharge end voltage of 2.5V, and then a rest period of 10 minutes was set.
[0115] (Capacity maintenance rate) The ratio of the discharge capacity after 300 cycles and after 500 cycles obtained in the above capacity confirmation test 2 to the discharge capacity obtained in the above initial charge and discharge (5) was calculated as the capacity retention rate [%). The results are shown in Table 3.
[0116] (Discharge capacity per unit of negative electrode active material) Table 3 shows the discharge capacity per unit of negative electrode active material as a value obtained by dividing the discharge capacity obtained in the initial charge and discharge (4) by the mass of the negative electrode active material contained in the region 5 of the negative electrode facing the positive electrode.
[0117] (Discharge capacity per unit area of positive electrode) The value obtained by dividing the discharge capacity obtained in the initial charge and discharge (4) by the area of the positive electrode is shown in Table 3 as the discharge capacity per unit area of the positive electrode.
[0118] [Table 3]
[0119] As shown in Table 3, in the storage devices of Examples 8 and 9 in which the content of the rubber-based binder in the negative electrode active material layer was 6.0 mass % or more, the effect of suppressing the decrease in the capacity retention rate after charge and discharge cycles was further improved.
[0120] [Examples 12 to 14 and Comparative Example 11] Except that graphite was not used as the negative electrode active material and the contents of silicon oxide as the negative electrode active material, SWCNT as the conductive agent, and CMC as the thickener were as shown in Table 4, the same operation as in Example 1 was carried out to obtain each storage element of Examples 12 to 14 and Comparative Example 11. [Example 15] The storage element of Example 15 was obtained in the same manner as in Example 1, except that hard carbon (HC) was used instead of graphite as the negative electrode active material, and the contents of silicon oxide as the negative electrode active material, HC, SWCNT as the conductive agent, and CMC as the thickener were as shown in Table 4.
[0121] (High rate discharge performance test) After the above-mentioned initial charge and discharge (1) and (2) were performed on each of the energy storage elements obtained in Examples 12 to 15 and Comparative Example 11, the following high-rate discharge performance test was performed under an environment of 25°C. Constant current and constant voltage charging was performed with a charging current of 0.2C and a charging end voltage of 4.5V. The end condition of charging was set to when the charging current reached 0.05C. A rest period of 10 minutes was set after charging. Then, constant current discharge was performed with a discharge current of 0.1C and a discharge end voltage of 2.5V, and then a rest period of 10 minutes was set. The obtained discharge capacity was referred to as "0.1C discharge capacity". Next, constant current and constant voltage charging was performed with a charging current of 0.2C and a charging end voltage of 4.5V. The end condition of charging was set to when the charging current reached 0.05C. A rest period of 10 minutes was set after charging. Then, constant current discharge was performed with a discharge current of 1.0C and a discharge end voltage of 2.5V, and then a rest period of 10 minutes was set. The obtained discharge capacity is referred to as “1.0 C discharge capacity”. The percentage of the 1.0 C discharge capacity to the 0.1 C discharge capacity is shown in Table 4 as "high rate discharge performance (1.0 C / 0.1 C [%])".
[0122] The discharge capacity per unit area of the positive electrode was determined in the same manner as described above for each of the energy storage devices of Examples 12 to 15 and Comparative Example 11. The results are shown in Table 4.
[0123] [Table 4]
[0124] As shown in Table 4, the content of carbon nanotubes in the negative electrode active material layer is 0.4 (0.4 × (n 2 In the energy storage devices of Examples 12 to 15, the content of carbon nanotubes exceeds 0.4 (0.4×(n 2 Compared with the energy storage element of Comparative Example 11 in which n=1) mass % of (2n+4) / (2n+3), the decrease in high-rate discharge performance was suppressed.
[0125] [Example 16 to Example 18 and Comparative Example 7-1] The average particle size of silicon oxide as the negative electrode active material was changed to 11 μm, the contents of silicon oxide and graphite as the negative electrode active material, the type and content of the binder, and the content of CMC as the thickener were set as shown in Table 5, and the non-aqueous electrolyte was changed to make LiPF6 at 1.5 mol / dm 3 Each of the energy storage elements of Examples 16 to 18 and Comparative Example 7-1 was obtained in the same manner as in Example 1, except that a nonaqueous electrolyte was dissolved in a mixed solvent of FEC and EMC at a volume ratio of 30:70.
[0126] (Charge and discharge cycle test 3) For each of the energy storage elements of Examples 16 to 18 and Comparative Example 7-1, after the above-mentioned initial charge and discharge (3), (4) and (5) were performed, the charge and discharge cycle test 3 was performed. The charge and discharge cycle test 3 was performed in the same manner as the charge and discharge cycle test 2 except that the number of test cycles was set to 300 cycles. Then, under the same conditions as the above-mentioned capacity confirmation test 2, the capacity confirmation test 4 was performed.
[0127] For each of the energy storage devices of Examples 16 to 18 and Comparative Example 7-1, the ratio of the discharge capacity after 300 cycles obtained in the above capacity confirmation test 4 to the discharge capacity obtained in the above initial charge and discharge (5) was determined as the capacity retention rate [%). The results are shown in Table 5.
[0128] [Table 5]
[0129] As shown in Table 5, in the storage elements of Example 17 and Example 18 in which the negative electrode active material layer contains a rubber-based binder as the main component of the binder, the effect of suppressing the decrease in capacity retention rate after charge and discharge cycles is further improved compared with the storage element of Comparative Example 7-1 that does not contain a rubber-based binder and the storage element of Example 16 that contains a rubber-based binder but is not the main component of the binder.
[0130] The above results show that the negative electrode contains 68% by mass or more of silicon-based negative electrode active material, 3.0% by mass or more of rubber-based binder and 0.4×(n 2 +4) / (2n+3) mass % or less (where n is the number of graphene layers forming the carbon nanotubes), the discharge capacity of the storage element can be increased and the decrease in capacity retention rate after charge and discharge cycles and the decrease in high-rate discharge characteristics can be suppressed. Possibility of industrial application
[0131] The present invention can be applied to power storage elements used as power sources for electronic devices such as personal computers and communication terminals, automobiles, and aircraft, and the like. Description of Reference Numerals
[0132] 1 electricity storage element; 2 electrode body; 3 container; 4 positive electrode terminal; 41 positive electrode lead; 5 negative electrode terminal; 51 negative electrode lead; 20 electricity storage unit; 30 electricity storage device.
Claims
1. A negative electrode for a storage element, comprising a negative electrode active material layer, wherein the negative electrode active material layer contains a silicon-based negative electrode active material, a rubber-based binder and carbon nanotubes, The content of the silicon-based negative electrode active material in the negative electrode active material layer is 68% by mass or more, The content of the rubber-based binder in the negative electrode active material layer is 3.0% by mass or more, The content of the carbon nanotubes in the negative electrode active material layer is 0.4×(n 2 +4) / (2n+3) mass % or less, wherein, n is the number of graphene layers forming the carbon nanotube. 2 . The negative electrode for an electric storage device according to claim 1 , wherein a content of the carbon nanotubes in the negative electrode active material layer is 0.4 mass % or less. 3 . The negative electrode according to claim 1 , wherein the negative electrode active material layer further contains a carbon-based material, and the total content of the carbon nanotubes and the carbon-based material in the negative electrode active material layer is 22% by mass or less. 4 . The negative electrode according to claim 1 , wherein a content of the rubber-based binder in the negative electrode active material layer is 6.0% by mass or more. The negative electrode according to claim 1 or 2, wherein the carbon nanotubes comprise single-walled carbon nanotubes. 6 . An electric storage element comprising the negative electrode according to claim 1 . 7 . A power storage device comprising two or more power storage elements, comprising one or more power storage elements according to claim 6 .