Alloy metal getter and preparation method thereof
Through the preparation of alloy metal getter, the safety hazards and low efficiency of the traditional hydrogen removal process are solved, and efficient hydrogen adsorption and desorption are achieved, the hydrogen purity and storage capacity are improved, and the process complexity and cost are reduced.
Patent Information
- Application Number
- CN202411011862.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional hydrogen removal processes have problems such as safety hazards, low efficiency and high process complexity in natural gas production. Especially high concentrations of hydrogen can easily burn the catalyst, and the treatment of moisture increases cost and complexity.
Using alloy metal getters, including Zr, V, Fe, Ti, Al, etc., through the vacuum furnace preparation method, suspended smelting and fast cooling treatment, alloy particles with high-efficiency hydrogen adsorption and desorption capabilities are obtained to ensure safety and purity. .
It realizes efficient hydrogen adsorption and desorption, improves the purity and storage capacity of hydrogen, reduces safety risks, extends the service life of getters, and reduces process complexity and cost.
Smart Images

Figure CN118874398A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of natural gas production, and in particular to an alloy metal getter and a preparation method thereof. Background Art
[0002] In the field of natural gas production, the process of extracting helium usually requires the treatment of crude helium containing hydrogen to meet the production needs of high-purity helium. Traditional hydrogen removal processes often use catalysts and excess oxygen to react to generate water, then remove water through a dehydration device, and finally remove oxygen and nitrogen components through cryogenic distillation. However, these traditional processes have many problems, which limit their efficiency and safety in practical applications.
[0003] First, the explosion-proof requirements of natural gas production sites require the introduction of oxygen to increase the safety distance between the site and equipment, increasing space waste and safety hazards. Secondly, in the traditional dehydrogenation process, high concentrations of hydrogen will cause catalytic combustion to release a large amount of heat energy, which can easily burn catalysts and purification equipment, posing serious safety risks. In addition, the water generated by the traditional process requires additional dehydration equipment to meet the requirements of high-purity helium, and the regeneration of the dehydration adsorbent needs to be considered, which increases the complexity and cost of the process. Summary of the invention
[0004] In order to solve the above technical problems, the present application provides an alloy metal getter and a preparation method thereof. In a first aspect, the present application provides an alloy metal getter comprising the following components: Zr: 10-60% (w / w); V: 5-50% (w / w); Fe: 5-50% (w / w); Ti: 3-10% (w / w); Al: 2-15% (w / w).
[0005] Optional, where: Mn<0.3%(w / w); C<0.01%(w / w); Hf<0.4%(w / w).
[0006] The second aspect of the present application provides a method for preparing an alloy metal getter, which is used to prepare the alloy metal getter as described in the first aspect and any optional aspect of the first aspect, and the preparation method comprises: Conduct air tightness test on the vacuum furnace until it is determined that the pressure rise rate of the vacuum furnace is ≤1Pa / h; Perform an ultimate vacuum test on the vacuum furnace at room temperature until the vacuum degree of the vacuum furnace is determined to be ≤5×10^-2Pa; Zirconium sheets with purities of 99.8%, vanadium sheets with purities of 99.8%, titanium sponge sheets with purities of 99%, and refined electrolytic aluminum sheets are selected as standby materials; The material to be used is placed in a crucible of a vacuum furnace and argon gas is introduced; Replace the vacuum in the vacuum furnace; After the replacement is completed, the alloy is obtained by suspension smelting; The alloy was turned over and melted three times; After melting the alloy, it is cast in a water-cooled mold for rapid cooling to embrittle the matrix; The rapidly cooled alloy is crushed into particles of 20 to 60 mesh; The alloy particles are processed and finally sieved to obtain alloy particles with a particle size that meets the target value.
[0007] Optional, airtightness test of the vacuum furnace includes: The vacuum furnace was filled with argon gas to 0.2 MPa, and a pressure-maintaining experiment was performed for 1 hour.
[0008] Optionally, the processing of the alloy particles includes: The alloy particles are ground by mechanical grinding.
[0009] Optionally, during the three times of turning over and smelting, the crucible is rotated before each smelting.
[0010] Optionally, during the rapid cooling process, a hydrogen gas flow is used to cool the alloy.
[0011] Optionally, mechanical grinding methods include ball milling, grinding mill or vibration mill.
[0012] It can be seen from the above technical solutions that this application has the following advantages: This getter has the following advantages: 1. The hydrogen diffusion rate inside the getter is fast, and the hydrogen can be quickly stored in the form of solid solution, thereby improving the adsorption efficiency and storage capacity of hydrogen.
[0013] 2. The adsorption of hydrogen by the getter is reversible, and can achieve reversible adsorption and desorption of hydrogen, which is conducive to the efficient utilization of energy in the process of adsorption and release of hydrogen.
[0014] 3. As time goes by, the weak chemical adsorption on the surface of the getter will gradually be replaced by stable strong chemical adsorption, reaching a thermodynamic equilibrium state, ensuring the stability and reliability of the adsorption and desorption process.
[0015] 4. The getter will not adsorb inert gases, ensuring that the getter is not disturbed by inert gases during the adsorption and desorption process, thereby improving the purity and adsorption efficiency of hydrogen.
[0016] 5. The getter has strong anti-poisoning performance for the dissociation adsorption products of water vapor, oxygen, carbon monoxide and other gases, ensuring that the getter's adsorption and desorption capabilities for hydrogen are not affected under certain temperature conditions, thereby extending the service life and stability of the getter. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The present invention is a schematic flow chart of an embodiment of a method for preparing an alloy metal getter provided in the present application. DETAILED DESCRIPTION
[0018] In the present application, the terms "upper", "lower", "left", "right", "front", "back", "top", "bottom", "inside", "outside", "middle", "vertical", "horizontal", "lateral", "longitudinal" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only used to illustrate the relative positional relationships between the various components or components, and do not particularly limit the specific installation orientations of the various components or components.
[0019] In addition, some of the above terms may be used to express other meanings in addition to indicating orientation or positional relationship. For example, the term "on" may also be used to express a certain dependency or connection relationship in some cases. For those of ordinary skill in the art, the specific meanings of these terms in this application can be understood according to specific circumstances.
[0020] In addition, the terms "installed", "set", "provided with", "connected", and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral structure; it can be a mechanical connection, or an electrical connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be an internal connection between two devices, elements, or components. For those of ordinary skill in the art, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0021] In addition, the structures, proportions, sizes, etc. drawn in the drawings in the present application are only used to match the contents disclosed in the specification for the technical personnel in this field to understand and read, and are not used to limit the restrictive conditions under which the present application can be implemented. Therefore, they have no substantive technical significance. Any structural modification, change in proportional relationship or adjustment of size should still fall within the scope of the technical content disclosed in the present application without affecting the effects and purposes that can be achieved by the present application.
[0022] The following will be combined with the drawings in this application to clearly and completely describe the technical solutions in this application. Obviously, the described embodiments are only part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0023] Embodiment 1: The present application first provides an embodiment of an alloy metal getter. This embodiment provides an alloy metal getter, and its specific components are as follows: Zirconium (Zr): The content in the alloy ranges from 10% to 60% (w / w), i.e. the mass percentage is between 10% and 60%. Zirconium is one of the main components used to provide the basic structure and specific properties of the getter.
[0024] Vanadium (V): The content in the alloy ranges from 5% to 50% (w / w), that is, the mass percentage is between 5% and 50%. Vanadium is one of the important components of the alloy and helps to adjust the hardness, strength and other mechanical properties of the alloy.
[0025] Iron (Fe): The content in the alloy ranges from 5% to 50% (w / w), that is, the mass percentage is between 5% and 50%. Iron is one of the main strengthening elements in the alloy, which helps to increase the strength and wear resistance of the alloy.
[0026] Titanium (Ti): The content in the alloy ranges from 3% to 10% (w / w), that is, the mass percentage is between 3% and 10%. Titanium is one of the added elements of the alloy, which helps to improve the corrosion resistance and high temperature resistance of the alloy.
[0027] Aluminum (Al): The content in the alloy ranges from 2% to 15% (w / w), that is, the mass percentage is between 2% and 15%. Aluminum is one of the added elements of the alloy and can be used to adjust the grain size and crystal morphology of the alloy, thereby affecting the mechanical properties and processing properties of the alloy.
[0028] Embodiment 2: In an optional embodiment, the content of each material is limited as follows: Manganese (Mn): The content must be kept below 0.3% (w / w), that is, the mass percentage is below 0.3%. The manganese content limit helps to ensure the purity and stability of the alloy and avoid the adverse effects of manganese on the alloy properties.
[0029] Carbon (C): The content must be kept below 0.01% (w / w), that is, the mass percentage is below 0.01%. Controlling the carbon content helps reduce the alloy's carburization tendency and improve the alloy's strength and corrosion resistance.
[0030] Hafnium (Hf): The content must be kept below 0.4% (w / w), that is, the mass percentage is below 0.4%. Limiting the content of hafnium helps prevent excessive solid solution or precipitation of hafnium in the alloy, thereby maintaining the uniformity and stability of the alloy.
[0031] Embodiment three: The present application also provides a method for preparing an alloy metal getter, see Figure 1 , the following is a description of the embodiment of the preparation method: The present application first provides an embodiment of a method for preparing an alloy metal getter, which comprises: S101. Perform air tightness test on the vacuum furnace until it is determined that the pressure increase rate of the vacuum furnace is ≤1Pa / h; In this step, the vacuum furnace is first tested for air tightness to ensure that the vacuum furnace can meet certain sealing standards. The test method can use a pressure gauge or other test equipment to ensure that the gas inside the vacuum furnace will not leak out. The test will continue until the vacuum furnace's pressure increase rate reaches the specified standard of ≤1Pa / h.
[0032] Specifically, the method may include filling the vacuum furnace with argon gas to 0.2 MPa and performing a pressure holding experiment for 1 hour.
[0033] The following example illustrates the test process: First, you need to prepare the equipment for testing, such as a pressure gauge or other equipment specifically for vacuum testing. These equipment include a vacuum gauge, a pressure gauge, a vacuum pump, and the corresponding pipe connections.
[0034] Determine the environmental conditions for the test, including ambient temperature and pressure, etc. Ensure that the test environment is stable so that the airtightness of the vacuum furnace can be accurately measured.
[0035] Connect the test equipment to the vacuum furnace's gas outlet or other appropriate interface. Make sure the connection is well sealed to prevent gas leakage.
[0036] Start the test equipment and record the vacuum and pressure at the initial moment. After starting the test, the test equipment will monitor the pressure changes inside the vacuum furnace.
[0037] Continuously monitor the pressure changes inside the vacuum furnace. By monitoring the rate of change of the pressure, the airtightness of the vacuum furnace can be evaluated. The pressure increase rate refers to the increase in pressure inside the vacuum furnace per unit time, usually in Pascals per hour (Pa / h). Ensure that the pressure change rate is within the specified range.
[0038] If the test finds that the air pressure change rate exceeds the specified range, it is necessary to adjust and repair the sealing components of the vacuum furnace in time to ensure that it can meet the required airtightness standards.
[0039] Continue testing until the pressure rise rate of the vacuum furnace reaches the specified standard of ≤1Pa / h. Once the standard is reached, it can be confirmed that the airtightness of the vacuum furnace has met the requirements.
[0040] Through the above steps, the air tightness test of the vacuum furnace can be effectively carried out, and it can be ensured that it reaches a certain sealing standard to meet the subsequent process requirements for preparing alloy metal getters.
[0041] S102, performing a limit vacuum test on the vacuum furnace at room temperature until it is determined that the vacuum degree of the vacuum furnace is ≤5×10^-2Pa; In this step, the vacuum furnace is tested for extreme vacuum to ensure that the vacuum degree meets the required standard. The vacuum degree of the vacuum furnace can be tested at room temperature using a vacuum gauge or other vacuum detection equipment. The test will continue until the vacuum degree of the vacuum furnace reaches the requirement of ≤5×10^-2Pa.
[0042] S103, selecting zirconium sheets with purities of 99.8%, vanadium sheets with purities of 99.8%, titanium sponge sheets with purities of 99%, and refined electrolytic aluminum sheets as standby materials; In this step, materials with specific purity are selected as raw materials for preparing the alloy. According to an embodiment, the selected materials include 99.8% pure zirconium sheets, 99.8% pure vanadium sheets, 99% pure sponge titanium and refined electrolytic aluminum sheets.
[0043] S104, placing the material to be used into a crucible of a vacuum furnace, and introducing argon gas; The selected materials to be used are placed in a crucible in a vacuum furnace, and an inert atmosphere is created by introducing argon gas to reduce the oxidation reaction of the materials at high temperatures.
[0044] S105, replacing the vacuum furnace by evacuating the vacuum furnace; In this step, the vacuum furnace is evacuated to remove air and gases from the furnace to ensure that the material is processed in an oxygen-free environment.
[0045] S106, after the replacement is completed, the alloy is obtained by suspension smelting; The materials to be used are heated to a molten state and mixed to form an alloy by suspension melting in a vacuum furnace.
[0046] S107, turning over and melting the alloy 3 times; In this step, the alloy is reheated several times to ensure that the alloy components are evenly mixed.
[0047] Specifically, the crucible is rotated before each smelting. The purpose of rotating the crucible is to heat the alloy material more evenly and prevent local overheating or uneven melting. By rotating the crucible, the alloy material can be ensured to be evenly heated and mixed during the melting process.
[0048] S108, casting the alloy after melting into a water-cooling mold for rapid cooling to embrittle the matrix; The molten alloy is poured into a water-cooled mold to quickly cool the alloy and embrittle its matrix.
[0049] Specifically, during the rapid cooling process, a hydrogen gas flow is used to cool the alloy. By using a hydrogen gas flow for rapid cooling treatment, the temperature of the alloy can be rapidly reduced, thereby effectively controlling its grain structure and properties.
[0050] S109, crushing the rapidly cooled alloy into particles of 20 to 60 mesh; The rapidly cooled alloy is crushed into particles with a particle size ranging from 20 to 60 meshes.
[0051] S110, processing the alloy particles, and finally screening to obtain alloy particles with a particle size that meets the target value.
[0052] The alloy particles are processed, which may include steps such as fine grinding or screening, to obtain alloy particles with a final particle size that meets the target value.
[0053] The preparation method of this embodiment has several advantages: This method uses high-purity materials such as 99.8% zirconium sheets, 99.8% vanadium sheets, 99% sponge titanium and refined electrolytic aluminum sheets to ensure the quality and performance of the alloy metal getter.
[0054] By processing in a vacuum furnace, air and impurities can be effectively removed to ensure the purity and stability of the alloy metal getter.
[0055] The alloy is obtained by suspension smelting, which can make the alloy composition more uniform and improve the stability and performance of the alloy.
[0056] By performing a rapid cooling treatment in a water-cooled mold, the matrix of the alloy can be embrittled, which is beneficial to subsequent processing and application.
[0057] Finally, the alloy particles are processed and screened to ensure that the size and particle size of the particles meet the target requirements, thereby improving the application effect and stability of the alloy metal getter.
[0058] It should be noted that the above description of the disclosed embodiments enables professionals and technicians in the field to implement or use the present application. Various modifications to these embodiments will be apparent to professionals and technicians in the field, and the general principles defined herein can be implemented in other embodiments without departing from the scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but should conform to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. An alloy metal getter, characterized in that: The components include: Zr: 10-60% (w / w); V: 5-50% (w / w); Fe: 5-50% (w / w); Ti: 3-10% (w / w); Al: 2-15% (w / w).
2. The alloy metal getter according to claim 1, characterized in that: in: Mn<0.3%(w / w); C<0.01%(w / w); Hf<0.4%(w / w).
3. A method for preparing an alloy metal getter, characterized in that: For preparing the alloy metal getter as claimed in claim 1 or 2, the preparation method comprises: Conduct air tightness test on the vacuum furnace until it is determined that the pressure rise rate of the vacuum furnace is ≤1Pa / h; Perform an ultimate vacuum test on the vacuum furnace at room temperature until the vacuum degree of the vacuum furnace is determined to be ≤5×10^-2Pa; Zirconium sheets with purities of 99.8%, vanadium sheets with purities of 99.8%, titanium sponge sheets with purities of 99%, and refined electrolytic aluminum sheets are selected as standby materials; The material to be used is placed in a crucible of a vacuum furnace and argon gas is introduced; Replace the vacuum in the vacuum furnace; After the replacement is completed, the alloy is obtained by suspension smelting; The alloy was turned over and melted three times; After melting the alloy, it is cast in a water-cooled mold for rapid cooling to embrittle the matrix; The rapidly cooled alloy is crushed into particles of 20 to 60 mesh; The alloy particles are processed and finally sieved to obtain alloy particles with a particle size that meets the target value.
4. The method for preparing the alloy metal getter according to claim 3, characterized in that: The airtightness test of the vacuum furnace includes: The vacuum furnace was filled with argon gas to 0.2 MPa, and a pressure-maintaining experiment was performed for 1 hour.
5. The method for preparing the alloy metal getter according to claim 3, characterized in that: The processing of the alloy particles comprises: The alloy particles are ground by mechanical grinding.
6. The method for preparing the alloy metal getter according to claim 3, characterized in that: During the three times of turning over and melting, the crucible is rotated before each melting.
7. The method for preparing the alloy metal getter according to claim 3, characterized in that: During the rapid cooling process, a hydrogen gas flow is used to cool the alloy.
8. The method for preparing the alloy metal getter according to claim 5, characterized in that: Mechanical grinding methods include ball milling, grinding mill or vibration mill.