Catalyst slurry, VOCs catalytic oxidation catalyst, and preparation methods and applications of catalyst slurry and VOCs catalytic oxidation catalyst

Perovskite composite oxides are prepared by combining precious metals, rare earth metals and additive metals, combining copper oxides and alkali metals to form high-stability catalysts, which solves the problem of insufficient activation performance of catalysts at high temperatures and low temperatures, and achieves the Efficient conversion and stability improvement of various VOCs.

CN118874486APending Publication Date: 2024-11-01CHINA PETROLEUM & CHEMICAL CORP +1

Patent Information

Application Number
CN202310483914.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing catalysts are prone to deactivate under high-temperature oxidation atmosphere and have insufficient oxidation performance on low-carbon hydrocarbons, making it difficult to efficiently treat a variety of VOCs at low temperatures.

Method used

The perovskite composite metal oxide is prepared by combining precious metals, rare earth metals and additive metals. Combining copper oxide and alkali metals, a high-stability catalyst is formed through specific slurry preparation methods and loading technology to improve the synergistic effect between active centers. Suppress reunion.

Benefits of technology

The high stability of the catalyst and the efficient conversion of a variety of VOCs at low temperatures are achieved. Especially when germanium is added, the catalytic performance is further improved, which is suitable for mass production and application of fixed bed catalytic materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874486A_ABST
    Figure CN118874486A_ABST
Patent Text Reader

Abstract

The invention relates to the field of catalyst preparation, and discloses catalyst slurry, a VOCs catalytic oxidation catalyst and preparation methods and applications of the catalyst slurry and the VOCs catalytic oxidation catalyst. The preparation method of the catalyst slurry comprises the following steps: (1) mixing a noble metal precursor, a rare earth metal precursor, an auxiliary metal precursor, a dispersing agent and a solvent, then adding ammonia water to adjust the pH value of the materials to 6-9, and stirring to obtain a mixed solution; after the reaction is finished, carrying out drying and roasting treatment to obtain a perovskite composite metal oxide; (2) mixing a copper precursor, an alkali metal precursor and the perovskite composite metal oxide, adjusting the pH value to 8-12, adding a binder and a matrix source, mixing, and grinding to obtain catalyst slurry; wherein the auxiliary metal is transition metal except precious metal, rare earth metal and Cu. The catalyst prepared by the method provided by the invention has high thermal stability, and can realize efficient conversion of various VOCs at low temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalyst preparation, and in particular to a method for preparing a catalyst slurry, a catalyst slurry prepared by the preparation method, a VOCs catalytic oxidation catalyst and a preparation method thereof, and application of the catalyst slurry or the VOCs catalytic oxidation catalyst in catalytic oxidation of VOCs. Background Art

[0002] Volatile Organic Compounds (VOCs) are the main pollutants in waste gas emitted during the production and processing of various industries such as petrochemicals, printing, and pharmaceuticals. They have a noticeable odor and can irritate or harm human organs. In severe cases, they can cause poisoning or cancer, endangering human health. In addition, VOCs participate in the formation of ozone and secondary aerosols in the atmospheric environment, and have an important impact on regional atmospheric ozone pollution and PM2.5 pollution.

[0003] VOCs pollution control can be divided into adsorption, incineration, catalytic oxidation, biological methods and membrane separation methods. Among them, catalytic oxidation technology is one of the most promising technologies for removing VOCs; and the development of high-performance catalytic oxidation catalysts is the key to achieving exhaust gas purification and green production. At present, catalytic oxidation catalysts are mostly based on honeycomb inert materials (such as cordierite, etc.) as carriers, loaded with active components with low-temperature oxidation properties to achieve VOCs catalytic oxidation.

[0004] VOCs catalytic oxidation catalysts usually use precious metals such as gold, silver, platinum, and palladium as active components. Precious metal catalysts show excellent oxidation activity for olefins and aromatics, but their oxidation performance for low-carbon alkanes common in the petrochemical industry is insufficient. To solve this problem, transition metal components can be introduced into VOCs catalysts to improve the activation performance of the catalyst for saturated carbon-hydrogen bonds. Such transition metals include manganese, cobalt, iron, etc. Through the combined application of multiple active centers, efficient treatment of complex VOCs components in the petrochemical industry can be achieved. CN106890642A discloses a platinum- and palladium-based catalytic oxidation catalyst for industrial kiln tail gas treatment and a preparation method thereof, wherein the coating material contains precious metals, aluminum oxide, cerium oxide, and manganese oxide.

[0005] However, in actual applications, both precious metal and non-precious metal active components tend to aggregate and deactivate under high temperature conditions in an oxidizing atmosphere, and some unstable transition metal active phases even undergo phase changes. How to improve the formulation and slurry preparation technology to provide a VOCs catalyst with high stability and high efficiency for simultaneously oxidizing alkanes, olefins, and aromatics at low temperatures is an urgent problem to be solved in this field. Summary of the invention

[0006] The purpose of the present invention is to overcome the problem of easy deactivation and instability of active components in catalysts in the prior art, and to provide a broad-spectrum catalytic oxidation catalyst with high stability and high efficiency in treating a variety of VOCs. The present invention specifically relates to a catalyst slurry, a VOCs catalytic oxidation catalyst, and their preparation methods and applications. The catalyst obtained by the present invention has high thermal stability and can achieve high-efficiency conversion of a variety of VOCs at low temperatures.

[0007] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a catalyst slurry, the method comprising:

[0008] (1) mixing a noble metal precursor, a rare earth metal precursor, an auxiliary metal precursor, a dispersant and a solvent, then adding ammonia water to adjust the pH of the material to 6-9, and reacting, and drying and calcining after the reaction to obtain a perovskite composite metal oxide;

[0009] (2) mixing a copper precursor, an alkali metal precursor and the perovskite composite metal oxide and adjusting the pH to 8-12, then adding a binder and a matrix source, mixing and grinding to obtain a catalyst slurry;

[0010] The additive metal is a transition metal other than precious metals, rare earth metals and Cu.

[0011] Preferably, the method further comprises: adding a germanium precursor in step (1) and / or step (2).

[0012] A second aspect of the present invention provides a catalyst slurry prepared according to the method described above.

[0013] The third aspect of the present invention provides a method for preparing a VOCs catalytic oxidation catalyst, which comprises loading the catalyst slurry as described above onto a carrier, and then performing drying and calcining treatment to obtain a VOCs catalytic oxidation catalyst.

[0014] A fourth aspect of the present invention provides a VOCs catalytic oxidation catalyst prepared according to the method described above.

[0015] A fifth aspect of the present invention provides a VOCs catalytic oxidation catalyst, the VOCs catalytic oxidation catalyst comprising a carrier and a catalyst layer supported on the carrier;

[0016] Wherein, the catalyst layer comprises active components and a matrix;

[0017] The active components include perovskite composite metal oxides, copper oxide, and alkali metal oxides; the perovskite composite metal oxides contain noble metals, rare earth metal oxides, and auxiliary metal oxides; and the auxiliary metals are transition metals other than noble metals, rare earth metals, and Cu.

[0018] Preferably, the active component further comprises germanium.

[0019] A sixth aspect of the present invention provides use of the catalyst slurry as described above or the VOCs catalytic oxidation catalyst as described above in catalytic oxidation of VOCs.

[0020] The catalyst in the present invention has high thermal stability and can achieve efficient conversion of various VOCs at low temperatures. In particular, when germanium is preferably contained, its performance can be further improved.

[0021] In the present invention, precious metals are combined with rare earth metals and auxiliary metals to prepare perovskite-type composite metal oxides, and used in combination with alkali metals and Cu, which effectively improves the synergistic effect between multiple active centers, inhibits agglomeration, effectively improves the utilization efficiency of active metals and the stability of the catalyst, and can improve the catalytic performance of the catalyst.

[0022] The preparation method provided in the present invention is easy to operate, suitable for batch production, and is expected to be extended to the preparation of various fixed-bed catalytic materials, thus having broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is the XRD spectrum of the perovskite composite oxide in Example 1;

[0024] Figure 2 This is the EXAFS spectrum of the perovskite composite oxide in Example 1 after hydrothermal aging at 800°C for 8 hours. DETAILED DESCRIPTION

[0025] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0026] A first aspect of the present invention provides a method for preparing a catalyst slurry, the method comprising:

[0027] (1) mixing a noble metal precursor, a rare earth metal precursor, an auxiliary metal precursor, a dispersant and a solvent, then adding ammonia water to adjust the pH of the material to 6-9, and reacting, and drying and calcining after the reaction to obtain a perovskite composite metal oxide;

[0028] (2) mixing a copper precursor, an alkali metal precursor and the perovskite composite metal oxide and adjusting the pH to 8-12, then adding a binder and a matrix source, mixing and grinding to obtain a catalyst slurry;

[0029] The additive metal is a transition metal other than precious metals, rare earth metals and Cu.

[0030] Preferably, the metal precursors (such as noble metal precursors, rare earth metal precursors, auxiliary metal precursors, copper precursors, germanium precursors and alkali metal precursors) are each independently a soluble salt thereof, such as at least one of acetates, nitrates and chlorides, more preferably nitrates.

[0031] Preferably, the noble metal is selected from at least one of platinum, palladium and rhodium. The noble metal precursor may be, for example, platinum nitrate, palladium nitrate and rhodium nitrate.

[0032] Preferably, the rare earth metal is lanthanum, and yttrium and / or praseodymium, that is, the rare earth metal is a combination of lanthanum and yttrium, a combination of lanthanum and praseodymium, or a combination of lanthanum, yttrium and praseodymium. The rare earth metal precursor may be, for example, lanthanum nitrate, yttrium nitrate, praseodymium nitrate, and the like.

[0033] Preferably, the auxiliary metal is selected from at least one of nickel, cobalt, manganese and iron. The rare earth metal precursor may be, for example, nickel nitrate, cobalt nitrate, manganese nitrate and iron nitrate.

[0034] Preferably, compared to 1 mol of lanthanum, the amount of the noble metal is 0.001-0.1 mol, for example, 0.001, 0.005, 0.01, 0.02, 0.04, 0.06, 0.08, 0.1 mol and any range between any two values, more preferably 0.01-0.06 mol; the amount of yttrium and / or praseodymium is 0.01-0.1 mol, for example, 0.001, 0.005, 0.01, The dosage of the auxiliary metal is 0.5-1.5 mol, for example, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5 mol and any range between any two values, more preferably 0.7-1.2 mol.

[0035] Preferably, the dispersant is selected from at least one of citric acid, diethanol and ethylenediaminetetraacetic acid, more preferably citric acid and ethylenediaminetetraacetic acid. Preferably, the molar ratio of citric acid to ethylenediaminetetraacetic acid is 1-2:1.

[0036] Preferably, compared to 1 mol of lanthanum, the amount of the dispersant used is 1.5-5 mol, for example, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5 mol and any range between any two values, more preferably 2-4 mol.

[0037] Preferably, the solvent is water. The amount of the solvent is not particularly limited, and preferably the La content in the mixed solution is 0.1-1.5 mol / L, for example, 0.1, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5 mol and any range between any two values.

[0038] In step (1), the noble metal precursor, the rare earth metal precursor, the auxiliary metal precursor, the dispersant and the solvent are mixed. The mixing method is not particularly limited. The noble metal precursor, the rare earth metal precursor, the auxiliary metal precursor and the dispersant can be dissolved in the solvent and then mixed. The metal precursor can also be dissolved to prepare a metal mixed solution, and then mixed with the dispersant solution, as long as the materials can be mixed uniformly. During the mixing process, stirring, ultrasound and other operations can be performed.

[0039] Ammonia water is added to the mixed material to adjust the pH of the material to 6-9, for example, it can be 6, 6.5, 7, 7.5, 8, 8.5, 9 and any range between any two values. The ammonia water added in this process can be commercially available ammonia water (the concentration can be 10-15 mol / L).

[0040] Preferably, in step (1), the reaction comprises stirring at 60-100° C. (e.g., 60, 70, 80, 90, 100° C. and any range between any two values) until evaporated to dryness. This process can be carried out in a water bath, and the evaporation can be performed until the rotor cannot rotate.

[0041] Preferably, in step (1), the drying conditions include: a drying temperature of 80-140°C (for example, 80, 90, 100, 110, 120, 130, 140°C and any range between any two values), and a drying time of 4-12h (for example, 4, 6, 8, 10, 12h and any range between any two values).

[0042] The drying may be vacuum drying, and the vacuum degree may be below 0.1 MPa.

[0043] Preferably, in step (1), the calcination is performed in two steps, more preferably comprising: in the first stage, the temperature is raised to 250-350°C (for example, 250, 260, 280, 300, 320, 340, 350°C and any range between any two values) at a rate of 3-8°C / min (for example, 3, 4, 5, 6, 7, 8°C / min and any range between any two values), and maintained for 0.5-3 hours (for example, 0.5, 1, 2, 3 hours); in the second stage, the temperature is continuously raised to 600-800°C (for example, 600, 650, 700, 750, 800°C and any range between any two values) at a rate of 3-8°C / min (for example, 3, 4, 5, 6, 7, 8°C / min and any range between any two values), and maintained for 1-6 hours (for example, 1, 2, 3, 4, 5, 6 hours and any range between any two values).

[0044] In step (2), the copper precursor, the alkali metal precursor and the perovskite composite metal oxide are mixed and the pH is adjusted to 8-12, for example, 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5, 12 and any range between any two values, more preferably 9.5-10, and then a binder and a matrix source are added, mixed and ground to obtain a catalyst slurry. It should be understood that a solvent is also added during the process to facilitate mixing and grinding.

[0045] Preferably, the copper precursor is copper nitrate.

[0046] Preferably, compared to 1 mol of lanthanum, the amount of copper used is 0.01-0.4 mol, for example, it can be 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4 mol and any range between any two values, more preferably 0.03-0.1 mol.

[0047] Preferably, the alkali metal is selected from at least one of sodium, potassium and rubidium. The alkali metal precursor may be, for example, sodium nitrate, potassium nitrate and rubidium nitrate.

[0048] Preferably, compared to 1 mol of lanthanum, the amount of alkali metal used is 0.01-0.1 mol, for example, it can be 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1 mol and any range between any two values, more preferably 0.02-0.05 mol.

[0049] Preferably, in step (2), the pH is adjusted to 8-12 using an alkaline solution. The alkaline solution may be selected from at least one of aqueous ammonia, sodium hydroxide, potassium hydroxide, sodium carbonate and potassium carbonate, preferably aqueous ammonia, and its concentration is not particularly limited.

[0050] Preferably, the binder is silica sol.

[0051] Preferably, compared to 1 mol of lanthanum, the amount of binder used is 0.1-2 mol, for example, it can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2 mol and any range between any two values, more preferably 0.5-1.2 mol.

[0052] The molar amount of the silica sol is calculated on a dry basis of silicon dioxide.

[0053] Preferably, the matrix source is a substance that can be converted into a matrix under calcination conditions, and the matrix is ​​selected from at least one of alumina, spinel, perovskite, silica-alumina, zeolite, kaolin, diatomaceous earth and perlite, preferably selected from at least one of alumina, spinel and perovskite, and further preferably alumina.

[0054] Preferably, the amount of the matrix source used is 200-500 g, more preferably 250-450 g, relative to 1 mol of lanthanum.

[0055] Preferably, the solid content of the catalyst slurry is 5-35% by weight, for example, it can be 5, 10, 15, 20, 25, 30, 35% by weight and any range between any two values.

[0056] The grinding method is preferably ball milling; preferably, the ball milling time is 1-5 hours, and the rotation speed is 500-1500 rpm. A vibration ball mill (such as the GZM-6 vibration ball mill of Tianjin Shengyuan Equipment Company) can be used for ball milling.

[0057] Preferably, in step (2), the grinding conditions are such that the average diameter of particles in the catalyst slurry is less than 15 μm, preferably 2-11 μm, for example, 2, 4, 6, 8, 10, 11 μm and any range between any two values.

[0058] The average diameter of the particles in the catalyst slurry is the equivalent volume diameter obtained by laser particle size method. Test instrument: Malvern Mastersizer 3000.

[0059] Preferably, the method further comprises: adding a germanium precursor in step (1) and / or step (2). For example, when adding in step (1), the germanium precursor may be added when the noble metal precursor, the rare earth metal precursor, the auxiliary metal precursor, the dispersant and the solvent are mixed; when adding in step (2), the germanium precursor may be added when the copper precursor, the alkali metal precursor and the perovskite composite metal oxide are mixed.

[0060] Preferably, the method further comprises: adding a germanium precursor in step (2).

[0061] Preferably, the precursor of germanium is a soluble salt of germanium, more preferably germanium nitrate.

[0062] Preferably, compared to 1 mol of lanthanum, the amount of germanium used is 0.001-0.1 mol, for example, it can be 0.001, 0.005, 0.01, 0.02, 0.04, 0.06, 0.08, 0.1 mol and any range between any two values, preferably 0.01-0.05 mol.

[0063] In the present invention, the stability and catalytic performance of the catalyst can be further improved under preferred conditions.

[0064] A second aspect of the present invention provides a catalyst slurry prepared according to the method described above.

[0065] The third aspect of the present invention provides a method for preparing a VOCs catalytic oxidation catalyst, which comprises loading the catalyst slurry as described above onto a carrier, and then performing drying and calcining treatment to obtain a VOCs catalytic oxidation catalyst.

[0066] Preferably, the catalyst slurry loading is such that based on the volume of the carrier, the loading amount of the catalyst layer is 20-140 g / L, for example, it can be 20, 40, 60, 80, 100, 120, 140 g / L and any range between any two values, more preferably 30-100 g / L.

[0067] Preferably, the drying conditions include: a temperature of 80-140°C (for example, 80, 90, 100, 110, 120, 130, 140°C and any range between any two values), and a time of 0.5-4h (for example, 0.5, 1, 2, 3, 4h and any range between any two values).

[0068] Preferably, the calcination conditions include: a calcination temperature of 250-550°C (e.g., 250, 280, 300, 350, 400, 450, 500, 550°C and any range between any two values), and a calcination time of 1-3h (e.g., 1, 1.5, 2, 2.5, 3h and any range between any two values). For example, the temperature may be raised to 250-550°C at a rate of 3-10°C / min (e.g., 3, 4, 6, 8, 10°C / min and any range between any two values) and maintained for 1-3h.

[0069] In the present invention, unless otherwise specified, calcination can be carried out under conventional conditions, that is, in an air atmosphere.

[0070] Preferably, the amount of each component is such that the loading amount of the perovskite composite metal oxide is 10-50 g / L, such as 10, 15, 20, 25, 30, 35, 40, 45, 50 g / L and any range between any two values, more preferably 18-35 g / L, and the loading amount of copper oxide is 0.1-4 g / L, such as 0.1, 0.2, 0.4, 0.6, 0.8, 1, 1.5, 2, 2.5, 3, 3.5, 4 g / L and any range between any two values, more preferably The loading amount of the alkali metal oxide is 0.05-0.5g / L, for example, it can be 0.05, 0.1, 0.15, 0.2, 025, 0.3, 0.35, 0.4, 0.45, 0.5g / L and any range between any two values, more preferably 0.1-0.3g / L; the loading amount of the matrix is ​​18-110g / L, for example, it can be 18, 20, 40, 60, 80, 100, 110g / L and any range between any two values, more preferably 30-70g / L.

[0071] Preferably, the amount of each component is such that the loading amount of the noble metal is 0.01-2 g / L, based on the volume of the carrier, in terms of the metal element, for example, 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.2, 1.4, 1.6, 1.8, 2 g / L and any range between any two values, more preferably 0.1-1 g / L; the loading amount of lanthanum is 6-28 g / L, for example, 6, 10, 15, 20, 25, 28 g / L and any range between any two values. The loading amount of yttrium and / or praseodymium is 0.01-1.1 g / L, for example, it can be 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1 g / L and any range between any two values, more preferably 0.1-0.65 g / L; the loading amount of the auxiliary metal is 2-11 g / L, for example, it can be 2, 3, 4, 5, 6, 7, 8, 9, 10 g / L and any range between any two values, more preferably 3-8 g / L.

[0072] Preferably, the amount of each component used is such that the germanium loading as the metal element is 0.05-1.5 g / L based on the volume of the carrier, for example, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.2, 1.4, 15 g / L and any range between any two values, more preferably 0.1-0.7 g / L.

[0073] The present invention has a wide range of choices for the carrier, and can be various carriers commonly used in the art, and the present invention has no particular limitation on this. For example, the carrier can be an inorganic oxide carrier. Preferably, the carrier is selected from at least one of cordierite, mullite, diamond, corundum, zirconium corundum, quartz, nepheline, feldspar, alumina and metal alloys.

[0074] Preferably, the carrier is a regular structure carrier, that is, the appearance of the carrier is a regular structure, which is easy to assemble, and the pore structure of the carrier can also be regular.

[0075] Preferably, the pore density of the cross section of the regular structure carrier is 50-400 pores / square inch, for example, it can be 50, 100, 150, 200, 250, 300, 350, 400 pores / square inch and any range between any two values.

[0076] Preferably, the cross-sectional area of ​​each hole in the carrier is 0.4-10 square millimeters, preferably 0.4-4 square millimeters.

[0077] Preferably, the open porosity of the carrier surface is 20-80%, more preferably 50-80%.

[0078] The holes may be of regular or irregular shapes, and the shapes of the holes may be the same or different, and each hole may be independently in the shape of a square, a regular triangle, a regular hexagon, a circle, or a corrugated shape.

[0079] The carrier of the present invention can be used for the catalyst bed provided in the fixed bed reactor. The carrier can be a whole carrier block, with a hollow channel structure formed inside, a catalyst layer can be distributed on the inner wall and / or outer wall of the channel, and the channel space can be used as a flow space for the fluid. The carrier can be a regular carrier with honeycomb openings in the cross section (referred to as a honeycomb carrier).

[0080] In the present invention, the catalyst slurry can be evenly loaded on the surface of the carrier by spraying, coating or immersion, and then dried and calcined to obtain a carrier with catalyst layers loaded on the inner and outer surfaces. For example, the carrier can be immersed in the catalyst slurry for 5-30 seconds for loading.

[0081] It should be understood that in the present invention, the preferred conditions can be more conducive to improving the performance of the catalyst, reducing the catalytic temperature, and improving the catalytic effect.

[0082] A fourth aspect of the present invention provides a VOCs catalytic oxidation catalyst prepared according to the method described above.

[0083] A fifth aspect of the present invention provides a VOCs catalytic oxidation catalyst, the VOCs catalytic oxidation catalyst comprising a carrier and a catalyst layer supported on the carrier;

[0084] Wherein, the catalyst layer comprises active components and a matrix;

[0085] The active components include perovskite composite metal oxides, copper oxide, and alkali metal oxides; the perovskite composite metal oxides contain noble metals, rare earth metal oxides, and auxiliary metal oxides; and the auxiliary metals are transition metals other than noble metals, rare earth metals, and Cu.

[0086] The structural formula of the perovskite composite metal oxide is ABO3, wherein A is a rare earth metal, and B is an auxiliary metal and a noble metal. It should be understood that ABO3 does not mean that the molar ratio of A, B and O is strictly 1:1:3, and the formation of the perovskite structure has anion and cation defects, so that the ratio deviates from the standard stoichiometric ratio. The noble metal can be in a single substance state or an oxide state.

[0087] Preferably, the active component further comprises germanium, which exists in the form of oxide.

[0088] Preferably, based on the volume of the carrier, the loading amount of the catalyst layer is 20-140 g / L, for example, it can be 20, 40, 60, 80, 100, 120, 140 g / L and any range between any two values, more preferably 30-100 g / L.

[0089] Preferably, based on the volume of the carrier, the loading amount of the perovskite composite metal oxide is 10-50 g / L, such as 10, 15, 20, 25, 30, 35, 40, 45, 50 g / L and any range between any two values, more preferably 18-35 g / L, and the loading amount of copper oxide is 0.1-4 g / L, such as 0.1, 0.2, 0.4, 0.6, 0.8, 1, 1.5, 2, 2.5, 3, 3.5, 4 g / L and any range between any two values, more preferably 0. 3-1g / L; the loading amount of the alkali metal oxide is 0.05-0.5g / L, for example, it can be 0.05, 0.1, 0.15, 0.2, 025, 0.3, 0.35, 0.4, 0.45, 0.5g / L and any range between any two values, more preferably 0.1-0.3g / L; the loading amount of the matrix is ​​18-110g / L, for example, it can be 18, 20, 40, 60, 80, 100, 110g / L and any range between any two values, more preferably 30-70g / L.

[0090] Preferably, the amount of each component is such that the loading amount of the noble metal is 0.01-2 g / L, based on the volume of the carrier, in terms of the metal element, for example, 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.2, 1.4, 1.6, 1.8, 2 g / L and any range between any two values, more preferably 0.1-1 g / L; the loading amount of lanthanum is 6-28 g / L, for example, 6, 10, 15, 20, 25, 28 g / L and any range between any two values. The loading amount of yttrium and / or praseodymium is 0.01-1.1 g / L, for example, it can be 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1 g / L and any range between any two values, more preferably 0.1-0.65 g / L; the loading amount of the auxiliary metal is 2-11 g / L, for example, it can be 2, 3, 4, 5, 6, 7, 8, 9, 10 g / L and any range between any two values, more preferably 3-8 g / L.

[0091] Preferably, the amount of each component used is such that the germanium loading as the metal element is 0.05-1.5 g / L based on the volume of the carrier, for example, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.2, 1.4, 15 g / L and any range between any two values, more preferably 0.1-0.7 g / L.

[0092] For the description of the carrier, matrix and various metal types, please refer to the first and third aspects and will not be repeated here.

[0093] A sixth aspect of the present invention provides use of the catalyst slurry as described above or the VOCs catalytic oxidation catalyst as described above in catalytic oxidation of VOCs.

[0094] The present invention will be described in detail below by way of examples. The following examples will further illustrate the present invention, but are not intended to limit the present invention.

[0095] The average diameter of the particles in the catalyst slurry is the equivalent volume diameter obtained by laser particle size method. Test instrument: Malvern Mastersizer 3000.

[0096] The activity evaluation of the catalytic oxidation reaction of toluene, propylene and propane was completed on a micro fixed bed reactor designed and manufactured by Tianjin Pengxiang Technology Co., Ltd., equipped with a Multigas 2030 infrared detector from MKS. The reaction was carried out under normal pressure, with an initial temperature of 150°C and a temperature program of 3°C / min until the VOCs pollutants were completely converted. The inlet gas composition was 450ppmC7H8 / 7% O2 / N2, and the air velocity was 12000h -1 .

[0097] The carrier is a VOC-specific cordierite honeycomb carrier purchased from Pingxiang Guanlin Environmental Protection Technology Co., Ltd. The carrier hole density is 300 holes / square inch, the cross-sectional area of ​​each hole is 1.5 square millimeters, the open porosity is 70%, and the hole shape is circular.

[0098] The pH of the silica sol used was about 9 and the solid content was 15%.

[0099] Example 1

[0100] (1) preparing 1L of a mixed solution containing 0.02mol / L palladium nitrate, 1mol / L lanthanum nitrate, 0.03mol / L yttrium nitrate and 0.98mol / L cobalt nitrate, and then preparing a mixed solution containing 1.5mol / L citric acid and 1mol / L ethylenediaminetetraacetic acid, and rapidly mixing the two solutions in a ratio of 1:1 under stirring conditions, and then adding ammonia water to adjust the pH of the material to 8, and evaporating to dryness in a water bath at 80°C under stirring conditions, and then drying at 100°C for 8h under a vacuum degree of 0.1Mpa, to obtain a foamed composite metal oxide precursor, taking out the sample, placing it in a muffle furnace, heating it to 300°C at a rate of 5°C / min, and maintaining it for 2h, and then continuing to heat it to 700°C at a rate of 5°C / min, and maintaining it for 4h, to obtain a perovskite composite metal oxide;

[0101] like Figure 1 As shown in the XRD spectrum, after calcination, a perovskite composite oxide diffraction peak is formed, indicating that a perovskite crystal phase structure is formed, and there is no noble metal diffraction peak, indicating that the noble metal active centers in the fresh catalyst are highly dispersed. Figure 2 As shown, the EXAFS spectrum of the perovskite composite metal oxide after hydrothermal aging treatment has no obvious palladium-palladium coordination shell, indicating that the precious metal palladium did not agglomerate in the form of oxide particles after hydrothermal aging treatment, but still exists in a highly dispersed form in the perovskite lattice.

[0102] (2) 0.04 mol of germanium nitrate, 0.07 mol of copper nitrate, 0.03 mol of potassium nitrate and the perovskite composite metal oxide prepared in step (1) were mixed, and an appropriate amount of ammonia water was added to adjust the pH to 10, and 0.12 mol of silica sol (molar amount on a dry basis) and 400 g of alumina powder were added and stirred for 2 h. The mixed solution was fully ground using a vibrating ball mill (Tianjin Shengyuan Equipment Co., Ltd., GZM-6). The specific grinding conditions were: ball milling time of 2.5 h, rotation speed of 1000 rpm, and an average particle diameter of 10.3 μm in the mixed solution after ball milling; the solid content of the slurry was controlled to be 18% by weight to obtain a catalyst slurry.

[0103] (3) The catalyst slurry was evenly coated on the surface of a 300-mesh regular structure carrier, so that the total coating amount on each liter of the ceramic carrier was 70 g.

[0104] The carrier coated with the catalyst slurry was dried at 140° C. for 2 h, and then calcined, and the temperature was increased to 400° C. at a rate of 5° C. / min and maintained for 2 hours to obtain a VOCs catalytic oxidation catalyst.

[0105] Example 2

[0106] (1) preparing 1L of a mixed solution containing 0.02mol / L platinum nitrate solution, 1mol / L lanthanum nitrate, 0.03mol / L yttrium nitrate and 0.98mol / L cobalt nitrate, and then preparing a mixed solution containing 1.5mol / L citric acid and 1mol / L ethylenediaminetetraacetic acid, and rapidly mixing the two solutions in a ratio of 1:1 under stirring conditions, adding ammonia water to adjust the pH of the material to 8, evaporating the mixture in a water bath at 85°C under stirring conditions, and then drying the mixture at a vacuum degree of 0.05Mpa and 120°C for 6h to obtain a foamed composite metal oxide precursor, taking out the sample, placing it in a muffle furnace, heating it to 300°C at a rate of 5°C / min, and maintaining it for 1.5 hours, and then continuing to heat it to 700°C at a rate of 5°C / min, and maintaining it for 3h, to obtain a perovskite composite metal oxide;

[0107] (2) 0.04 mol of germanium nitrate, 0.07 mol and 0.03 mol of potassium nitrate and the perovskite composite metal oxide prepared in step (1) are mixed, an appropriate amount of ammonia water is added to adjust the pH to 10, 0.12 mol of silica sol (on a dry basis) and 400 g of alumina powder are added, and the mixture is stirred for 2 h at a speed of 900 rpm. After ball milling, the average particle diameter of the mixed solution is 9.5 μm; the solid content of the slurry is controlled to be 20% by weight to obtain a catalyst slurry.

[0108] (3) The catalyst slurry was evenly coated on the surface of a 300-mesh regular structure carrier, so that the total coating amount on each liter of the ceramic carrier was 70 g.

[0109] The carrier coated with the catalyst slurry was dried at 140° C. for 2 h, and then calcined, and the temperature was increased to 400° C. at a rate of 5° C. / min and maintained for 2 hours to obtain a VOCs catalytic oxidation catalyst.

[0110] Example 3

[0111] (1) preparing 1L of a mixed solution containing 0.02mol / L platinum nitrate solution, 1mol / L lanthanum nitrate, 0.05mol / L yttrium nitrate and 0.99mol / L cobalt nitrate, and then preparing a mixed solution containing 1.5mol / L citric acid and 1mol / L ethylenediaminetetraacetic acid, and rapidly mixing the two solutions in a ratio of 1:1 under stirring conditions, adding ammonia water to adjust the pH of the material to 8, evaporating the mixture in a water bath at 85°C under stirring conditions, and then drying the mixture at a vacuum degree of 0.05Mpa and 120°C for 6h to obtain a foamed composite metal oxide precursor, taking out the sample, placing it in a muffle furnace, heating it to 300°C at a rate of 5°C / min, and maintaining it for 1.5 hours, and then continuing to heat it to 700°C at a rate of 5°C / min, and maintaining it for 3h, to obtain a perovskite composite metal oxide;

[0112] (2) 0.04 mol of germanium nitrate, 0.05 mol and 0.025 mol of potassium nitrate and the perovskite composite metal oxide prepared in step (1) are mixed, an appropriate amount of ammonia water is added to adjust the pH to 10, 0.1 mol of silica sol (on a dry basis) and 400 g of alumina powder are added, and the mixture is stirred for 2 h at a speed of 900 rpm. After ball milling, the average particle diameter of the mixed solution is 9.9 μm; the solid content of the slurry is controlled to be 15% by weight to obtain a catalyst slurry.

[0113] (3) The catalyst slurry was evenly coated on the surface of a 300-mesh regular structure carrier, so that the total coating amount on each liter of the ceramic carrier was 70 g.

[0114] The carrier coated with the catalyst slurry was dried at 140° C. for 2 h, and then calcined, and the temperature was increased to 400° C. at a rate of 5° C. / min and maintained for 2 hours to obtain a VOCs catalytic oxidation catalyst.

[0115] Example 4

[0116] In step (1), 2.5 mol / L ethylene glycol was used as the dispersant, and other conditions were the same as those in Example 1.

[0117] Example 5

[0118] Germanium nitrate is added in step (1), specifically, 1 L of a mixed solution containing 0.04 mol / L germanium nitrate, 0.02 mol / L palladium nitrate, 1 mol / L lanthanum nitrate, 0.03 mol / L yttrium nitrate and 0.98 mol / L cobalt nitrate is prepared, and then a mixed solution containing 1.5 mol / L citric acid and 1 mol / L ethylenediaminetetraacetic acid is prepared, and the two solutions are quickly mixed in a ratio of 1:1 under stirring conditions, and other conditions are the same as those in Example 1.

[0119] Example 6

[0120] In step (2), germanium nitrate was not added, and other conditions were the same as those in Example 1.

[0121] Example 7

[0122] In step (1), the pH was adjusted to 6, and the other conditions were the same as in Example 1.

[0123] Example 8

[0124] In step (1), the pH was adjusted to 7, and the other conditions were the same as in Example 1.

[0125] Example 9

[0126] In step (2), the pH was adjusted to 9, and other conditions were the same as in Example 1.

[0127] Example 10

[0128] In step (1), the pH was adjusted to 11, and the other conditions were the same as in Example 1.

[0129] Comparative Example 1

[0130] In step (2), no copper precursor salt is added, and other conditions are the same as those in Example 1.

[0131] Comparative Example 2

[0132] In step (2), no alkali metal precursor salt is added, and other conditions are the same as those in Example 1.

[0133] Comparative Example 3

[0134] In step (1), only a single-stage calcination is used, the temperature is raised to 350° C. at a rate of 5° C. / min and maintained for 2 hours, and no perovskite composite oxide crystal structure is formed. Other conditions are the same as in Example 1.

[0135] The performance of the VOCs catalytic oxidation materials obtained in the examples and comparative examples was evaluated using propylene, toluene and propane as model compounds. 99 The conversion temperatures are shown in Table 1.

[0136] The catalysts prepared in the examples and comparative examples were tested for catalyst aging performance. 99 The results of the conversion temperatures are shown in Table 1.

[0137] The catalyst aging conditions are: air atmosphere, containing 10% water vapor, temperature 800°C, 10h.

[0138] Table 1 T of fresh and hydrothermally aged catalyst samples 99

[0139]

[0140]

[0141] As can be seen from Table 1, the T 99 The conversion temperatures of propylene, toluene and propane are all lower than those of the comparative examples, and the catalyst stability in the aging performance test is better than that of the comparative examples. The VOCs catalytic material prepared by the present invention has a higher pollutant degradation efficiency and is expected to be extended to the preparation of various fixed bed catalytic materials, and has broad application prospects.

[0142] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing a catalyst slurry, characterized in that: The method includes: (1) mixing a noble metal precursor, a rare earth metal precursor, an auxiliary metal precursor, a dispersant and a solvent, then adding ammonia water to adjust the pH of the material to 6-9, and reacting, and drying and calcining after the reaction to obtain a perovskite composite metal oxide; (2) mixing a copper precursor, an alkali metal precursor and the perovskite composite metal oxide and adjusting the pH to 8-12, then adding a binder and a matrix source, mixing and grinding to obtain a catalyst slurry; The additive metal is a transition metal other than precious metals, rare earth metals and Cu.

2. The method according to claim 1, wherein: The noble metal is at least one selected from platinum, palladium and rhodium; and / or The rare earth metal is lanthanum, and yttrium and / or praseodymium; and / or The additive metal is selected from at least one of nickel, cobalt, manganese and iron; and / or The dispersant is selected from at least one of citric acid, diethanol and ethylenediaminetetraacetic acid, preferably citric acid and ethylenediaminetetraacetic acid; and / or The solvent is water; and / or The alkali metal is at least one selected from sodium, potassium and rubidium; and / or The binder is silica sol; and / or The matrix source is a substance that can be converted into a matrix under calcination conditions, and the matrix is ​​selected from at least one of alumina, spinel, perovskite, silica-alumina, zeolite, kaolin, diatomaceous earth and perlite, preferably selected from at least one of alumina, spinel and perovskite, and more preferably alumina; Preferably, the metal precursors are each independently a soluble salt thereof, more preferably a nitrate thereof.

3. The method according to claim 2, wherein: Compared to 1 mol of lanthanum, the amount of precious metal is 0.001-0.1 mol, preferably 0.01-0.06 mol; the amount of yttrium and / or praseodymium is 0.01-0.1 mol, preferably 0.02-0.05 mol; the amount of auxiliary metal is 0.5-1.5 mol, preferably 0.7-1.2 mol; the amount of dispersant is 1.5-5 mol, preferably 2-4 mol; the amount of copper is 0.01-0.4 mol, preferably 0.03-0.1 mol; the amount of alkali metal is 0.01-0.1 mol, more preferably 0.02-0.05 mol; the amount of binder is 0.1-2 mol, preferably 0.5-1.2 mol; and / or Compared to 1 mol of lanthanum, the amount of the matrix source is 200-500 g, preferably 250-450 g; and / or The solid content of the catalyst slurry is 5-35% by weight.

4. The method according to claim 1, wherein: In step (1), the reaction method includes stirring at 60-100° C. until evaporated to dryness; and / or The drying conditions include: drying temperature of 80-140°C, vacuum degree of less than 0.1 MPa, and drying time of 4-12 hours; and / or The calcination method is a two-step calcination, preferably including: in the first stage, the temperature is increased to 250-350°C at a rate of 3-8°C / min and maintained for 0.5-3 hours; in the second stage, the temperature is further increased to 600-800°C at a rate of 3-8°C / min and maintained for 1-6 hours.

5. The method according to claim 1, wherein: In step (2), the pH is adjusted to 8-12 using an alkaline solution, wherein the alkaline solution is selected from at least one of aqueous ammonia, sodium hydroxide, potassium hydroxide, sodium carbonate and potassium carbonate; and / or In step (2), the grinding conditions are such that the average diameter of particles in the catalyst slurry is less than 15 μm, preferably 2-11 μm.

6. The method according to any one of claims 1 to 5, wherein: The method further comprises: adding a germanium precursor in step (1) and / or step (2); Preferably, the precursor of germanium is a soluble salt of germanium, more preferably germanium nitrate; Preferably, compared to 1 mol of lanthanum, the amount of germanium used is 0.001-0.1 mol, preferably 0.01-0.05 mol.

7. The catalyst slurry prepared according to the method according to any one of claims 1 to 6.

8. A method for preparing a VOCs catalytic oxidation catalyst, characterized in that: The method comprises loading the catalyst slurry according to claim 7 onto a carrier, and then drying and calcining the carrier to obtain a VOCs catalytic oxidation catalyst; Preferably, the catalyst slurry loading is such that the loading of the catalyst layer is 20-140 g / L, more preferably 30-100 g / L, based on the volume of the carrier; Preferably, the drying conditions include: temperature of 80-140°C and time of 0.5-4h; Preferably, the calcination conditions include: a calcination temperature of 250-550° C. and a calcination time of 1-3 h.

9. The method according to claim 8, wherein: The carrier is a regular structure carrier, Preferably, the cross-section of the carrier has a pore density of 50-400 pores / square inch and an open porosity of 20-80%; Preferably, the carrier is selected from at least one of cordierite, mullite, diamond, corundum, zirconium corundum, quartz, nepheline, feldspar, alumina and metal alloys.

10. The VOCs catalytic oxidation catalyst prepared according to the method of claim 8 or 9.

11. A VOCs catalytic oxidation catalyst, characterized in that: The VOCs catalytic oxidation catalyst comprises a carrier and a catalyst layer supported on the carrier; Wherein, the catalyst layer comprises active components and a matrix; The active components include perovskite composite metal oxides, copper oxide, and alkali metal oxides; the perovskite composite metal oxides contain noble metals, rare earth metal oxides, and auxiliary metal oxides; the auxiliary metals are transition metals other than noble metals, rare earth metals, and Cu; Preferably, the active component further comprises germanium; Preferably, based on the volume of the carrier, the loading amount of the catalyst layer is 20-140 g / L, more preferably 30-100 g / L; Preferably, based on the volume of the carrier, the loading amount of the perovskite composite metal oxide is 10-50 g / L, more preferably 18-35 g / L, the loading amount of the copper oxide is 0.1-4 g / L, more preferably 0.3-1 g / L; the loading amount of the alkali metal oxide is 0.05-0.5 g / L, more preferably 0.1-0.3 g / L; the loading amount of the matrix is ​​18-110 g / L, more preferably 30-70 g / L; Preferably, the amount of each component is such that, based on the volume of the carrier, the loading amount of the noble metal is 0.01-2 g / L, more preferably 0.1-1 g / L, the loading amount of lanthanum is 6-28 g / L, more preferably 10-20 g / L, the loading amount of yttrium and / or praseodymium is 0.01-1.1 g / L, more preferably 0.1-0.65 g / L, and the loading amount of the auxiliary metal is 2-11 g / L, more preferably 3-8 g / L. Preferably, the amount of each component used is such that the germanium loading amount calculated as metal element is 0.05-1.5 g / L, more preferably 0.1-0.7 g / L, based on the volume of the carrier.

12. The VOCs catalytic oxidation catalyst according to claim 11, wherein: The carrier is a regular structure carrier, preferably, the pore density of the cross section of the carrier is 50-400 pores / square inch, and the open porosity is 20-80%; preferably, the carrier is selected from at least one of cordierite, mullite, diamond, corundum, zirconium corundum, quartz, nepheline, feldspar, alumina and metal alloy; and / or The matrix is ​​selected from at least one of alumina, spinel, perovskite, silica-alumina, zeolite, kaolin, diatomaceous earth and perlite, preferably selected from at least one of alumina, spinel and perovskite, more preferably alumina; and / or The noble metal is at least one selected from platinum, palladium and rhodium; and / or The rare earth metal is lanthanum, and yttrium and / or praseodymium; and / or The additive metal is selected from at least one of nickel, cobalt, manganese and iron; and / or The alkali metal is at least one selected from the group consisting of sodium, potassium and rubidium.

13. Use of the catalyst slurry according to claim 7 or the VOCs catalytic oxidation catalyst according to claim 11 or 12 in catalytic oxidation of VOCs.

Citation Information

Patent Citations

  • Catalyst used for treating benzene substances in industrial waste gas and preparation method of catalyst

    CN106890642A

  • Precious metal low-load catalyst for VOCs (volatile organic chemicals) catalytic combustion and preparation method

    CN107913719A

  • Catalyst for catalytic combustion of VOCs and preparation method thereof

    CN110614101A

  • Treatment method of incompletely regenerated flue gas

    CN111346502A

  • Precious metal-rare earth perovskite type monolithic three-way catalyst and preparation method thereof

    CN111672519A

Cited By

  • Cobalt-nickel catalyst for low-temperature catalytic degradation of VOCs and preparation method of cobalt-nickel catalyst

    CN119680547A

  • A cobalt-nickel catalyst for catalytic degradation of VOCs at low temperature and a preparation method thereof

    CN119680547B

  • Preparation method of high-temperature-resistant high-space-velocity VOCs catalytic combustion catalyst for acid ester waste gas and catalyst

    CN120714656A