Corrosion-resistant cation ultraviolet curing coating and preparation method thereof

By combining a nano-container loaded with corrosion inhibitors in a cationic UV-curable coating with epoxy resin, the synergistic effect of rare earth oxides and rare earth metal salts is utilized to solve the problem of insufficient anti-corrosion performance of cationic UV-curable coatings, achieving a highly efficient anti-corrosion effect, and making it suitable for metal material surfaces in various environments.

CN118931316APending Publication Date: 2024-11-12NANTONG UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411173139.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing cationic UV-curable coatings have shortcomings in corrosion resistance. Traditional doping with corrosion inhibitors leads to deactivation and coating failure. Furthermore, existing nanotechnology-modified coatings have limited corrosion resistance or are costly.

Method used

A corrosion-resistant cationic UV-curable coating is prepared by combining a nano-container loaded with corrosion inhibitors with epoxy resin, and by allowing the nano-container to release the corrosion inhibitors under external stimuli. Rare earth oxides and rare earth metal salts are used as corrosion inhibitors. The nano-container includes SiO2 microcapsules, mesoporous TiO2 nanoparticles, etc., which synergistically improve the anti-corrosion effect.

Benefits of technology

It significantly improves the corrosion resistance of coatings, has a simple formulation, is suitable for metal material surfaces in various environments, and has good weather resistance and low cost advantages.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005009913320000061
    Figure BDA0005009913320000061
Patent Text Reader

Abstract

The invention discloses a corrosion-resistant cation ultraviolet curing coating and a preparation method thereof, and the corrosion-resistant cation ultraviolet curing coating comprises the following components in parts by weight: 80-90 parts of epoxy resin, 5-15 parts of a solvent, 3-8 parts of a photoinitiator, 1-4 parts of a corrosion inhibitor loaded nano container and 1-7 parts of an auxiliary agent. The corrosion inhibitor comprises one or a combination of two of a rare earth oxide, a rare earth metal salt and a rare earth hydroxide. Wherein the epoxy resin is bisphenol A epoxy resin. The nano container and the corrosion inhibitor have a certain anti-corrosion effect, the nano container loaded with the corrosion inhibitor is prepared, the nano container and the corrosion inhibitor have a synergistic effect, and the anti-corrosion effect can be greatly improved. According to the scheme, the formula is simple, the anti-corrosion effect is good, and the cation ultraviolet curing anti-corrosion coating can be widely applied to the surfaces of metal materials in various environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of substrate coatings, and specifically relates to a corrosion-resistant cationic ultraviolet light-curing coating and a preparation method thereof. Background Art

[0002] In recent years, cationic UV-curing coatings have also shown great promise in the development of protective coatings for metal substrates. However, cationic UV-curing coatings also have the problem of insufficient anti-corrosion performance. Traditionally, corrosion inhibitors are usually directly doped into the coating, but direct addition has some defects, which not only leads to the inactivation of the corrosion inhibitor, but also causes the coating to fail. Therefore, a technology based on loading corrosion inhibitors in nanocontainers and self-releasing them under appropriate external stimuli is regarded as a very promising anti-corrosion measure. Epoxy resin has the advantages of controllable cross-linking degree and wide curing temperature. More importantly, epoxy resin has good adhesion on the metal surface, which has become a guarantee for its high efficiency in anti-corrosion. Epoxy coatings are used for metal protection because they can act as a barrier between the metal substrate and the corrosive medium, and the complete coating has a good barrier effect on corrosive ions and water molecules.

[0003] Among various methods of preventing corrosion, the use of corrosion inhibitors is one of the cheapest and most effective methods. Rare earth metal salts and rare earth oxides, such as cerium oxide or lanthanum chloride, are more environmentally friendly and have been shown to be good corrosion inhibitors that work by reducing cathode redox reactions. Nano-microsphere materials or two-dimensional nanofillers are used as nano-containers to load nano-rare earth materials. Through the synergistic effect of the two, they are added to cationic UV-curing coatings based on epoxy resins to achieve excellent anti-corrosion properties.

[0004] At present, in order to obtain better anti-corrosion effect, the anti-corrosion performance of nanotechnology modified coatings mainly adopts nanomaterial compounding technology, aiming to obtain better and more lasting anti-corrosion effect through the synergistic effect of nanomaterials.

[0005] For example, the invention patent with announcement number CN105907243B discloses a method for machine preparation of conductive anti-corrosion coating for power grid grounding network. The invention prepares anti-corrosion coating with improved conductivity by compounding graphene and carbon nanotubes, but the anti-corrosion coating prepared by this method has poor mechanical properties; Patent CN 102807774A discloses "a surface modification method for cuprous oxide antifouling agent", and uses chitosan-gum arabic to prepare a chitosan-gum arabic cuprous oxide microcapsule powder, which is added to the antifouling coating as an antifouling agent. Since the surface of the cuprous oxide particles is smooth and the bonding strength between the cuprous oxide and the coating is low, the service life of the coating does not exceed one year. Patent CN114181586B discloses a water-based epoxy electrostatic oil-resistant anticorrosive coating and its preparation method, which uses homemade water-based nano-silver modified epoxy emulsion and water-based modified amine curing agent as base materials, and water-based elastic carbon nanotube composite conductive mica powder as functional conductive filler, which improves the flexibility and conductivity of the coating on the inner wall of the oil tank, but the surface of the paint film has insufficient anti-fouling and anti-waxing performance, and its heat resistance and acid resistance need to be studied. Some of the above technologies have problems such as limited anti-corrosion performance or too high cost, and there is a lack of nano anti-corrosion technology for cationic UV-curing coatings. Summary of the invention

[0006] The present application provides a corrosion-resistant cationic UV-curing coating and a preparation method thereof to solve the above-mentioned technical problems.

[0007] In order to solve the above technical problems, a technical solution adopted in the present application is: a corrosion-resistant cationic UV-curing coating, which is composed of the following components in parts by weight: 80-90 parts of epoxy resin, 5-15 parts of solvent, 3-8 parts of photoinitiator, 1-4 parts of nanocontainer loaded with corrosion inhibitor, and 1-7 parts of additive.

[0008] Furthermore, the epoxy resin is a bisphenol A type epoxy resin, and the epoxy value of the epoxy resin is between 0.3 and 0.6 (eq / 100g).

[0009] Furthermore, the solvent is any one of 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, 3,3'-(oxybismethylene)bis(3-ethyl)oxetane, 1,4-butanediol diglycidyl ether, or neopentyl glycol diglycidyl ether, or a combination of at least two thereof.

[0010] Furthermore, the photoinitiator is one or a combination of triarylsulfonium hexafluoroantimonate, diphenyl-(4-phenylsulfonium)phenylsulfonium hexafluoroantimonate, and triphenylsulfonium hexafluorophosphate.

[0011] Furthermore, the auxiliary agent includes a defoamer and a fluorinated acrylate leveling agent.

[0012] Another technical solution adopted in the present application is: a method for preparing a corrosion-resistant cationic UV-curing coating, comprising the following steps:

[0013] Preparation of a nanocontainer loaded with a corrosion inhibitor: adding a nanocontainer to deionized water with a mass fraction of 5% to 15% and stirring thoroughly, then adding an aqueous solution containing a corrosion inhibitor with a mass fraction of 5% to 15% to the above suspension to prepare a mixed solution, adding the mixed solution to a high-speed ball mill for mixing and dispersion for 2 to 6 hours, filtering and precipitating, and vacuum drying the precipitate at 60 to 80° C. to obtain a nanocontainer loaded with a corrosion inhibitor;

[0014] Preparation of nano-dispersion: Add the nano-container loaded with corrosion inhibitor into the solvent and stir it thoroughly at a speed of 500-800 r / min for 1-3 hours;

[0015] Preparation of cationic UV-curing coating: Add the nano-dispersion into the epoxy resin and stir it thoroughly for 2 to 5 hours at a speed of 200 to 500 r / min. Then add the photoinitiator and the auxiliary agent and continue to stir it thoroughly for 2 to 4 hours at a speed of 200 to 600 r / min.

[0016] Furthermore, the molar ratio of the corrosion inhibitor to the nanocontainer is 0.5 to 5:100.

[0017] Furthermore, the nanocontainer includes one or a combination of two of SiO2 microcapsules, mesoporous TiO2 nanoparticles, layered hydroxides, montmorillonite, zeolite, hydroxyapatite, inorganic hollow spheres, carbon nanotubes, graphene oxide, and hexagonal boron nitride.

[0018] Furthermore, the corrosion inhibitor includes one or a combination of two of rare earth oxides, rare earth metal salts and rare earth hydroxides.

[0019] Furthermore, the rare earth in the rare earth hydroxide is one of lanthanum, cerium, neodymium and yttrium.

[0020] The beneficial effects of the present application are as follows: the nano-container and the corrosion inhibitor in the present application both have certain anti-corrosion effects, and the nano-container loaded with the corrosion inhibitor is prepared, and the two play a synergistic effect, which can greatly improve the anti-corrosion effect. The scheme of the present application has a simple formula and a good anti-corrosion effect, and the cationic ultraviolet light curing anti-corrosion coating can be widely used on the surface of metal materials in various environments. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is further described in detail below in conjunction with specific embodiments.

[0022] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways than those described herein. Therefore, the present invention is not limited to the specific embodiments of the following disclosure.

[0023] The present application provides a corrosion-resistant cationic UV-curing coating, which is composed of the following components by weight: 80 to 90 parts of epoxy resin, 5 to 15 parts of solvent, 3 to 8 parts of photoinitiator, 1 to 4 parts of nanocontainer loaded with corrosion inhibitor, and 1 to 7 parts of auxiliary agent. Among them, the epoxy resin is bisphenol A type epoxy resin, and the epoxy value of the epoxy resin is between 0.3 and 0.6 (eq / 100g). The solvent is any one of 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, 3,3'-(oxybismethylene)bis(3-ethyl)oxetane, 1,4-butanediol diglycidyl ether or neopentyl glycol diglycidyl ether, or a combination of at least two. The photoinitiator is one or two combinations of triarylsulfonium hexafluoroantimonate, diphenyl-(4-phenylsulfur)phenylsulfonium hexafluoroantimonate, and triphenylsulfur hexafluorophosphate. Additives include defoamers and fluorinated acrylate leveling agents.

[0024] The auxiliary agent includes a defoamer and a fluorinated acrylic leveling agent. The defoamer is any one of TEGO Airex920, Deqian 6800 or BYK057 or a combination of at least two thereof.

[0025] The present application provides a method for preparing a corrosion-resistant cationic UV-curing coating, comprising the following steps:

[0026] Preparation of a nanocontainer loaded with a corrosion inhibitor: adding a nanocontainer to deionized water with a mass fraction of 5% to 15% and stirring thoroughly, then adding an aqueous solution containing a corrosion inhibitor with a mass fraction of 5% to 15% to the above suspension to prepare a mixed solution, adding the mixed solution to a high-speed ball mill for mixing and dispersion for 2 to 6 hours, filtering and precipitating, and vacuum drying the precipitate at 60 to 80° C. to obtain a nanocontainer loaded with a corrosion inhibitor;

[0027] Preparation of nano-dispersion: Add the nano-container loaded with corrosion inhibitor into 5-15 parts of solvent, and stir thoroughly for 1-3 hours at a speed of 500-800 r / min;

[0028] Preparation of cationic UV-curing coating: Add the nano-dispersion into 80-90 parts of epoxy resin, stir thoroughly for 2-5 hours at a speed of 200-500 r / min. Then add 3-8 parts of initiator and 1-7 parts of auxiliary agent, and continue to stir thoroughly for 2-4 hours at a speed of 200-600 r / min.

[0029] The molar ratio of the corrosion inhibitor to the nanocontainer is 0.5 to 5:100. The nanocontainer includes SiO2 microcapsules, mesoporous TiO2 nanoparticles, layered hydroxides, montmorillonite, zeolite, hydroxyapatite, inorganic hollow spheres, carbon nanotubes, graphene oxide, hexagonal boron nitride, or a combination of two. The corrosion inhibitor includes a rare earth oxide, a rare earth metal salt, and a rare earth hydroxide, or a combination of two. The rare earth in the rare earth hydroxide is one of lanthanum (La), cerium (Ce), neodymium (Nd), and yttrium (Y).

[0030] Example 1

[0031] SiO2 microcapsules were added to 5% deionized water and stirred thoroughly. Then, an aqueous solution (mass fraction of 10%) containing a corrosion inhibitor, cerium nitrate (Ce(NO3)3), was added to the above suspension to prepare a mixed solution (the molar ratio of the corrosion inhibitor to the nanocontainer was 1:100). The mixed solution was added to a high-speed ball mill for mixing and dispersion for a period of time (3h), filtered and precipitated, and the precipitate was vacuum dried at 60°C to obtain a nanocontainer loaded with a corrosion inhibitor. The prepared nanocontainer loaded with a corrosion inhibitor (2 parts) was added to a 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate solvent (10 parts) and stirred thoroughly for 3h at a speed of 800r / min.

[0032] The nano-dispersion was added to epoxy resin (80-90 parts), and stirred at a speed of 400 r / min for 3 hours. Then, a photoinitiator triarylsulfonium hexafluoroantimonate (5 parts), a TEGO Airex 920 defoamer (1 part) and a fluorinated acrylate leveling agent (1 part) were added, and the mixture was stirred at a speed of 200 / min for 2 hours to obtain a cationic UV-curing coating.

[0033] Example 2

[0034] The layered hydroxide was added to deionized water (mass fraction is 10%) and stirred thoroughly, and then an aqueous solution (mass fraction is 8%) containing corrosion inhibitor lanthanum silicate (La2SiO5) was added to the above suspension to prepare a mixed solution (the molar ratio of corrosion inhibitor to nanocontainer is 2:100), and the mixed solution was added to a high-speed ball mill for mixing and dispersion for a period of time (3h), filtered and precipitated, and the precipitate was vacuum dried at 60°C to obtain a nanocontainer loaded with corrosion inhibitor. The prepared nanocontainer loaded with corrosion inhibitor (2 parts) was added to 3,3'-(oxybismethylene)bis(3-ethyl)oxetane solvent (10 parts) and stirred thoroughly for 3h at a speed of 800r / min. This nanodispersion was added to epoxy resin (80-90 parts) and stirred thoroughly for 3h at a speed of 400r / min. Then, a photoinitiator triarylsulfonium hexafluoroantimonate (5 parts), a Deqian 6800 defoamer (1.5 parts) and a fluorinated acrylate leveling agent (1 part) were added, and the mixture was stirred for 2 hours at a rotation speed of 200 / min to obtain a cationic UV-curing coating.

[0035] Example 3

[0036] Hexagonal boron nitride was added to deionized water (mass fraction was 10%) and stirred thoroughly. Then, an aqueous solution containing corrosion inhibitor cerium oxide (CeO2) (mass fraction was 10%) was added to the above suspension to prepare a mixed solution (the molar ratio of corrosion inhibitor to nanocontainer was 4:100). The mixed solution was added to a high-speed ball mill for mixing and dispersion for a period of time (3h), filtered and precipitated, and the precipitate was vacuum dried at 60°C to obtain a nanocontainer loaded with corrosion inhibitor. The prepared nanocontainer loaded with corrosion inhibitor (2 parts) was added to 3,3'-(oxybismethylene)bis(3-ethyl)oxetane solvent (10 parts) and stirred thoroughly for 3h at a speed of 800r / min. This nanodispersion was added to epoxy resin (80-90 parts) and stirred thoroughly for 3h at a speed of 400r / min. Then, a photoinitiator triarylsulfonium hexafluoroantimonate (5 parts), a BYK057 defoamer (1.5 parts) and a fluorinated acrylate leveling agent (1 part) were added, and the mixture was stirred for 2 hours at a rotation speed of 200 / min to obtain a cationic UV-curing coating.

[0037] Table 1 is a comparison of the conventional UV samples and the coatings in each embodiment.

[0038]

[0039] According to the comparative data in Table 1 above, it can be seen that the coating prepared in the present application has good weather resistance and corrosion resistance.

[0040] The most important advantages of UV-curable coatings include: (1) low investment cost (using UV lamps instead of ovens / stoves); (2) low energy requirements for crosslinking even at room temperature; and (3) reduced solvent emissions. Compared with free radical UV curing, cationic UV curing technology has the advantages of low cost, excellent adhesion and high solvent resistance. At the same time, the nanocontainer and corrosion inhibitor in this application both have certain anti-corrosion effects. The preparation of nanocontainers loaded with corrosion inhibitors has a synergistic effect, which can greatly improve the anti-corrosion effect. The solution of this application is simple in formula and has good anti-corrosion effect. Cationic UV-curable anti-corrosion coatings can be widely used on metal material surfaces in various environments.

[0041] The above description is only an embodiment of the present application and does not limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the specification of the present application, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A corrosion-resistant cationic UV-curing coating, characterized in that: The invention is composed of the following components in parts by weight: 80-90 parts of epoxy resin, 5-15 parts of solvent, 3-8 parts of photoinitiator, 1-4 parts of nano container loaded with corrosion inhibitor, and 1-7 parts of auxiliary agent.

2. The corrosion-resistant cationic UV-curing coating according to claim 1, characterized in that: The epoxy resin is a bisphenol A type epoxy resin, and the epoxy value of the epoxy resin is between 0.3 and 0.6 (eq / 100g).

3. The corrosion-resistant cationic UV-curing coating according to claim 1, characterized in that: The solvent is any one of 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, 3,3'-(oxybismethylene)bis(3-ethyl)oxetane, 1,4-butanediol diglycidyl ether or neopentyl glycol diglycidyl ether, or a combination of at least two thereof.

4. The corrosion-resistant cationic UV-curing coating according to claim 1, characterized in that: The photoinitiator is one or a combination of triarylsulfonium hexafluoroantimonate, diphenyl-(4-phenylsulfonium)phenylsulfonium hexafluoroantimonate, and triphenylsulfonium hexafluorophosphate.

5. The corrosion-resistant cationic UV-curing coating according to claim 1, characterized in that: The auxiliary agents include defoaming agents and fluorine-containing acrylate leveling agents.

6. A method for preparing a corrosion-resistant cationic UV-curing coating, characterized in that: The following steps are involved: Preparation of a nanocontainer loaded with a corrosion inhibitor: adding a nanocontainer to deionized water with a mass fraction of 5% to 15% and stirring thoroughly, then adding an aqueous solution containing a corrosion inhibitor with a mass fraction of 5% to 15% to the above suspension to prepare a mixed solution, adding the mixed solution to a high-speed ball mill for mixing and dispersion for 2 to 6 hours, filtering and precipitating, and vacuum drying the precipitate at 60 to 80° C. to obtain the nanocontainer loaded with the corrosion inhibitor; Preparation of nano-dispersion: adding the nano-container loaded with the corrosion inhibitor into a solvent, and stirring the mixture for 1 to 3 hours at a rotation speed of 500 to 800 r / min to obtain the nano-dispersion; Preparation of cationic UV-curable coating: Add the nano-dispersion liquid into epoxy resin and stir it thoroughly for 2 to 5 hours at a speed of 200 to 500 r / min. Then add photoinitiator and auxiliary agent and continue stirring thoroughly for 2 to 4 hours at a speed of 200 to 600 r / min to obtain nano-dispersion liquid.

7. The method according to claim 6, characterized in that The molar ratio of the corrosion inhibitor to the nano container is 0.5-5:

100.

8. The method according to claim 6, characterized in that The nano container comprises one or a combination of two of SiO2 microcapsules, mesoporous TiO2 nanoparticles, layered hydroxides, montmorillonite, zeolite, hydroxyapatite, inorganic hollow spheres, carbon nanotubes, graphene oxide, and hexagonal boron nitride.

9. The method according to claim 7, characterized in that: The corrosion inhibitor comprises rare earth oxide, rare earth metal salt and rare earth hydroxide or a combination of two thereof.

10. The method according to claim 9, characterized in that The rare earth in the rare earth hydroxide is one of lanthanum, cerium, neodymium and yttrium.

Citation Information

Cited By

  • Corrosion inhibition and rust prevention powder containing lanthanum cerium oxide and preparation method of corrosion inhibition and rust prevention powder

    CN121779966A

  • A corrosion-inhibiting and rust-preventing powder containing lanthanum and cerium oxide and its preparation method

    CN121779966B