Centrifugal casting method of inner flange metal pipe
Through centrifugal casting method, the flange cavity is formed using resin sand core and retaining ring, and combined with the design of threaded conical brazing blocks and asbestos gaskets, the problems of deformation and material consumption in flange metal pipe production are solved, achieving high efficiency , low-cost production process.
Patent Information
- Application Number
- CN202410888362.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-01
AI Technical Summary
In the production of existing flange metal pipes, there are problems such as high deformation, large processing allowance, long production cycle and high material consumption, especially these problems caused by sand casting methods cannot be effectively solved.
A centrifugal casting method of inner flange metal tube is adopted to form a flange cavity by making resin sand core and resin sand retaining ring, and fixing it with threaded conical brazing blocks and asbestos gaskets to quickly solidify the molten iron to form an internal method To reduce thermal cracking and cast pipe deformation.
It effectively improves product quality, reduces costs, shortens production cycle, reduces material consumption, improves output, and avoids the occurrence of thermal cracking.
Smart Images

Figure CN118875240A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a manufacturing technology of an inner flange metal pipe, in particular to a centrifugal casting method of an inner flange metal pipe. Background Art
[0002] At present, most flange metal pipes produced in China adopt the sand casting method. The metal pipes produced by this method have problems such as high deformation, large processing allowance, long production cycle, and high material consumption. Summary of the Invention
[0003] The technical problem to be solved by the present invention is to overcome the defects of the above-mentioned technology and provide a centrifugal casting method for an inner flange metal pipe.
[0004] To solve the above technical problems, the present invention provides a technical solution for a centrifugal casting method of an inner flange metal pipe: an inner retaining ring made of resin sand is fixed in the pipe membrane to form a flange cavity between the inner retaining ring and the pipe membrane, and continuous casting is performed to form the flange, comprising the following steps:
[0005] Step 1: Make resin sand core;
[0006] Step 2: Use the resin sand retaining ring core box 21 to make a resin sand retaining ring 4 with the same outer diameter and inner diameter as the pipe mold baffle, and apply refractory paint on the flange surface after it is made;
[0007] Step 3: Make a fixed casting trough and a movable casting car; the movable casting car is provided with a fixed molten iron ladle 9, left and right movable guide ladles 10, and two molten iron flow channels A and B in the trough;
[0008] Step 4: Install the resin sand core and resin sand retaining ring;
[0009] Step 5: Casting the pipe.
[0010] The advantages of the present invention compared with the prior art are:
[0011] 1. Changed the old traditional sand casting method, effectively improved product quality, reduced costs and increased output;
[0012] 2. A flange cavity is formed using a resin sand core and fixed with a threaded tapered brazing block. When the pipe mold is just being cast, the spring can firmly connect the brazing block to the pipe mold due to its expansion, and the asbestos gasket can extend the validity period of the spring. The tapered shape allows the incoming molten iron to solidify quickly, interacting with the chilled iron to form a liquid molten iron flange cavity, allowing the flange to be quickly formed.
[0013] 3. Since the brazing block is threaded, its length and diameter are determined by the wall thickness, diameter and flange height of the cast pipe. Therefore, when the molten iron is poured, the external thread will quickly dissolve with the cast pipe, forming a state of external dissolution and internal support.
[0014] 4. Due to the heat preservation effect of the resin sand retaining ring and the second spraying, the molten iron remains liquid, which is conducive to the formation of the flange;
[0015] 5. Excess molten iron flows into the inner cavity of the cast pipe through the overflow port. Since the core bone and chill of the resin sand core are fixed with resin sand, the sand core has a certain degree of yielding, so that the cast pipe will not produce thermal cracking. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a structural schematic diagram of equipment used in implementing a centrifugal casting method for an inner flange metal pipe according to the present invention.
[0017] Figure 2 The present invention is a structural schematic diagram of a device for producing a resin sand core in a centrifugal casting method for an inner flange metal pipe.
[0018] Figure 3 The invention discloses a structural schematic diagram of a core round tube assembly and a chiller in a centrifugal casting method for an inner flange metal tube.
[0019] Figure 4 The invention discloses a structural schematic diagram of a centrifugal casting method for an inner flange metal pipe during installation of a core round pipe, chiller and reinforcing ribs.
[0020] Figure 5 The invention discloses a structural schematic diagram of the assembly and fastening of a resin sand core in a centrifugal casting method for an inner flange metal pipe.
[0021] Figure 6 The present invention is a structural schematic diagram of a resin sand core box and a resin sand retaining ring core box in a centrifugal casting method for an inner flange metal pipe.
[0022] Figure 7 The present invention is a schematic diagram of a resin sand core installation in a centrifugal casting method for an inner flange metal pipe.
[0023] Figure 8 The present invention is a schematic diagram of the installation and positioning of a resin sand core in a centrifugal casting method for an inner flange metal pipe.
[0024] As shown in the figure:
[0025] 1. Pipe mold, 2. Pipe mold fixing hole, 3. Threaded tapered brazing block, 4. Resin sand retaining ring, 5. Pipe mold retaining ring, 6. Resin sand core, 7. Fixed casting flow channel, 8. Pipe mold fixing pin, 9. Molten iron fixed ladle, 10. Left and right movable guide ladle, 11. Core bone round tube assembly, 12. Chill, 13. Asbestos gasket, 14. Spring, 15. Spring washer, 16. Nut, 17. Bolt one, 18. Bolt two, 19. Overflow hole model rod, 20. Resin sand core box, 21. Resin sand retaining ring core box, 22. Movable casting cart, 23. Bolt three, 24. Wooden plywood retaining ring. DETAILED DESCRIPTION
[0026] To make the objectives, technical solutions, and advantages of the embodiments of the present invention more clear, the technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings herein can be arranged and designed in various different configurations.
[0027] Example 1, combined with the attached Figure 1-8 A centrifugal casting method for an inner flange metal pipe is provided, wherein an inner retaining ring made of resin sand is fixed in the pipe film to form a flange cavity between the inner retaining ring and the pipe film, and continuous casting is performed to form the flange, comprising the following steps:
[0028] Step 1: Making resin sand core
[0029] a. Place the resin sand core box on the vibration platform and align the three oil top holes with the oil top;
[0030] b. With an iron tube, a nut 16 is welded to the inner wall at one end, a piece of iron plate is welded at each end, and holes are punched up and down to form a core bone tube assembly 11;
[0031] c. Making a chill 12 and welding a plurality of connecting bars on it;
[0032] d. Make a threaded tapered brazing block 3. Its diameter, length and number on each resin sand core are determined according to the diameter and wall thickness of the cast pipe. An asbestos gasket 13, a spring 14 and a spring washer 15 are arranged in sequence between the threaded tapered brazing block 3 and the nut 16. A bolt 17 is screwed onto the nut 16. Figure 2 ;
[0033] e. Insert the chill 12 into one end of the core bone round tube assembly 11, place multiple chills 12 into the resin sand core box 20 in sequence, and fix them to the resin sand core box 20 in sequence with the second bolt 18. Then, string the reinforcement ribs into the holes of the iron block and tighten them, and then connect them to the reinforcement ribs on the chill 12. After the connection is completed, put the overflow hole model rod 19, pour the resin sand into the resin sand core box 20 and vibrate it. After the completion, loosen the second bolt 18 and pull it out, push it out with an oil jack, apply refractory paint on the chill surface and flange surface of the sand core, and then perform dynamic balancing correction; see attached. Figure 3 , Attachment Figure 4 .
[0034] Step 2:
[0035] Use resin sand retaining ring core box 21 to make resin sand retaining ring 4 with the same outer diameter and inner diameter as pipe mold baffle 5, and apply refractory paint on the flange surface after it is done. Figure 6 .
[0036] Step 3:
[0037] 1. Make a fixed casting chute 7 and a movable casting car 22;
[0038] 2. A fixed molten iron ladle 9 and left and right movable guide ladles 10 are provided on the movable casting car 22, and two molten iron flow channels A and B are provided in the chute.
[0039] Step 4: Installation of resin sand core and resin sand retaining ring
[0040] a. First, screw the bolt 17 into the nut 16, then sequentially place the spring washer 15, spring 14, and asbestos washer 13 into the core bone round tube assembly 11. Finally, place the threaded tapered brazing block 3, which has been pickled and coated with brazing agent, into the area flush with the round tube diameter and secure it with a weak adhesive to prevent it from falling off during installation.
[0041] b. Hang the resin sand core into the pipe mold 1, then put the positioning blocks C and D into the pipe mold 1, fix the position, and place the sand core on the positioning blocks C and D. After placing them, place the positioning block E on the sand core; see Figure 7 、 Figure 8 ;
[0042] c. After the sand core is placed, use bolt 3 23 to adjust it so that the sand core and the pipe mold 1 are concentric. Then tighten bolt 17 step by step and symmetrically to fix the sand core firmly in the pipe mold 1. Then loosen bolt 3 23 and pull it out. Then nail the wooden plywood retaining ring 24 to the sand core. Repeat the same process on both sides. See attached. Figure 5 ;
[0043] d. Place the resin sand retaining ring 4 and the pipe mold retaining ring 5 into the pipe mold 1 in sequence, and insert the pipe mold fixing pin 8 into the pipe mold fixing hole 2 and tighten it. Repeat the same process on both sides.
[0044] e. Then rotate the pipe mold 1 and spray the flange cavity for the second time. Due to the obstruction of the wooden plywood retaining ring 24, the paint can be prevented from being sprayed onto the threaded tapered brazing block 3, affecting the dissolution of the threaded tapered brazing block 3.
[0045] Step 5: Casting of cast pipe
[0046] a. Place the fixed casting trough 7 in front of the pipe mold 1 so that the casting port is vertically aligned with the pipe mold flange cavity;
[0047] b. When the speed reaches the specified value, the movable casting car 22 starts casting using the flow channel A in the chute. At the same time, the fixed molten iron ladle 9 also casts at a small flow rate. Due to the rapid cooling of the chill 12 and the threaded tapered brazing block 3, and the secondary spraying of the thermal insulation coating on the flange cavity, the sand core solidifies quickly, forming a flange high-temperature molten iron cavity. After the flange is formed, the excess molten iron flows from the overflow port to the inner cavity of the cast pipe;
[0048] c. When the movable casting car 22 retreats to the rear of the pipe mold 1 and the runner B is aligned with the flange cavity, stop the movable casting car 22 and quickly push the left and right movable guide ladles 10 to cast the two runners A and B simultaneously. The distance between the runners A and B depends on the retreat speed of the movable casting car 22, the flow rate and flow rate of the molten iron. Similarly, after the flange is formed, the excess molten iron flows into the cast pipe from the overflow port. To reduce the deformation of the cast pipe, the cast pipe temperature is lowered to 200-180 degrees. Then the pipe mold 1 stops rotating, the fixed casting trough 7 is pulled away, and the cast pipe is pulled out. See attached. Figure 1 .
[0049] In the description of the embodiments of the present invention, it should be noted that if the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc. appear, the orientation or position relationship indicated is based on the orientation or position relationship shown in the accompanying drawings, or the orientation or position relationship in which the product of the invention is usually placed when in use. It is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation. Therefore, it should not be understood as limiting the present invention. In addition, the terms "first", "second", "third", etc. are only used to distinguish the description and should not be understood as indicating or implying relative importance.
[0050] Furthermore, the use of terms such as "horizontal," "vertical," and "overhanging" does not necessarily imply that the component must be absolutely horizontal or overhanging, but rather that it can be slightly tilted. For example, "horizontal" simply means that its direction is more horizontal than "vertical," not that the structure must be completely horizontal, but rather that it can be slightly tilted.
[0051] In the description of the embodiments of the present invention, "a plurality of" means at least two.
[0052] In the description of the embodiments of the present invention, it should be noted that, unless otherwise expressly specified or limited, the terms "disposed," "installed," "connected," and "connected" should be understood in a broad sense. For example, they can refer to fixed connections, detachable connections, or integral connections; they can refer to mechanical connections or electrical connections; they can refer to direct connections or indirect connections through an intermediate medium; and they can refer to internal connections between two components. Those skilled in the art will understand the specific meanings of the above terms in the present invention based on specific circumstances.
[0053] The present invention and its embodiments are described above. This description is not restrictive. The drawings show only one embodiment of the present invention, and the actual structure is not limited thereto. In short, if a person skilled in the art is inspired by this and, without departing from the purpose of the present invention, designs structures and embodiments similar to this technical solution without inventiveness, they shall fall within the scope of protection of the present invention.
Claims
1. A centrifugal casting method for an inner flange metal pipe, characterized in that The method comprises the following steps: fixing an inner retaining ring made of resin sand in a tube membrane, forming a flange cavity between the inner retaining ring and the tube membrane retaining ring, and continuously casting to form a flange. Step 1: Make resin sand core; Step 2: Use the resin sand retaining ring core box to make a resin sand retaining ring with the same outer diameter and inner diameter as the pipe mold baffle, and apply refractory paint on the flange surface after it is completed; Step 3: Make a fixed casting trough and a movable casting car; the movable casting car is provided with a fixed molten iron ladle, left and right movable guide ladles, and two molten iron flow channels A and B are provided in the trough; Step 4: Install the resin sand core and resin sand retaining ring; Step 5: Casting the pipe.
2. The centrifugal casting method of an inner flange metal pipe according to claim 1, characterized in that: The step 1 specifically includes: a. Place the resin sand core box on the vibration platform and align the three oil top holes with the oil top; b. Use an iron round tube, weld a nut on the inner wall of one end, weld an iron plate on each end, and punch holes on the top and bottom to make a core bone round tube assembly; c. Make a chill and weld multiple connecting bars on it; d. Making a threaded tapered brazing block, the diameter, length and number of which on each resin sand core are determined according to the diameter and wall thickness of the cast pipe. An asbestos gasket, a spring and a spring gasket are arranged in sequence between the threaded tapered brazing block and the nut, and a bolt is screwed on the nut; e. Insert the chiller into one end of the core bone round tube assembly, put multiple chillers into the resin sand core box in turn, fix them on the resin sand core box in turn with bolt 2, then string the reinforcing ribs into the holes of the iron block and tighten them, and then connect them to the reinforcing ribs on the chiller. After the connection is completed, put on the overflow hole model rod, pour the resin sand into the resin sand core box for vibration, and after completion, loosen bolt 2 and pull it out, push it out with an oil jack, apply refractory coating on the chiller surface and flange surface of the sand core, and then perform dynamic balancing correction.
3. The centrifugal casting method of an inner flange metal pipe according to claim 1, characterized in that: The step 4 specifically includes: a. First, screw the bolt into the nut, then put the spring washer, spring, and asbestos washer into the core bone round tube assembly in order, and finally put the threaded tapered brazing block that has been pickled and coated with brazing agent into the place that is flush with the diameter of the round tube, and apply weak glue to fix it to prevent it from falling off during installation; b. Hang the resin sand core into the tube mold, then put the positioning blocks C and D into the tube mold, fix the position, put the sand core on the positioning blocks C and D, and then put the positioning block E on the sand core; c. After the sand core is placed, use bolt 3 to adjust it so that the sand core and the pipe mold are concentric, then tighten bolt 1 step by step and symmetrically to fix the sand core firmly in the pipe mold, then loosen bolt 3 and pull it out, then nail the wooden plywood retaining ring to the sand core, and do the same on both sides; d. Put the resin sand retaining ring and the pipe mold retaining ring into the pipe mold in turn, and insert the pipe mold fixing pin into the pipe mold fixing hole and tighten it. Do the same on both sides; e. Then rotate the pipe mold and spray the flange cavity for the second time. Due to the shielding of the wooden plywood retaining ring, the paint can be prevented from being sprayed onto the threaded tapered brazing block, which will affect the dissolution of the threaded tapered brazing block.
4. The centrifugal casting method of an inner flange metal pipe according to claim 1, characterized in that: The step five specifically includes: a. Place the fixed casting trough in front of the pipe mold so that the casting port is vertically aligned with the flange cavity of the pipe mold; b. When the speed reaches the specified value, the movable casting car starts to cast with the A flow channel in the flow trough, and the fixed molten iron ladle also casts with a small flow rate. Due to the rapid cooling of the cold iron and the threaded tapered brazing block, and the secondary spraying of the thermal insulation coating on the flange cavity, the sand core solidifies quickly to form a flange high-temperature molten iron cavity. After the flange is formed, the excess molten iron flows from the overflow port to the inner cavity of the casting pipe; c. When the movable casting car retreats to the back of the pipe mold and the B runner gate is aligned with the flange cavity, stop the movable casting car, quickly push the left and right movable guide ladles to cast the A and B runners at the same time. The front and rear distance between the A runner gate and the B runner gate depends on the retreat speed of the movable casting car, the flow rate and flow rate of the molten iron. Similarly, after the flange is formed, the excess molten iron flows into the cast pipe from the overflow port. In order to reduce the deformation of the cast pipe, when the cast pipe temperature is reduced to 200 degrees-180 degrees, the pipe mold 1 stops rotating, the fixed casting flow channel 7 is pulled away, and the cast pipe can be pulled out.