Double-ion welding process for improving performance of charging barrel

By employing a dual-ion welding process and ion nitriding treatment on the barrel to form a wear-resistant and corrosion-resistant packing layer, the problem of short barrel service life is solved, achieving cost reduction and performance improvement.

CN118875445APending Publication Date: 2024-11-01NINGBO HAOLI METAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410996979.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In die-casting companies, the service life of the barrel is lower than expected, mainly because the pouring port and the joint between the barrel and the mold are easily corroded, resulting in a decline in performance. Existing solutions increase manufacturing and procurement costs.

Method used

A filler layer is formed in a predetermined area of ​​the barrel using a dual ion welding process, and then formed through ion nitriding treatment using welding wire with specific components and optimized process parameters, including preheating, spiral welding, grinding and other steps, resulting in a wear-resistant and corrosion-resistant filler layer.

Benefits of technology

It significantly extends the service life of the barrel, reduces costs, and improves barrel performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118875445A_ABST
    Figure CN118875445A_ABST
Patent Text Reader

Abstract

The invention discloses a double-ion welding technology for improving the performance of a charging barrel. The double-ion welding technology comprises the following steps that firstly, a filler layer is formed in a preset area through welding wire welding by means of an ion welding device; secondly, ion nitriding treatment is conducted on the filler layer through an ion nitriding furnace, a strengthening process is designed in the scheme, welding wires are solidified and filled in a preset area through ion welding to form the filler layer, nitriding treatment is conducted on the filler layer, and the filler layer formed through double-ion welding is excellent in the aspects of abrasion resistance, corrosion resistance and the like; and when applied to the charging barrel, the charging barrel can be greatly prolonged in service life and reduced in cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of material technology, and in particular to a dual ion welding process for improving barrel performance. Background Art

[0002] Die-casting molding devices are often used in die-casting enterprises of non-ferrous metals such as brass, aluminum and zinc alloy. The barrel of the die-casting machine is a key component. According to market feedback: the service life of the barrel is lower than the expected life. The main reason is that the barrel cavity at the pouring port and the cavity where the barrel and the mold are connected are easily corroded, the performance is reduced, and the service life is shortened. To solve this problem, most companies use higher-specification steel to form barrels, which leads to higher manufacturing and procurement costs and needs to be improved. Summary of the invention

[0003] To solve at least one of the above technical defects, the present invention provides the following technical solutions:

[0004] This application document discloses a dual ion welding process for improving barrel performance, comprising the following steps:

[0005] First, forming a filler layer in a predetermined area by welding with a welding wire using an ion welding device;

[0006] Second, the filler layer is subjected to ion nitriding treatment by using an ion nitriding furnace.

[0007] This scheme designs an enhanced process. Through ion welding, the welding wire is solidified and filled in a predetermined area to form a filler layer. The filler layer is nitrided. The filler layer formed by double ion welding has excellent performance in wear resistance and corrosion resistance. When applied to the barrel, it can greatly extend the service life of the barrel and reduce costs.

[0008] Furthermore, by mass, the components of the welding wire are as follows: C0.6-1.0%, Cr15-17%, B3.5-4.5%, Si3.0-4.0%, Fe0-25%, unavoidable impurities ≤1%, Ni balance, specific welding wire components, combined with the dual ion process, help to further improve the performance of the filler layer.

[0009] Furthermore, during the welding process, preheating is performed to make the temperature of the predetermined area at 180-220°C, and then welding is performed with welding wire. Preheating and welding help to improve the bonding strength of the filler layer.

[0010] Furthermore, the parameters of the ion welding device are as follows: welding gun argon gas 15-25L / min, shielding gas 5-7L / min, welding speed 300-600mm / min, welding method is spiral welding or surfacing, and the optimal parameters help to further improve the performance of the filler layer.

[0011] Furthermore, the filler layer has a thickness of 0.5-2 mm.

[0012] Furthermore, the ion nitridation treatment parameters are as follows: treatment temperature 500-550°C, treatment voltage 650-750V, treatment time 30-40h, ammonia flow rate 600-1600L / h, gas pressure 260-400Pa, duty cycle 60-80%, and the preferred parameters help to further improve the performance of the packing layer.

[0013] Furthermore, a grinding step is included, in which a predetermined area is ground before welding, which helps to improve the bonding strength and the uniformity of the thickness of the filler layer.

[0014] Furthermore, it also includes a grinding step, in which the filler layer is ground after welding, or the nitride layer is ground after ion nitriding, such as grinding away tiny cracks in the welding area. For example, the nitride layer after nitriding has requirements on size and surface properties, and then it is polished to meet the requirements, or the local hard part is ground away to make the performance more uniform.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] 1. The present invention uses a breakthrough dual ion welding process to form a filler layer, so as to strengthen the performance of a predetermined area at a fixed point. For example, when strengthening on the barrel, it helps to increase the service life and reduce costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0018] Figure 1 It is a schematic diagram of the barrel structure;

[0019] Figure 2 It is a schematic diagram of the barrel structure;

[0020] Wherein, the accompanying drawings are marked as follows:

[0021] 1. Barrel; 2. Pour port; 3. Packing layer. DETAILED DESCRIPTION

[0022] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.

[0023] Example 1

[0024] like Figure 1 , Figure 2As shown, the dual ion welding process forms a filler layer 3 (or lining layer) at the inner circumferential wall of the barrel 1 cavity connected to the pouring port 2, and forms a filler layer at the inner circumferential wall of the cavity opening at the rear end of the barrel cavity (i.e., the cavity opening connected to the mold gate sleeve).

[0025] Specifically, a dual ion welding process for improving barrel performance includes the following steps:

[0026] First, turn and grind the predetermined welding area of ​​the barrel wall.

[0027] Second, preheating the predetermined welding area to 200° C., and then forming a filler layer in the predetermined welding area by welding with welding wire through an ion welding device, wherein the welding wire components account for, by mass, C0.98%, Cr15.89%, B3.82%, Si3.35%, Fe24.25%, unavoidable impurities ≤1%, Ni remainder, and the welding method is spiral welding.

[0028] The parameter settings of the ion welding device are as follows: welding gun argon gas 20L / min, shielding gas 5L / min, welding speed 350mm / min, welding current 160A, and nozzle distance 6mm.

[0029] The thickness of the welded filler layer is 1 mm.

[0030] Third, grind the filler layer to eliminate tiny cracks or other defects.

[0031] Fourth, the filler layer is subjected to ion nitriding treatment by an ion nitriding furnace, and the ion nitriding treatment parameters are as follows: treatment temperature 520±2°C, treatment voltage 700V, treatment time 35h, ammonia flow rate 700L / h, gas pressure 350Pa, and duty cycle 70%.

[0032] Fifth, the nitride layer is polished to meet the predetermined size and make the surface smooth.

[0033] Example 2

[0034] The difference from Example 1 is that, by mass, the welding wire components account for: C0.7%, Cr16.5%, B4.3%, Si3.9%, Fe20%, unavoidable impurities ≤1%, and Ni balance.

[0035] The parameter settings of the ion welding device are: welding gun argon gas 25L / min, shielding gas 6L / min, welding speed 420mm / min, welding current 160A, and nozzle distance 6mm.

[0036] The thickness of the welded filler layer is 1.5 mm.

[0037] The ion nitridation treatment parameters are as follows: treatment temperature 540±2°C, treatment voltage 680V, ​​treatment time 38h, ammonia flow rate at 1000L / h, gas pressure at 320Pa, and duty cycle at 70%.

[0038] Example 3

[0039] The difference from Example 1 is that, by mass, the welding wire components account for: C0.85%, Cr16%, B4%, Si3.4%, Fe18%, unavoidable impurities ≤1%, and Ni as the balance.

[0040] The parameter settings of the ion welding device are as follows: welding gun argon gas 17L / min, shielding gas 7L / min, welding speed 510mm / min, welding current 160A, and nozzle distance 6mm.

[0041] The thickness of the welded filler layer is 2 mm.

[0042] The ion nitridation treatment parameters are as follows: treatment temperature 540±2°C, treatment voltage 720V, treatment time 40h, ammonia flow rate at 1200L / h, gas pressure at 400Pa, and duty cycle at 70%.

[0043] Comparative Example 1

[0044] The difference from Example 1 is that the welding wire components are as follows: C 0.84%, Cr 13%, B 4.2%, Si 3.6%, Fe 19%, unavoidable impurities ≤ 1%, and Ni as the balance.

[0045] Comparative Example 2

[0046] The difference from Example 1 is that arc welding replaces plasma welding.

[0047] Comparative Example 3

[0048] The difference from Example 1 is that the plasma treatment step is omitted.

[0049] The performance of the packing layer formed in the above embodiment and comparative example was tested, as shown in the following table:

[0050] Table 1

[0051]

[0052]

[0053] Corrosion resistance description: Aluminum liquid impacts the welding layer, and the impact time for each mold is 8S;

[0054] Lifespan description: Cumulative number of uses.

[0055] It can be seen from Table 1 that the filler layer formed by dual ion welding far exceeds the filler layer formed by the comparative example in hardness, corrosion resistance, wear resistance, etc. From the comparison of the performance data of Example 4 with Examples 1-3, it can be seen that the welding wire of a specific component and the filler layer formed by dual ion welding have more transitional performance.

[0056] The above are only preferred embodiments of the present invention. The protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. A dual ion welding process for improving barrel performance, characterized in that: The following steps are involved: First, forming a filler layer in a predetermined area by welding with a welding wire using an ion welding device; Second, the filler layer is ion nitrided by an ion nitriding furnace.

2. A dual ion welding process for improving barrel performance as claimed in claim 1, characterized in that: By mass, the components of the welding wire are as follows: C0.6-1.0%, Cr15-17%, B3.5-4.5%, Si3.0-4.0%, Fe0-25%, unavoidable impurities ≤1%, and Ni balance.

3. A dual ion welding process for improving barrel performance as claimed in claim 1, characterized in that: During the welding process, the predetermined area is preheated to a temperature of 180-220°C, and then welded with welding wire.

4. A dual ion welding process for improving barrel performance as claimed in claim 3, characterized in that: The parameters of the ion welding device are as follows: welding gun argon gas: 15-25L / min, shielding gas: 5-7L / min, welding speed: 300-600mm / min, welding method is spiral welding or surfacing.

5. A dual ion welding process for improving barrel performance as claimed in claim 1, characterized in that: The thickness of the filler layer is 0.5-2 mm.

6. A dual ion welding process for improving barrel performance as claimed in claim 1, characterized in that: The ion nitridation treatment parameters are as follows: treatment temperature 500-550°C, treatment voltage 650-750V, treatment time 30-40h, ammonia flow rate 600-1600L / h, gas pressure 260-400Pa, and duty cycle 60-80%.

7. A dual ion welding process for improving barrel performance as claimed in claim 1, characterized in that: A grinding step is also included to grind the predetermined area before welding.

8. A dual ion welding process for improving barrel performance as claimed in claim 1, characterized in that: The method further comprises a grinding step, wherein the filler layer is ground after welding, or the nitrided layer is ground after ion nitriding.