A process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste
A process utilizing coal gangue and additives like a water-blocking modifier through wet ball milling and steam curing addresses the low strength and waterproof issues of coal gangue tiles, resulting in high-strength, durable floor tiles for modern buildings.
Patent Information
- Application Number
- CN202411391117.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-10-08
AI Technical Summary
Coal gangue solid waste is difficult to utilize effectively due to its high porosity and water absorption, leading to low strength and poor waterproof performance in floor tiles, limiting their application in engineering projects with high strength and waterproof requirements.
A process involving the comprehensive utilization of coal gangue, cement, quicklime, kaolin, basalt, a water-blocking modifier, water reducer, early strength agent, defoaming agent, and water, followed by wet ball milling and constant-pressure steam curing to form high-strength floor tiles.
The process enhances the mechanical strength and waterproof performance of floor tiles, making them suitable for modern buildings with improved durability and extended service life.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of building materials, and in particular to a process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste. Background Art
[0002] Coal gangue is a large amount of solid waste generated during coal mining and washing. The traditional treatment methods mainly include stacking and landfilling, but these methods have problems such as land resource loss, environmental pollution and gas emissions. In recent years, with the enhancement of environmental awareness and the promotion of the concept of resource recycling, the comprehensive utilization of coal gangue has become a research hotspot. Among them, converting coal gangue into building materials, especially high-strength floor tiles, has significant economic and environmental benefits. Coal gangue has good physical properties, but its high porosity and strong water absorption result in limited waterproof performance of the prepared high-strength floor tiles, which are prone to penetration and shedding, affecting their mechanical strength and service life, and limiting their application in engineering projects with high strength and waterproof requirements. Therefore, it is of great significance to develop a process for the comprehensive utilization of coal gangue solid waste to prepare high-strength floor tiles. Summary of the invention
[0003] In order to overcome the above-mentioned technical problems, the purpose of the present invention is to provide a process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste, by uniformly mixing coal gangue, cement, quicklime, kaolin, basalt, water-blocking modifier, water reducer, early strength agent, defoaming agent and water, and then subjecting the mixture to wet ball milling to obtain a mixed slurry, and then pouring the mixed slurry into a mold to form a floor tile body, and then subjecting the floor tile body to constant-pressure steam curing to obtain high-strength floor tiles, thereby solving the problem that the existing coal gangue solid waste floor tiles have the disadvantages of low strength and poor waterproofness, and are difficult to meet the actual needs of engineering applications.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste comprises the following steps:
[0006] Step 1: Weigh 45-55 parts of coal gangue, 22-28 parts of cement, 8-12 parts of quicklime, 7-11 parts of kaolin, 11-17 parts of basalt, 2.5-9.5 parts of water-blocking modifier, 1.2-2.4 parts of water reducer, 1-3 parts of early strength agent, 0.5-0.9 parts of defoaming agent and 51-63 parts of water according to weight, and set aside;
[0007] Step 2: Evenly mix the coal gangue, cement, quicklime, kaolin, basalt, water-blocking modifier, water-reducing agent, early strength agent, defoaming agent and water, and then wet-ball mill to obtain a mixed slurry;
[0008] Step 3: Pour the mixed slurry into a mold to form a floor tile body, and then cure the floor tile body with constant pressure steam at a pressure of 15-20MPa and a temperature of 170-180°C for 10-12 hours to obtain a high-strength floor tile.
[0009] As a further solution of the present invention: the water blocking modifier is prepared by the following steps:
[0010] Step s1: 1,1,5,5-tetramethyl-3,3-diphenyltrisiloxane, allylamine, chloroplatinic acid and anhydrous tetrahydrofuran are added to a three-necked flask equipped with a stirrer, a thermometer and an air guide tube, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 20-25° C. and a stirring rate of 300-400 r / min for 20-30 min, and then the temperature is raised to 60-65° C. and the stirring reaction is continued for 3-5 h. After the reaction is completed, the reaction product is cooled to room temperature, and then the solvent is removed by rotary evaporation to obtain intermediate 1;
[0011] Step s2: Add intermediate 1, 2,3,4-trihydroxybenzaldehyde and anhydrous ethanol to a three-necked flask equipped with a stirrer, a thermometer and an air duct, introduce nitrogen protection, stir and react for 20-30 minutes at a temperature of 20-25°C and a stirring rate of 300-400r / min, then raise the temperature to 60-65°C and continue to stir and react for 6-8 hours. After the reaction is completed, cool the reaction product to room temperature, pour it into ice water, let it stand to precipitate, and then vacuum filter it. Wash the filter cake with distilled water for 2-3 times, and then place it in a vacuum drying oven and dry it at a temperature of 50-55°C for 3-5 hours to obtain intermediate 2;
[0012] Step s3: Add intermediate 2, benzyltriethylammonium chloride and anhydrous ethanol to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a constant pressure dropping funnel, introduce nitrogen protection, stir and react for 10-15 minutes at a temperature of 20-25°C and a stirring rate of 300-400r / min, then add epichlorohydrin dropwise while stirring, control the dropping rate to 1-2 drops / s, and continue to stir and react for 7-8 hours under the condition of heating to 70-75°C after the dropwise addition is completed, and then continue to stir and react for 10-15 minutes under the condition of cooling to 30-35°C, and then add potassium hydroxide solution dropwise while stirring, control the dropping rate to 1-2 drops / s, and continue to stir and react for 6-7 hours under the condition of heating to 60-65°C after the dropwise addition is completed, and after the reaction is completed, cool the reaction product to room temperature, then vacuum filter, and rotary evaporate the filtrate to remove the solvent to obtain intermediate 3;
[0013] Step s4: Add intermediate 3, hexafluoroisopropanol, aluminum phosphotungstate and anhydrous toluene to a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir the reaction at a temperature of 20-25°C and a stirring rate of 300-400r / min for 20-30min, then heat the temperature to 90-95°C and stir the reaction for 6-8h. After the reaction, cool the reaction product to room temperature, add it to ethyl acetate, and then let it stand for stratification. Wash the organic phase with sodium bicarbonate solution and saturated sodium chloride solution 2-3 times in turn, and then dry it with anhydrous magnesium sulfate. Then, vacuum filter it, and rotary evaporate the filtrate to remove the solvent to obtain a water-blocking modifier.
[0014] As a further solution of the present invention: the water reducer is one of SP401 polycarboxylic acid high-efficiency water reducer and high-efficiency water reducer 2651F.
[0015] As a further solution of the present invention: the early strength agent is one of calcium chloride and triethanolamine.
[0016] As a further solution of the present invention: the defoamer is one of the defoamer byk-a530, the defoamer byk-024 and the defoamer byk-028.
[0017] As a further solution of the present invention: the usage ratio of the 1,1,5,5-tetramethyl-3,3-diphenyltrisiloxane, allylamine, chloroplatinic acid and anhydrous tetrahydrofuran in step s1 is 10 mmol: 11-13 mmol: 0.01-0.03 g: 40-50 mL.
[0018] As a further solution of the present invention: the usage ratio of the intermediate 1, 2,3,4-trihydroxybenzaldehyde and anhydrous ethanol in step s2 is 10mmol:22-25mmol:40-50mL.
[0019] As a further scheme of the present invention: the usage ratio of the intermediate 2, benzyltriethylammonium chloride, anhydrous ethanol, epichlorohydrin and potassium hydroxide solution in step s3 is 10 mmol: 0.01-0.05 g: 50-60 mL: 64-68 mmol: 10-12 mL.
[0020] As a further solution of the present invention: the mass fraction of the potassium hydroxide solution in step s3 is 35-40%.
[0021] As a further solution of the present invention: the usage ratio of the intermediate 3, hexafluoroisopropanol, aluminum phosphotungstate and anhydrous toluene in step s4 is 10 mmol: 15-25 mmol: 0.1-0.2 g: 60-80 mL.
[0022] As a further solution of the present invention: the mass fraction of the sodium bicarbonate solution in step s4 is 10-15%.
[0023] Beneficial effects of the present invention:
[0024] The invention discloses a process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste. The process comprises the following steps: uniformly mixing coal gangue, cement, quicklime, kaolin, basalt, a water-blocking modifier, a water-reducing agent, an early strength agent, a defoaming agent and water, and then subjecting the mixture to wet ball milling to obtain a mixed slurry. The mixed slurry is then poured into a mold to form a floor tile body, and then the floor tile body is subjected to constant-pressure steam curing to obtain a high-strength floor tile. The process utilizes coal gangue solid waste as a main raw material for comprehensive utilization to prepare high-strength floor tiles, thereby achieving effective utilization of coal gangue solid waste, reducing environmental pollution and waste of resources, and conforming to the concept of sustainable development. Moreover, by optimizing the process and raw material ratio, the production cost is reduced, the market competitiveness of the product is improved, and the product has good economic and social benefits. The prepared floor tiles have the advantages of high strength, high wear resistance and good waterproof performance, meet the high requirements of modern buildings on material performance, and can be widely used in the field of architectural decoration.
[0025] In the process of preparing high-strength floor tiles, a water-blocking modifier is first prepared. First, 1,1,5,5-tetramethyl-3,3-diphenyltrisiloxane and allylamine are reacted. Si-H on 1,1,5,5-tetramethyl-3,3-diphenyltrisiloxane reacts with the alkenyl group on allylamine to introduce amino groups to obtain intermediate 1. Then, intermediate 1 and 2,3,4-trihydroxybenzaldehyde are reacted. The amino groups on intermediate 1 react with the aldehyde groups on 2,3,4-trihydroxybenzaldehyde to form a hydrosilylation reaction. The intermediate 2 is then reacted with epichlorohydrin to form a Schiff base structure, and a large number of hydroxyl groups are introduced to obtain intermediate 2. The intermediate 2 is then reacted with epichlorohydrin, and the hydroxyl groups on the intermediate 2 react with epichlorohydrin to undergo ring-opening and ring-closing reactions, and epoxy groups are introduced to obtain intermediate 3. Finally, the intermediate 3 is reacted with hexafluoroisopropanol, and part of the epoxy groups on the intermediate 3 react with the hydroxyl groups on the hexafluoroisopropanol to introduce a large number of fluorine elements to obtain a water-blocking modifier. The water-blocking modifier contains an organic silicon structure, and the presence of organic silicon can be on the surface of high-strength floor tiles. A smooth and continuous hydrophobic film is formed, which significantly reduces the surface energy and makes it difficult for water molecules to adhere. The introduction of a large amount of fluorine elements can reduce the surface energy, so that the waterproof performance of the hydrophobic film can be further improved. A double waterproof barrier is constructed on the surface of the high-strength floor tile, which can effectively isolate the erosion of water and oxygen to the high-strength floor tile, slow down the weathering process of the high-strength floor tile, and improve its weather resistance and durability. In addition, the molecular structure of the water-blocking modifier contains a large number of epoxy groups. The presence of epoxy groups can react chemically with certain active groups (such as hydroxyl, carboxyl, and amino) in the high-strength floor tile to form a stable chemical bond, which not only enhances the binding force between the particles of the various components of the high-strength floor tile, fills the micropores and cracks in the high-strength floor tile, and reduces internal defects, thereby significantly improving the compressive strength and wear resistance of the floor tile, but also makes the water-blocking modifier more firmly attached to the surface of the high-strength floor tile stone, not easy to fall off, thereby maintaining its waterproof effect for a long time, so that the high-strength floor tile can maintain high performance for a long time, and extend the service life of the high-strength floor tile. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Embodiment 1:
[0028] This embodiment is a process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste, comprising the following steps:
[0029] Step S1: 10 mmol 1,1,5,5-tetramethyl-3,3-diphenyltrisiloxane, 11 mmol allylamine, 0.01 g chloroplatinic acid and 40 mL anhydrous tetrahydrofuran were added to a three-necked flask equipped with a stirrer, a thermometer and a gas guide tube, and nitrogen was introduced for protection. The mixture was stirred at 20° C. and a stirring rate of 300 r / min for 20 min, and then the temperature was raised to 60° C. and the stirring reaction was continued for 3 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain intermediate 1;
[0030] Step S2: 10 mmol of intermediate 1, 22 mmol of 2,3,4-trihydroxybenzaldehyde and 40 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer and an air duct, and nitrogen was introduced for protection. The reaction was stirred for 20 min at a temperature of 20° C. and a stirring rate of 300 r / min, and then the temperature was raised to 60° C. and the stirring reaction was continued for 6 h. After the reaction was completed, the reaction product was cooled to room temperature, poured into ice water, and then allowed to stand for precipitation, and then vacuum filtered. The filter cake was washed twice with distilled water, and then placed in a vacuum drying oven and dried at a temperature of 50° C. for 3 h to obtain intermediate 2;
[0031] Step S3: 10 mmol of intermediate 2, 0.01 g of benzyltriethylammonium chloride and 50 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a constant pressure dropping funnel, and nitrogen was introduced for protection. The mixture was stirred for 10 min at a temperature of 20 ° C and a stirring rate of 300 r / min. Then, 64 mmol of epichlorohydrin was added dropwise while stirring, and the dropping rate was controlled to be 1 drop / s. After the addition was completed, the mixture was heated to 70 ° C and continued to stir for 7 h. After the addition was completed, the mixture was cooled to 30 ° C and continued to stir for 10 min. Then, 10 mL of a 3% potassium hydroxide solution was added dropwise while stirring, and the dropping rate was controlled to be 1 drop / s. After the addition was completed, the mixture was heated to 60 ° C and continued to stir for 6 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 3;
[0032] Step S4: 10 mmol of intermediate 3, 15 mmol of hexafluoroisopropanol, 0.1 g of aluminum phosphotungstate and 60 mL of anhydrous toluene were added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen was introduced for protection. The reaction was stirred for 20 min at a temperature of 20 ° C and a stirring rate of 300 r / min, and then the temperature was raised to 90 ° C and stirred for 6 h. After the reaction, the reaction product was cooled to room temperature, and then added to ethyl acetate, and then allowed to stand for stratification. The organic phase was washed twice with a 10% mass fraction of sodium bicarbonate solution and a saturated sodium chloride solution, and then dried with anhydrous magnesium sulfate, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain a water-blocking modifier;
[0033] Step S5: weigh 45 parts of coal gangue, 22 parts of cement, 8 parts of quicklime, 7 parts of kaolin, 11 parts of basalt, 2.5 parts of water-blocking modifier, 1.2 parts of water reducer, 1 part of early strength agent, 0.5 parts of defoamer and 51 parts of water according to weight parts, and set aside; the water reducer is SP401 polycarboxylic acid high-efficiency water reducer; the early strength agent is calcium chloride; the defoamer is BYK-A530 defoamer;
[0034] Step S6: uniformly mixing coal gangue, cement, quicklime, kaolin, basalt, water-blocking modifier, water-reducing agent, early strength agent, defoaming agent and water, and then wet-ball milling to obtain a mixed slurry;
[0035] Step S7: pour the mixed slurry into a mold to form a floor tile body, and then perform constant pressure steam curing on the floor tile body at a pressure of 15 MPa and a temperature of 170° C. for 10 hours to obtain a high-strength floor tile.
[0036] Embodiment 2:
[0037] This embodiment is a process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste, comprising the following steps:
[0038] Step S1: 10 mmol 1,1,5,5-tetramethyl-3,3-diphenyltrisiloxane, 12 mmol allylamine, 0.02 g chloroplatinic acid and 45 mL anhydrous tetrahydrofuran were added to a three-necked flask equipped with a stirrer, a thermometer and a gas guide tube, and nitrogen was introduced for protection. The mixture was stirred at 22° C. and a stirring rate of 350 r / min for 25 min, and then the temperature was raised to 62° C. and the stirring reaction was continued for 4 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain intermediate 1;
[0039] Step S2: 10 mmol of intermediate 1, 23 mmol of 2,3,4-trihydroxybenzaldehyde and 45 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer and an air duct, and nitrogen was introduced for protection. The reaction was stirred for 25 min at a temperature of 22° C. and a stirring rate of 350 r / min, and then the temperature was raised to 62° C. and the stirring reaction was continued for 7 h. After the reaction was completed, the reaction product was cooled to room temperature, poured into ice water, and then allowed to stand for precipitation, and then vacuum filtered. The filter cake was washed twice with distilled water, and then placed in a vacuum drying oven and dried at a temperature of 52° C. for 4 h to obtain intermediate 2;
[0040] Step S3: 10 mmol of intermediate 2, 0.03 g of benzyltriethylammonium chloride and 55 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a constant pressure dropping funnel, and nitrogen was introduced for protection. The reaction was stirred for 12 min at a temperature of 22 ° C and a stirring rate of 350 r / min, and then 66 mmol of epichlorohydrin was added dropwise while stirring, and the dropping rate was controlled to be 1 drop / s. After the dropwise addition was completed, the temperature was raised to 72 ° C and the stirring reaction was continued for 7.5 h. After the temperature was cooled to 32 ° C, the stirring reaction was continued for 12 min. After that, 11 mL of a potassium hydroxide solution with a mass fraction of 38% was added dropwise while stirring, and the dropping rate was controlled to be 1 drop / s. After the dropwise addition was completed, the temperature was raised to 62 ° C and the stirring reaction was continued for 6.5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 3;
[0041] Step S4: 10 mmol of intermediate 3, 20 mmol of hexafluoroisopropanol, 0.15 g of aluminum phosphotungstate and 70 mL of anhydrous toluene were added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen was introduced for protection. The reaction was stirred for 25 min at a temperature of 22 ° C and a stirring rate of 350 r / min, and then the temperature was raised to 92 ° C and stirred for 7 h. After the reaction, the reaction product was cooled to room temperature, and then added to ethyl acetate, and then allowed to stand for stratification. The organic phase was washed twice with a sodium bicarbonate solution with a mass fraction of 12% and a saturated sodium chloride solution, and then dried with anhydrous magnesium sulfate, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain a water-blocking modifier;
[0042] Step S5: weigh 50 parts of coal gangue, 25 parts of cement, 10 parts of quicklime, 9 parts of kaolin, 14 parts of basalt, 6 parts of water-blocking modifier, 1.8 parts of water reducer, 2 parts of early strength agent, 0.7 parts of defoamer and 57 parts of water according to weight parts, and set aside; the water reducer is SP401 polycarboxylic acid high-efficiency water reducer; the early strength agent is triethanolamine; the defoamer is BYK-024 defoamer;
[0043] Step S6: uniformly mixing coal gangue, cement, quicklime, kaolin, basalt, water-blocking modifier, water-reducing agent, early strength agent, defoaming agent and water, and then wet-ball milling to obtain a mixed slurry;
[0044] Step S7: pour the mixed slurry into a mold to form a floor tile body, and then perform constant pressure steam curing on the floor tile body at a pressure of 18 MPa and a temperature of 175° C. for 11 hours to obtain a high-strength floor tile.
[0045] Embodiment 3:
[0046] This embodiment is a process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste, comprising the following steps:
[0047] Step S1: 10 mmol 1,1,5,5-tetramethyl-3,3-diphenyltrisiloxane, 13 mmol allylamine, 0.03 g chloroplatinic acid and 50 mL anhydrous tetrahydrofuran were added to a three-necked flask equipped with a stirrer, a thermometer and a gas guide tube, and nitrogen was introduced for protection. The mixture was stirred at 25° C. and a stirring rate of 400 r / min for 30 min, and then the temperature was raised to 65° C. and the stirring reaction was continued for 5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain intermediate 1;
[0048] Step S2: 10 mmol of intermediate 1, 25 mmol of 2,3,4-trihydroxybenzaldehyde and 50 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer and an air duct, and nitrogen was introduced for protection. The mixture was stirred at 25° C. and a stirring rate of 400 r / min for 30 min, and then the mixture was heated to 65° C. and the stirring reaction was continued for 8 h. After the reaction was completed, the reaction product was cooled to room temperature, poured into ice water, and then allowed to stand for precipitation, and then vacuum filtered. The filter cake was washed with distilled water 3 times, and then placed in a vacuum drying oven and dried at 55° C. for 5 h to obtain intermediate 2;
[0049] Step S3: 10 mmol of intermediate 2, 0.05 g of benzyltriethylammonium chloride and 60 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a constant pressure dropping funnel, and nitrogen was introduced for protection. The reaction was stirred for 15 min at a temperature of 25 ° C and a stirring rate of 400 r / min. Then, 68 mmol of epichlorohydrin was added dropwise while stirring, and the dropping rate was controlled to 2 drops / s. After the addition was completed, the temperature was raised to 75 ° C and the stirring reaction was continued for 8 h. After that, the temperature was cooled to 35 ° C and the stirring reaction was continued for 15 min. Then, 12 mL of a 40% potassium hydroxide solution was added dropwise while stirring, and the dropping rate was controlled to 2 drops / s. After the addition was completed, the temperature was raised to 65 ° C and the stirring reaction was continued for 7 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 3;
[0050] Step S4: 10 mmol of intermediate 3, 25 mmol of hexafluoroisopropanol, 0.2 g of aluminum phosphotungstate and 80 mL of anhydrous toluene were added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen was introduced for protection. The reaction was stirred for 30 minutes at a temperature of 25°C and a stirring rate of 400 r / min, and then the temperature was raised to 95°C and the reaction was stirred for 8 hours. After the reaction was completed, the reaction product was cooled to room temperature, and then added to ethyl acetate, and then allowed to stand for stratification. The organic phase was washed three times with a sodium bicarbonate solution and a saturated sodium chloride solution with a mass fraction of 15%, and then dried with anhydrous magnesium sulfate. After vacuum filtration, the filtrate was rotary evaporated to remove the solvent to obtain a water-blocking modifier;
[0051] Step S5: weigh 55 parts of coal gangue, 28 parts of cement, 12 parts of quicklime, 11 parts of kaolin, 17 parts of basalt, 9.5 parts of water-blocking modifier, 2.4 parts of water reducer, 3 parts of early strength agent, 0.9 parts of defoamer and 63 parts of water according to weight parts, and set aside; the water reducer is high-efficiency water reducer 2651F; the early strength agent is triethanolamine; the defoamer is BYK-028 defoamer;
[0052] Step S6: uniformly mixing coal gangue, cement, quicklime, kaolin, basalt, water-blocking modifier, water-reducing agent, early strength agent, defoaming agent and water, and then wet-ball milling to obtain a mixed slurry;
[0053] Step S7: pour the mixed slurry into a mold to form a floor tile body, and then perform constant pressure steam curing on the floor tile body at a pressure of 20 MPa and a temperature of 180° C. for 12 hours to obtain a high-strength floor tile.
[0054] Comparative Example 1:
[0055] This comparative example is a process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste, comprising the following steps:
[0056] Step S1: weigh 55 parts of coal gangue, 28 parts of cement, 12 parts of quicklime, 11 parts of kaolin, 17 parts of basalt, 2.4 parts of water reducer, 3 parts of early strength agent, 0.9 parts of defoamer and 63 parts of water according to weight parts, and set aside; the water reducer is high-efficiency water reducer 2651F; the early strength agent is triethanolamine; the defoamer is BYK-028 defoamer;
[0057] Step S2: uniformly mixing coal gangue, cement, quicklime, kaolin, basalt, water reducing agent, early strength agent, defoaming agent and water, and then wet-ball milling to obtain a mixed slurry;
[0058] Step S3: pour the mixed slurry into a mold to form a floor tile body, and then perform constant pressure steam curing on the floor tile body at a pressure of 20 MPa and a temperature of 180° C. for 12 hours to obtain a high-strength floor tile.
[0059] Comparative Example 2:
[0060] This comparative example is a process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste, comprising the following steps:
[0061] Step S1: weigh 55 parts of coal gangue, 28 parts of cement, 12 parts of quicklime, 11 parts of kaolin, 17 parts of basalt, 9.5 parts of 1,5,5-tetramethyl-3,3-diphenyltrisiloxane, 2.4 parts of water reducer, 3 parts of early strength agent, 0.9 parts of defoamer and 63 parts of water according to weight parts, and set aside; the water reducer is high-efficiency water reducer 2651F; the early strength agent is triethanolamine; the defoamer is BYK-028 defoamer;
[0062] Step S2: uniformly mixing coal gangue, cement, quicklime, kaolin, basalt, 1,5,5-tetramethyl-3,3-diphenyltrisiloxane, a water reducing agent, an early strength agent, a defoaming agent and water, and then wet-ball milling to obtain a mixed slurry;
[0063] Step S3: pour the mixed slurry into a mold to form a floor tile body, and then perform constant pressure steam curing on the floor tile body at a pressure of 20 MPa and a temperature of 180° C. for 12 hours to obtain a high-strength floor tile.
[0064] Comparative Example 3:
[0065] This comparative example is a process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste, comprising the following steps:
[0066] Step S1: weigh 55 parts of coal gangue, 28 parts of cement, 12 parts of quicklime, 11 parts of kaolin, 17 parts of basalt, 9.5 parts of hexafluoroisopropanol, 2.4 parts of water reducer, 3 parts of early strength agent, 0.9 parts of defoamer and 63 parts of water according to weight parts, and set aside; the water reducer is high-efficiency water reducer 2651F; the early strength agent is triethanolamine; the defoamer is BYK-028 defoamer;
[0067] Step S2: uniformly mixing coal gangue, cement, quicklime, kaolin, basalt, hexafluoroisopropanol, water reducing agent, early strength agent, defoaming agent and water, and then wet-ball milling to obtain a mixed slurry;
[0068] Step S3: pour the mixed slurry into a mold to form a floor tile body, and then perform constant pressure steam curing on the floor tile body at a pressure of 20 MPa and a temperature of 180° C. for 12 hours to obtain a high-strength floor tile.
[0069] The high-strength floor tiles of Examples 1-3 and Comparative Examples 1-3 were tested, and the test results are shown in the following table:
[0070]
[0071] Referring to the data in the above table, based on the comparison between Examples 1-3 and Comparative Examples 1-3, it can be known that adding a water-blocking modifier can significantly improve the hydrophobic and water-blocking properties of high-strength floor tiles, while also improving the mechanical strength of high-strength floor tiles.
[0072] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0073] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste, characterized in that: The following steps are involved: Step 1: Weigh 45-55 parts of coal gangue, 22-28 parts of cement, 8-12 parts of quicklime, 7-11 parts of kaolin, 11-17 parts of basalt, 2.5-9.5 parts of water-blocking modifier, 1.2-2.4 parts of water reducer, 1-3 parts of early strength agent, 0.5-0.9 parts of defoaming agent and 51-63 parts of water according to weight, and set aside; Step 2: Evenly mix the coal gangue, cement, quicklime, kaolin, basalt, water-blocking modifier, water-reducing agent, early strength agent, defoaming agent and water, and then wet-ball mill to obtain a mixed slurry; Step 3: Pour the mixed slurry into a mold to form a floor tile body, and then cure the floor tile body with constant pressure steam at a pressure of 15-20 MPa and a temperature of 170-180°C for 10-12 hours to obtain a high-strength floor tile; Wherein, the water blocking modifier is prepared by the following steps: Step s1: stirring 1,1,5,5-tetramethyl-3,3-diphenyltrisiloxane, allylamine, chloroplatinic acid and anhydrous tetrahydrofuran for reaction, cooling the reaction product after the reaction is completed, and then rotary evaporating to obtain intermediate 1; Step s2: stirring the intermediate 1, 2,3,4-trihydroxybenzaldehyde and anhydrous ethanol to react, cooling the reaction product after the reaction, then pouring it into ice water, then standing it to precipitate, then vacuum filtering it, washing the filter cake and drying it to obtain the intermediate 2; Step s3: stirring the intermediate 2, benzyltriethylammonium chloride and anhydrous ethanol for reaction, then adding epichlorohydrin dropwise while stirring, continuing to stir the reaction after the addition is complete, then cooling and adding potassium hydroxide solution dropwise while stirring, continuing to stir the reaction after the addition is complete, cooling the reaction product after the reaction is complete, then vacuum filtering, and rotary evaporating the filtrate to obtain the intermediate 3; Step s4: Stir the intermediate 3, hexafluoroisopropanol, aluminum phosphotungstate and anhydrous toluene for reaction. After the reaction, cool the reaction product and then add it to ethyl acetate. Let it stand for stratification. Wash the organic phase with sodium bicarbonate solution and saturated sodium chloride solution in turn, dry it, and then vacuum filter it. Rotary evaporate the filtrate to obtain a water-blocking modifier.
2. The process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste according to claim 1, characterized in that: The water reducer is one of SP401 polycarboxylic acid high-efficiency water reducer and high-efficiency water reducer 2651F.
3. The process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste according to claim 1, characterized in that: The early strength agent is one of calcium chloride and triethanolamine.
4. The process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste according to claim 1, characterized in that: The defoamer is one of byk-a530 defoamer, byk-024 defoamer and byk-028 defoamer.
5. The process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste according to claim 1, characterized in that: The usage ratio of the 1,1,5,5-tetramethyl-3,3-diphenyltrisiloxane, allylamine, chloroplatinic acid and anhydrous tetrahydrofuran in step s1 is 10 mmol: 11-13 mmol: 0.01-0.03 g: 40-50 mL.
6. The process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste according to claim 1, characterized in that: The usage ratio of the intermediate 1, 2,3,4-trihydroxybenzaldehyde and anhydrous ethanol in step s2 is 10mmol:22-25mmol:40-50mL.
7. The process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste according to claim 1, characterized in that: The usage ratio of the intermediate 2, benzyltriethylammonium chloride, anhydrous ethanol, epichlorohydrin and potassium hydroxide solution in step s3 is 10mmol:0.01-0.05g:50-60mL:64-68mmol:10-12mL.
8. The process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste according to claim 1, characterized in that: The mass fraction of the potassium hydroxide solution in step s3 is 35-40%.
9. The process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste according to claim 1, characterized in that: The usage ratio of the intermediate 3, hexafluoroisopropanol, aluminum phosphotungstate and anhydrous toluene in step s4 is 10 mmol: 15-25 mmol: 0.1-0.2 g: 60-80 mL.
10. The process for preparing high-strength floor tiles by comprehensive utilization of coal gangue solid waste according to claim 1, characterized in that: The mass fraction of the sodium bicarbonate solution in step s4 is 10-15%.