Converter vanadium extraction smelting method for high-chromium vanadium-titanium molten iron

By adding materials containing alumina and iron oxides to the vanadium extraction process in the converter, the blowing process was optimized, which solved the problem of viscous vanadium slag in high-chromium vanadium-titanium molten iron, improved fluidity and smelting efficiency, and reduced costs.

CN118879975APending Publication Date: 2024-11-01CHINA IRON & STEEL RESEARCH INSTITUTE GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410922727.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the process of vanadium extraction from high-chromium vanadium-titanium molten iron in converter smelting, the vanadium slag is viscous, has poor fluidity, carries a large amount of iron, and has high smelting costs and long cycle.

Method used

In the vanadium extraction process in a converter, alumina-containing materials and iron oxide materials are added to control the oxygen lance position and oxygen consumption during the blowing process. The composition of vanadium slag is optimized by adjusting the furnace temperature and oxidation reaction through batch addition.

Benefits of technology

The melting temperature of vanadium slag was lowered, its fluidity was improved, the smelting cycle was shortened, the smelting cost was reduced, and the national standard requirements for the composition of vanadium slag were met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879975A_ABST
    Figure CN118879975A_ABST
Patent Text Reader

Abstract

The invention relates to a converter vanadium extraction smelting method for high-chromium vanadium-titanium molten iron, belongs to the technical field of ferrous metallurgy, and solves the technical problems that vanadium slag for smelting the high-chromium vanadium-titanium molten iron through converter vanadium extraction is thick, poor in fluidity and large in iron carrying amount, and semisteel smelting is high in cost and long in period. A converter vanadium extraction smelting method for high-chromium vanadium-titanium molten iron comprises the steps that S1, the high-chromium vanadium-titanium molten iron or vanadium-containing pig iron and the high-chromium vanadium-titanium molten iron are mixed into an oxygen top-blown converter; s2, after oxygen supply blowing is started, the materials containing the aluminum oxide are added in batches according to the proportion of the total amount of 6.1-13 kg / t, and adding is completed within 180 s after blowing is started; meanwhile, according to the temperature change in the furnace, the iron oxide material is added in batches according to the proportion of the total amount of 16.0-28.0 kg / t; and S3, after oxygen supply blowing is carried out for 280-360 s, tapping is carried out, and semisteel smelting is finished. By means of the method, the melting temperature of the vanadium slag is greatly reduced, and the fluidity of the molten pool of the vanadium extraction converter is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of iron and steel metallurgy, and particularly relates to a method for smelting vanadium from a high-chromium vanadium-titanium molten iron converter. Background Art

[0002] The converter vanadium extraction process is a molten iron pretreatment process that oxidizes the vanadium in the molten iron into vanadium slag before it enters the steelmaking process. It is also called pyrometallurgy or semi-steel smelting. During the blowing process, oxygen is blown into the molten iron to oxidize the vanadium in the molten iron. The generated V 2 O 3 Vanadium slag can be obtained by entering the slag phase together with the oxides of other easily oxidizable elements such as Si, Ti, Mn, Cr in the molten iron.

[0003] For chromium-containing vanadium-titanium magnetite with high chromium oxide content, Cr 2 O 3 The mass percentage of [Cr] is about 0.5%. The molten iron obtained by smelting this vanadium-titanium magnetite also has a relatively high chromium content, with the mass percentage of [Cr] in the molten iron exceeding 0.25%. Due to the inherent metallic properties of Cr, during the converter vanadium extraction process, most of the [Cr] in the molten iron will be oxidized together with [V] and enter the vanadium slag, thus making the (Cr) in the vanadium slag 2 O 3 ) mass percentage reaches more than 5%, which increases the melting point and viscosity of the vanadium slag, easily leading to the vanadium slag drying out, resulting in a relatively high content of metallic iron in the vanadium slag, which is generally about 25% of the mass of the vanadium slag.

[0004] In view of the semi-steel smelting of high-chromium vanadium-titanium hot metal, Chinese patent CN116121481A proposes "adding slag conditioning agent to the converter, the slag conditioning agent includes iron oxide balls and river sand", "the river sand includes 61-65% SiO 2 ", iron oxide balls contain 16.5-19% SiO 2 , that is, by increasing the SiO 2 The melting point of vanadium slag is reduced by reducing the content of phase, thereby greatly reducing the viscosity of the slag, and then reducing the content of iron in the slag. However, the technical effect of this patent is limited. Although it has been reduced, the iron content is still almost more than 20% of the mass percentage of vanadium slag.

[0005] Chinese patent CN104694698A adds slag adjusting agent in the process of extracting vanadium and chromium from high-chromium vanadium-chromium molten iron. The amount of slag adjusting agent added is positively correlated with the [V]+[Cr] content in the molten iron. The maximum amount added is 6kg / tFe. The main components of the slag adjusting agent include Al 2 O 3 , MgO and FeO, among which Al 2 O 30%~30%, MgO5~35%, Al 2 O 3 The total content of vanadium and chromium is controlled between 35% and 60%, and the embodiment of the patent controls the iron content of vanadium-chromium slag to less than 10%. However, the amount of coolant added per ton of iron in the patent is large, the oxygen blowing time is long, and the oxygen supply per ton of iron is large, which not only has a high semi-steel smelting cost, but also a long smelting cycle, which is not conducive to continuous operation. Summary of the invention

[0006] In view of the above technical problems, the present invention provides a method for vanadium extraction and smelting of high-chromium vanadium-titanium molten iron in a converter, which can solve at least one of the technical problems of vanadium slag being thick, poor in fluidity, and having a large amount of iron in the converter vanadium extraction and smelting of high-chromium vanadium-titanium molten iron, as well as high semi-steel smelting cost and long cycle.

[0007] The purpose of the present invention is mainly achieved through the following technical solutions:

[0008] The present invention provides a high-chromium vanadium-titanium molten iron converter vanadium extraction smelting method, comprising the following steps:

[0009] Step S1, adding high-chromium vanadium-titanium molten iron, or vanadium-containing pig iron blocks and high-chromium vanadium-titanium molten iron into an oxygen top-blown converter;

[0010] Step S2, after oxygen blowing starts, aluminum oxide materials are added in batches at a ratio of 6.1 to 13 kg / t of total charge, and the addition is completed within 180 seconds after blowing starts; at the same time, according to the temperature change in the furnace, iron oxide materials are added in batches at a ratio of 16.0 to 28.0 kg / t of total charge;

[0011] Step S3, after oxygen blowing for 280 to 360 seconds, steel is tapped, and semi-steel smelting is completed.

[0012] Furthermore, in step S1, the vanadium-containing pig iron block and the high-chromium vanadium-titanium molten iron have the same composition, which is as follows in terms of mass percentage: C3.86-4.36%, Si0.15-0.30%, Mn0.12-0.30%, P0.10-0.13%, S0.006-0.026%, Ti0.04-0.25%, Cr0.25-0.85%, V0.31-0.36%, and the remainder is Fe and unavoidable impurities.

[0013] Furthermore, in step S1, the temperature of the charge is controlled within the range of 1200-1300°C.

[0014] Further, in step S2, the main component of the alumina-containing material is 72-85% of Al 2 O 3 5~15% SiO 2 , particle size is 10~20mm.

[0015] Furthermore, in step S2, the main component of the iron oxide material is iron oxide, which contains 56.0-62.0% of Fe element in terms of mass percentage, and has a particle size of less than 5 mm.

[0016] Furthermore, in step S2, the oxygen lance position is controlled during the blowing process: from 0 to 120 seconds, the low lance position is controlled at 1.4 to 1.5 m; from 121 to 220 seconds, the high lance position is controlled at 1.55 to 1.6 m; and after 221 seconds, the low lance position is controlled at 1.2 to 1.3 m.

[0017] Furthermore, in step S2, the oxygen consumption is 11.0-14.0 Nm 3 / tLoading amount.

[0018] Furthermore, in step S3, the semi-steel components are as follows in terms of mass percentage: [C] ≥ 3.0%, [V] < 0.05%, [Cr] 0.07-0.25%, [Mn] 0.03-0.08%, [P] 0.10-0.13%, [S] 0.010-0.026%, the remainder being Fe and unavoidable impurities, and the semi-steel temperature is 1320-1398°C.

[0019] Furthermore, [C] is 3.0 to 3.9%, and [V] is 0.02 to 0.029%.

[0020] Furthermore, in step S3, the main components of the vanadium slag at the end of blowing are as follows: FeO20-25%, SiO 2 10~18%, V 2 O 3 10~20%,Al 2 O 3 16.1~25.0%, Cr 2 O 3 6~25%, MnO3~8%, TiO 2 3~12%, CaO1~5%, CaO / V 2 O 3 ≤0.25, MgO2~4%; in addition to the main components of vanadium slag, the weight of metallic iron M.Fe carried by vanadium slag is 4~15%.

[0021] Compared with the prior art, the present invention can achieve at least one of the following technical effects:

[0022] (1) The present invention adds alumina-containing materials during vanadium extraction and smelting in a converter, controls the alumina content of the vanadium slag at the end of blowing to be 16.1-25%, and the melting temperature of the vanadium slag is 1353° C. on average, ranging from 1345-1362° C., thereby greatly reducing the melting temperature of the vanadium slag and increasing the fluidity of the molten pool of the vanadium extraction converter.

[0023] (2) The converter vanadium smelting method of the present invention has an oxygen supply time of no more than 6 minutes, a short oxygen blowing time, a short smelting cycle, and is conducive to continuous operation.

[0024] (3) In the converter vanadium extraction and smelting method of the present invention, [C] in the final semi-steel is ≥3.0%, and [V] is <0.05%, thereby achieving the purpose of extracting vanadium and retaining carbon.

[0025] (4) The converter vanadium smelting method of the present invention, V in vanadium slag 2 O 3 10~20%、SiO 2 <24%、CaO / V 2 O 3 ≤0.25, M.Fe<19%, phosphorus-free, meeting the requirements of national standard YB / T008-2006 on vanadium slag composition. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference numerals refer to like components throughout the drawings.

[0027] Figure 1 Contains 18% Al 2 O 3 Thermal analysis diagram of vanadium slag;

[0028] Figure 2 Contains 23% Al 2 O 3 Thermal analysis diagram of vanadium slag;

[0029] Figure 3 Contains 6.7% Al 2 O 3 Thermal analysis diagram of vanadium slag;

[0030] Figure 4 Contains 4.5% Al 2 O 3 Thermal analysis diagram of vanadium slag. DETAILED DESCRIPTION

[0031] A method for extracting vanadium from a high-chromium vanadium-titanium hot metal converter is described in further detail below in conjunction with specific examples. These examples are only used for comparison and explanation purposes, and the present invention is not limited to these examples.

[0032] A high-chromium vanadium-titanium hot metal converter vanadium extraction smelting method comprises the following steps:

[0033] Step S1, adding high-chromium vanadium-titanium molten iron, or vanadium-containing pig iron blocks and high-chromium vanadium-titanium molten iron into an oxygen top-blown converter;

[0034] Step S2, after oxygen blowing starts, aluminum oxide materials are added in batches at a ratio of 6.1 to 13 kg / t of total charge, and the addition is completed within 180 seconds after blowing starts; at the same time, according to the temperature change in the furnace, iron oxide materials are added in batches at a ratio of 16.0 to 28.0 kg / t of total charge;

[0035] Step S3, after oxygen blowing for 280 to 360 seconds, steel is tapped, and semi-steel smelting is completed.

[0036] Specifically, in step S1, the vanadium-containing pig iron block and the high-chromium vanadium-titanium molten iron have the same composition, and the mass percentage is: C3.86-4.36%, Si0.15-0.30%, Mn0.12-0.30%, P0.10-0.13%, S0.006-0.026%, Ti0.04-0.25%, Cr0.25-0.85%, V0.31-0.36%, and the remainder is Fe and unavoidable impurities; the temperature of the charge is controlled within the range of 1200-1300°C through the proportioning of the vanadium-containing pig iron block and the high-chromium vanadium-titanium molten iron.

[0037] Specifically, in step S2, the main component of the alumina-containing material is 72-85% of Al 2 O 3 5~15% SiO 2 The particle size is 10-20 mm, the total addition amount is 6.1-13.0 kg / t, the loading amount is the total weight of the vanadium-containing pig iron block and the high-chromium vanadium-titanium molten iron, the alumina-containing material is added evenly in 2-3 batches, and the addition is completed within 180 seconds after the blowing starts; the alumina-containing material is added to increase the alumina content in the vanadium slag, adjust the composition of the vanadium slag, and reduce the melting point and viscosity of the vanadium slag.

[0038] The main component of the iron oxide material is iron oxide, which contains 56.0-62.0% of Fe element according to the mass percentage, has a particle size of less than 5 mm, and a total added amount of 16.0-28.0 kg / t of loading amount, which is the total weight of the vanadium-containing pig iron block and the high-chromium vanadium-titanium molten iron; the iron oxide material is used as a coolant in the smelting process, and is added in batches to control the slow rise of the furnace temperature so that the semi-steel temperature at the end of blowing is within the range of 1320-1398°C.

[0039] During the blowing process, the oxygen lance position is controlled at 1.4-1.5m from 0 to 120 seconds, the high lance position is controlled at 1.55-1.6m from 121 to 220 seconds, and the low lance position is controlled at 1.2-1.3m after 221 seconds. The oxygen consumption is 11.0-14.0Nm 3 / tLoading amount.

[0040] It should be noted that the existing converter vanadium extraction principle shows that due to the absolute advantage of Fe atomic concentration in molten iron, the main reaction mode is that oxygen first reacts with Fe atoms in molten iron to form FeO, and then FeO reacts with other elements in molten iron, such as Ti, Si, Mn, V, Cr, and C to form the corresponding oxidation product TiO 2 、SiO 2 、MnO、V 2 O 3 Cr 2 O 3 , CO. Thermodynamic data show that different elements have different affinities with oxygen. At the same temperature, there is a sequence of element oxidation. Metal oxidation is carried out in the order of Ti, Si, V, Mn, and Cr. The oxygen potential line of C and the oxygen potential line of other metal elements have opposite directions. The two must have an intersection. The temperature corresponding to the intersection is the exchange temperature of the metal and carbon oxidation sequence, that is, the conversion temperature of selective oxidation. Therefore, for the purpose of vanadium extraction and carbon preservation, the temperature of the molten iron in the vanadium extraction reaction process needs to be controlled as much as possible below the carbon-vanadium conversion temperature. The oxidation of Fe, Ti, Si, V, Mn, Cr, and C releases a lot of heat, so it is necessary to add a coolant, such as iron oxide material, to control the rise in the temperature of the molten iron. The existing converter vanadium extraction process shows that the semi-steel smelting temperature should be controlled below 1400°C.

[0041] In addition, the oxygen element in the iron oxide material added as a coolant also provides a part of the oxygen source for the oxidation of metal and carbon in the molten iron. This part of oxygen and the top-blown oxygen of the converter together constitute the amount of oxygen required for the oxidation reaction.

[0042] Specifically, in step S3, the semi-steel composition is as follows according to the mass percentage: [C] ≥ 3.0%, [V] < 0.05%, [Cr] 0.07-0.25%, [Mn] 0.03-0.08%, [P] 0.10-0.13%, [S] 0.010-0.026%, the balance is Fe and unavoidable impurities, and the semi-steel temperature is 1320-1398° C. In the semi-steel composition of the present invention, [C] ≥ 3.0%, preferably [C] 3.0-3.9%; [V] < 0.05%, preferably [V] 0.02-0.029%, which well achieves the purpose of extracting vanadium and retaining carbon.

[0043] The main components of the vanadium slag at the end of blowing are as follows: FeO20-25%, SiO 2 10~18%, V 2 O 3 10~20%,Al 2 O 3 16.1~25.0%, Cr 2 O 3 6~25%, MnO3~8%, TiO2 3~12%, CaO1~5%, CaO / V 2 O 3 ≤0.25, MgO2~4%; in addition, the weight of metallic iron carried by the vanadium slag in addition to the main components of the vanadium slag is 4~15% of the total weight of the vanadium slag, that is, M.Fe4~15%.

[0044] It should be noted that research shows that after vanadium extraction, C and V meet the requirements of the above-mentioned semi-steel composition, that is, when the oxidation rate of C is about 20% and the oxidation rate of V is about 90%, the remaining Ti and Si in the semi-steel are traces, that is, the oxidation rates of Ti and Si are close to 100%, the oxidation rate of Mn is about 75%, and the oxidation rate of Cr is about 70%. The oxidation products of these metals TiO 2 、SiO 2 、MnO、V 2 O 3 Cr 2 O 3 and FeO, as well as A1 added during slag adjustment 2 O 3 、SiO 2 Together they constitute the main components of vanadium slag after vanadium extraction.

[0045] According to the results of industrial tests, after adding alumina-containing materials, the Al content in vanadium slag can be controlled. 2 O 3 When the content of vanadium slag is 16.1-25.0%, the melting temperature of vanadium slag is 1353℃ on average, ranging from 1345℃ to 1362℃. 2 O 3 The melting temperature of vanadium slag with low vanadium content is 1494℃ on average, ranging from 1431℃ to 1516℃, which indicates that the fluidity of vanadium slag increases after adding alumina. Figure 1 Contains 18% Al 2 O 3 Thermoanalysis diagram of vanadium slag shows that the melting temperature of vanadium slag is 1351℃; Figure 2 Contains 23% Al 2 O 3 The thermal analysis diagram of vanadium slag shows that the melting temperature of vanadium slag is 1345℃; Figure 3 Contains 6.7% Al 2 O 3 The thermal analysis diagram of vanadium slag shows that the melting temperature of vanadium slag is 1500℃; Figure 4 Contains 4.5% Al 2 Thermal analysis diagram of O3 vanadium slag, the melting temperature of vanadium slag is 1512℃.

[0046] The existing silica slag-adjusting process shows that although it can also play a role in reducing the melting temperature and improving fluidity, the effect is limited. At the same time, it also increases the silica content in the vanadium slag, such as more than 25%. The national standard has an upper limit on the silica content in vanadium slag, which cannot exceed 24%. Therefore, the silica slag-adjusting agent cannot meet the national standard requirements for vanadium slag. The amount of existing alumina slag-adjusting agents added is limited, such as adding a maximum of 1.8kg / t of molten iron, which makes the alumina content in the final vanadium slag less than 16.1%, and the melting temperature of the vanadium slag is limited to drop, such as not lower than 1400℃, and there will be no good vanadium extraction effect.

[0047] The present invention reduces the high Cr content by adding alumina-containing materials in the converter vanadium extraction smelting. 2 O 3 The melting temperature of vanadium slag improves the fluidity of vanadium slag. After oxygen blowing smelting for no more than 6 minutes, the semi-steel composition achieves the purpose of extracting vanadium and retaining carbon. Not only is the smelting efficiency high, but also the V in vanadium slag is 2 O 3 10~20%、SiO 2 <24%、CaO / V 2 O 3 ≤0.25, M.Fe<19%, phosphorus-free, meeting the requirements of national standard YB / T008-2006 on vanadium slag composition.

[0048] Example 1

[0049] A high-chromium vanadium-titanium hot metal converter vanadium extraction smelting method:

[0050] Step S1, adding 85 tons of high chromium vanadium titanium molten iron into an oxygen top-blown converter with a nominal capacity of 80t; the composition of the high chromium vanadium titanium molten iron is as follows in terms of mass percentage: C3.86%, Si0.15%, Mn0.12%, P0.10%, S0.006%, Ti0.04%, Cr0.25%, V0.31%, and the remainder is Fe and unavoidable impurities; the temperature of the molten iron entering the furnace is 1200°C.

[0051] Step S2, after oxygen blowing starts, the alumina material is added in two batches at a total amount of 6.1 kg / t, 259.25 kg is added when blowing starts, and 259.25 kg is added after 180 seconds of blowing. The iron oxide material is added in three batches at a total amount of 16.0 kg / t, 200 kg is added when blowing starts, 580 kg is added after 100 seconds of blowing, and 580 kg is added after 200 seconds of blowing. The oxygen gun position is controlled during the blowing process, 0 to 120 seconds, the low gun position is controlled at 1.4 m; 121 to 220 seconds, the high gun position is controlled at 1.55 m; after 221 seconds, the low gun position is controlled at 1.2 m. The oxygen consumption is 11.0 Nm3 / t loading amount, i.e. 935Nm 3 ;

[0052] According to the mass percentage, the main component of the alumina-containing material is 72% A1 2 O 3 , 15% SiO 2 , the particle size is 10-20mm; the main component of the iron oxide material is iron oxide, which contains 56.0% Fe element according to the mass percentage, and the particle size is less than 5mm.

[0053] Step S3, after oxygen blowing for 280s, steel is tapped, and semi-steel smelting is completed.

[0054] The semi-steel composition is as follows: [C] 3.0%, [V] 0.02%, [Cr] 0.07%, [Mn] 0.03%, [P] 0.10%, [S] 0.010%, the remainder is Fe and unavoidable impurities, and the semi-steel temperature is 1320°C; the main components of the vanadium slag are as follows: FeO 25%, SiO 2 10%, V 2 O 3 20%, Al 2 O 3 16.1%,Cr 2 O 3 6%, MnO5%, TiO 2 9.9%, CaO4%, CaO / V 2 O 3 =0.2, MgO4%; in addition, the weight of metallic iron carried by the vanadium slag in addition to the main components of the vanadium slag is 15% of the total weight of the vanadium slag, that is, M.Fe15%.

[0055] Example 2

[0056] A high-chromium vanadium-titanium hot metal converter vanadium extraction smelting method:

[0057] Step S1, adding 80 tons of high chromium vanadium titanium molten iron and 10 tons of vanadium-containing pig iron blocks into an oxygen top-blown converter with a nominal capacity of 80t; the components of the high chromium vanadium titanium molten iron and the vanadium-containing pig iron blocks are as follows in terms of mass percentage: C4.36%, Si0.30%, Mn0.30%, P0.13%, S0.026%, Ti0.25%, Cr0.85%, V0.36%, and the remainder is Fe and unavoidable impurities; the charging temperature is 1300°C.

[0058] Step S2, after oxygen blowing starts, the alumina-containing material is added in three batches at a total amount of 13kg / t, 390kg is added when blowing starts, 390kg is added after 90s of blowing, and 390kg is added after 180s of blowing; the iron oxide material is added in two batches at a total amount of 28kg / t, 1500kg is added when blowing starts, and 1020kg is added after 200s of blowing; the oxygen lance position is controlled during the blowing process, 0-120 seconds, the low lance position is controlled at 1.5m; 121-220 seconds, the high lance position is controlled at 1.6m; after 221 seconds, the low lance position is controlled at 1.3m. The oxygen consumption is 14.0Nm 3 / t loading amount, i.e. 1260Nm 3 ;

[0059] According to the mass percentage, the main component of the alumina-containing material is 85% A1 2 O 3 , 5% SiO 2 , the particle size is 10-20mm; the main component of the iron oxide material is iron oxide, which contains 62.0% Fe element according to the mass percentage, and the particle size is less than 5mm.

[0060] Step S3, after oxygen blowing for 360s, steel is tapped, and semi-steel smelting is completed.

[0061] The semi-steel composition is as follows: [C] 3.9%, [V] 0.029%, [Cr] 0.25%, [Mn] 0.08%, [P] 0.13%, [S] 0.026%, the remainder is Fe and unavoidable impurities, and the semi-steel temperature is 1398°C; the main components of the vanadium slag are as follows: FeO 20%, SiO 2 15%, V 2 O 3 10%,Al 2 O 3 19%, Cr 2 O 3 25%, MnO3%, TiO 2 5%, CaO1%, CaO / V 2 O 3 =0.1, MgO2%; in addition, the weight of metallic iron carried by the vanadium slag in addition to the main components of the vanadium slag is 4% of the total weight of the vanadium slag, that is, M.Fe4%.

[0062] Example 3

[0063] A high-chromium vanadium-titanium hot metal converter vanadium extraction smelting method:

[0064] Step S1, adding 130 tons of high chromium vanadium titanium molten iron into an oxygen top-blown converter with a nominal capacity of 120t; the composition of the high chromium vanadium titanium molten iron is as follows in terms of mass percentage: C4.11%, Si0.225%, Mn0.21%, P0.115%, S0.016%, Ti0.145%, Cr0.55%, V0.335%, and the remainder is Fe and unavoidable impurities; the temperature of the molten iron entering the furnace is 1250°C.

[0065] Step S2, after oxygen blowing starts, the alumina material is added in two batches at a ratio of 9.5 kg / t of total charge, 617.5 kg is added when blowing starts, and 617.5 kg is added after 180 seconds of blowing; the iron oxide material is added in three batches at a ratio of 22.0 kg / t of total charge, 953 kg is added when blowing starts, 953 kg is added after 100 seconds of blowing, and 954 kg is added after 200 seconds of blowing; the oxygen lance position is controlled during the blowing process, 0 to 120 seconds, the low lance position is controlled at 1.45m; 121 to 220 seconds, the high lance position is controlled at 1.57m; after 221 seconds, the low lance position is controlled at 1.25m. The oxygen consumption is 12.5Nm 3 / t loading amount, i.e. 1625Nm 3 ;

[0066] According to the mass percentage, the main component of the alumina-containing material is 78.5% A1 2 O 3 , 10% SiO 2 , the particle size is 10-20mm; the main component of the iron oxide material is iron oxide, which contains 58.0% Fe element according to the mass percentage, and the particle size is less than 5mm.

[0067] Step S3, after oxygen blowing for 320s, steel is tapped, and semi-steel smelting is completed.

[0068] The semi-steel composition is as follows: [C] 3.45%, [V] 0.025%, [Cr] 0.16%, [Mn] 0.055%, [P] 0.115%, [S] 0.018%, the remainder is Fe and unavoidable impurities, and the semi-steel temperature is 1359°C; the main components of the vanadium slag are as follows: FeO 21%, SiO 2 18%, V 2 O 3 15%, Al 2 O 3 25%, Cr 2 O 3 10%, MnO3%, TiO 2 3%, CaO2%, CaO / V 2 O 3=0.13, MgO3%; in addition, the weight of metallic iron carried by the vanadium slag in addition to the main components of the vanadium slag is 10% of the total weight of the vanadium slag, that is, M.Fe10%.

[0069] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A high-chromium vanadium-titanium hot metal converter vanadium extraction smelting method, characterized in that: The method comprises the following steps: Step S1, adding high-chromium vanadium-titanium molten iron, or vanadium-containing pig iron blocks and high-chromium vanadium-titanium molten iron into an oxygen top-blown converter; Step S2, after oxygen blowing starts, aluminum oxide materials are added in batches at a ratio of 6.1 to 13 kg / t of total charge, and the addition is completed within 180 seconds after blowing starts; at the same time, according to the temperature change in the furnace, iron oxide materials are added in batches at a ratio of 16.0 to 28.0 kg / t of total charge; Step S3, after oxygen blowing for 280 to 360 seconds, steel is tapped, and semi-steel smelting is completed.

2. The method according to claim 1, characterized in that: In the step S1, the vanadium-containing pig iron block and the high-chromium vanadium-titanium molten iron have the same composition, which is as follows in terms of mass percentage: C3.86-4.36%, Si0.15-0.30%, Mn0.12-0.30%, P0.10-0.13%, S0.006-0.026%, Ti0.04-0.25%, Cr0.25-0.85%, V0.31-0.36%, and the remainder is Fe and unavoidable impurities.

3. The method according to claim 1, characterized in that: In the step S1, the temperature of the charge is controlled within the range of 1200-1300°C.

4. The method according to claim 1, characterized in that: In the step S2, the main components of the alumina-containing material are 72-85% of Al2O3 and 5-15% of SiO2 in terms of mass percentage, and the particle size is 10-20 mm.

5. The method according to claim 1, characterized in that In the step S2, the main component of the iron oxide material is iron oxide, which contains 56.0-62.0% of Fe element in terms of mass percentage and has a particle size of less than 5 mm.

6. The method according to claim 1, characterized in that In step S2, the oxygen lance position is controlled during the blowing process: from 0 to 120 seconds, the low lance position is controlled at 1.4 to 1.5 m; from 121 to 220 seconds, the high lance position is controlled at 1.55 to 1.6 m; and after 221 seconds, the low lance position is controlled at 1.2 to 1.3 m.

7. The method according to claim 1, characterized in that In step S2, the oxygen consumption is 11.0-14.0 Nm 3 / tLoading amount.

8. The method according to claim 1, characterized in that In step S3, the semi-steel components are as follows in terms of mass percentage: [C] ≥ 3.0%, [V] < 0.05%, [Cr] 0.07-0.25%, [Mn] 0.03-0.08%, [P] 0.10-0.13%, [S] 0.010-0.026%, the remainder being Fe and unavoidable impurities, and the semi-steel temperature is 1320-1398°C.

9. The method according to claim 8, characterized in that The [C] is 3.0 to 3.9%, and the [V] is 0.02 to 0.029%.

10. The method according to claim 1, characterized in that In the step S3, the main components of the vanadium slag at the end of blowing are as follows in terms of mass percentage: FeO20-25%, SiO210-18%, V2O310-20%, Al2O316.1-25.0%, Cr2O36-25%, MnO3-8%, TiO23-12%, CaO1-5%, CaO / V2O3≤0.25, MgO2-4%; in addition to the main components of the vanadium slag, the weight of metallic iron M.Fe carried by the vanadium slag is 4-15%.