Alloy particles, dust core, electronic component, electronic device, motor, and generator
By controlling the peak intensity ratio of FeO and Fe2SiO4 in the cover part of the alloy particles, the FeO content is reduced and the Fe2SiO4 content is improved, the eddy current loss and strength problems of the powdered magnetic core are solved, and more efficient core performance is achieved.
Patent Information
- Application Number
- CN202380028023.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-12-21
- Filing Date
- 2023-08-18
- Publication Date
- 2024-11-01
AI Technical Summary
The eddy current loss of the powdered magnetic core composed of conventional alloy particles is insufficient and has low strength.
The alloy particles formed of iron and silicon are formed by the cover part of the film containing Fe2SiO4. The strongest peak intensity ratio of FeO is ensured by X-ray diffraction measurement to be 0.2 or less of the strongest peak intensity of Fe2SiO4. The cover part is formed to reduce the FeO content and increase the Fe2SiO4 content, thereby reducing eddy current loss and increasing strength.
It has achieved a reduction in eddy current loss and an increase in strength, and is suitable for applications such as electronic components and motors.
Smart Images

Figure CN118891692A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to alloy particles, powder magnetic cores, electronic components, electronic devices, motors, and generators. Background Art
[0002] The alloy particles constituting the powder magnetic core disclosed in Patent Document 1 include soft magnetic particles containing Fe and a grain boundary layer between adjacent soft magnetic particles. The compound layer included in the cover layer is formed by reacting a silicone resin with a ferrite plating layer.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2019-75566 Summary of the invention
[0006] Problem that the invention aims to solve
[0007] However, the dust core composed of the alloy particles of Patent Document 1 does not sufficiently reduce the eddy current loss and also has low strength.
[0008] The present disclosure is made in view of the above-mentioned actual situation, and an object of the present disclosure is to provide alloy particles constituting a powder magnetic core having low eddy current loss and high strength. The present disclosure can be implemented in the following manner.
[0009] Solutions for solving problems
[0010] [1] An alloy particle comprising: a core portion formed of an alloy containing iron and silicon; and a covering portion covering the core portion;
[0011] The aforementioned covering portion contains Fe2SiO4,
[0012] The coating portion is measured by X-ray diffraction.
[0013] The strongest peak intensity of FeO is set as IA,
[0014] When the strongest peak intensity of the above-mentioned Fe2SiO4 is set to IB,
[0015] The value of the peak intensity ratio (IA / IB) is 0.2 or less.
[0016] [2] A powder magnetic core comprising a plurality of alloy particles as described in [1].
[0017] [3] An electronic component comprising the powder magnetic core described in [2].
[0018] [4] The electronic component according to [3], comprising a powder magnetic core and a coil.
[0019] [5] An electronic device comprising the electronic component described in [3] or [4].
[0020] [6] An electric motor comprising the powder magnetic core described in [2].
[0021] [7] A generator comprising the powder magnetic core described in [2].
[0022] Effects of the Invention
[0023] The alloy particles disclosed herein can provide alloy particles with low eddy current loss and high strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram showing a cross section of the powder magnetic core of the present embodiment.
[0025] Figure 2 This is a diagram showing the results of XRD measurement of the alloy particles according to the present embodiment.
[0026] Figure 3 Schematic diagram of an inductor using the powder magnetic core according to the present embodiment.
[0027] Figure 4 Schematic diagram of an inductor using the powder magnetic core according to the present embodiment.
[0028] Figure 5 Schematic diagram of an inductor using the powder magnetic core according to the present embodiment.
[0029] Figure 6 This is a schematic diagram of a noise filter using the powder magnetic core of this embodiment.
[0030] Figure 7 Schematic diagram of a reactor using the powder magnetic core according to the present embodiment.
[0031] Figure 8 Schematic diagram of a transformer using the powder magnetic core of this embodiment.
[0032] Fig. 9 This is a circuit diagram of a noise filter using the powder magnetic core of this embodiment.
[0033] Fig.10 This is a schematic diagram of a motor using the powder magnetic core of this embodiment.
[0034] Fig.11 This is a schematic diagram of a generator using the powder magnetic core according to the present embodiment. DETAILED DESCRIPTION
[0035] Hereinafter, the present disclosure will be described in detail. It should be noted that, in this specification, for numerical ranges, the description using "-" includes lower limits and upper limits unless otherwise specified. For example, the description of "10-20" includes "10" as the lower limit and "20" as the upper limit. That is, "10-20" and "10 or more and 20 or less" have the same meaning. In addition, in this specification, the upper limit and lower limit of each numerical range can be arbitrarily combined.
[0036] 1. Alloy particles 5
[0037] (1) Composition of Alloy Particles 5
[0038] like Figure 1 As shown, the alloy particle 5 includes: a core portion 1 and a coating portion 3 formed on the surface of the core portion 1. The coating portion 3 contains Fe2SiO4. For the alloy particle 5 disclosed herein, when the coating portion 3 is measured by XRD (X-ray diffraction) at 25°C, the peak intensity ratio (IA / IB) of the strongest peak intensity IA of FeO to the strongest peak intensity IB of Fe2SiO4 is 0.2 or less.
[0039] The powder magnetic core 7 of the present disclosure is produced, for example, by press-molding the alloy particles 5. The powder magnetic core 7 includes a plurality of alloy particles 5.
[0040] (2) Core 1
[0041] The core 1 is a soft magnetic metal particle containing iron and silicon. As the core 1, particles of soft magnetic iron-based alloys can be widely used. As iron-based alloys, Fe-Si alloys, Fe-Si-Cr alloys, and Fe-Si-Al alloys (Sendisilicon aluminum alloys) can be suitably used. Among these, Fe-Si alloys, Fe-Si-Cr alloys, and Fe-Si-Al alloys (Sendisilicon aluminum alloys) are preferred from the viewpoints of magnetic permeability, coercive force, and frequency characteristics.
[0042] When using an Fe—Si alloy, for example, an alloy having a composition of Si: 1 mass % to 10 mass % and the balance: Fe and inevitable impurities can be used.
[0043] When using a Fe—Si—Cr alloy, for example, an alloy having a composition of 1 mass % to 10 mass % Si, 10 mass % to 20 mass % Cr, and the balance of Fe and inevitable impurities can be used.
[0044] The average particle size of the core 1 is not particularly limited. The average particle size of the core 1 is preferably 10 μm or more and 70 μm or less, more preferably 10 μm or more and 50 μm or less, and further preferably 10 μm or more and 40 μm or less. The average particle size of the core 1 can be appropriately changed according to the frequency band used. In particular, when it is envisaged to be used in a high frequency band exceeding 500 kHz, it is preferably 10 μm or more and 50 μm or less.
[0045] The average particle size of the core 1 is as follows: the area equivalent circle diameter is calculated based on the particle area obtained by observing the cross section of the compressed magnetic core 7 by FE-SEM (field emission scanning electron microscope), and is used as the average particle size. Specifically, the average circle equivalent diameter is calculated as follows. In a specified observation field of view (for example, 200μm×200μm), focus on multiple cores 1 that can be observed without defects. Calculate the diameter (area circle equivalent diameter) of an ideal circle (true circle) having an area equal to the area (projected area) of each particle image of the core 1 as the circle equivalent diameter of each particle. Then, the circle equivalent diameter of each particle is arithmetic averaged to obtain the average circle equivalent diameter. Here, the average circle equivalent diameter is equivalent to the average particle size. The circle equivalent diameter of each particle and the average circle equivalent diameter can be obtained using general image analysis software.
[0046] (3) Covering part 3
[0047] The thickness of coating 3 is not particularly limited. In order to ensure sufficient strength and relative magnetic permeability, the thickness of coating 3 is preferably 0.01 μm to 1 μm. The thickness of coating 3 is preferably 0.015% to 10% of the average particle size of core 1.
[0048] The thickness of the coating 3 can be measured by cutting the alloy particle 5 and observing the cross section using a TEM (transmission electron microscope) or a SEM (scanning electron microscope). The thickness of the coating 3 is measured at 10 or more measurement points and the average value is taken as the thickness of the coating 3 .
[0049] (4) Peak intensity ratio (IA / IB)
[0050] (4.1) Peak intensity ratio (IA / IB) value
[0051] In the alloy particles 5, for the coating portion 3, when the oxide is measured by XRD at 25°C, the peak intensity ratio (IA / IB) of the strongest peak intensity IA of FeO to the strongest peak intensity IB of Fe2SiO4 is less than 0.2, preferably less than 0.14, and more preferably less than 0.09.
[0052] Setting the peak intensity ratio (IA / IB) to a value of 0.2 or less is an indicator that a large amount of Fe2SiO4 is contained in the coating 3 and a large amount of FeO is not contained. It should be noted that the peak intensity ratio (IA / IB) is usually greater than 0.
[0053] When the coating portion 3 is formed on the surface of the core portion 1 by plating, the peak intensity ratio (IA / IB) can be adjusted by changing the pH of the solution.
[0054] The strongest peak intensities IA and IB of the coating 3 composed of Fe2SiO4 can be obtained by XRD (X-ray diffraction) measurement of the powder magnetic core 7 composed of the alloy particles 5. The XRD measurement is performed, for example, under the following conditions.
[0055] ·Device: Rigaku SmartLab
[0056] X-ray: CuKα
[0057] X-ray wavelength: (Kα1), (Kα2)
[0058] Tube voltage: 40kV
[0059] Tube current: 30mA
[0060] Scanning speed: 5° / min
[0061] Sampling amplitude: 0.02°
[0062] ·Measurement range (2θ): 10°-80°
[0063] Entrance slit: 1 / 2°
[0064] · Light receiving slit 1: 15.000mm
[0065] · Light receiving slit 2: 20.000mm
[0066] In the diffraction pattern of the powder magnetic core 7 obtained by XRD measurement, the Kα2 component is removed, and the peaks derived from the core 1, the measurement cuvette, etc. are removed, and peaks derived from Fe 2 SiO 4 and FeO are obtained.
[0067] (4.2) An example of the measurement results of the strongest peak intensities IA and IB
[0068] Figure 2 An example of the measurement result of X-ray diffraction measured using CuKα (Kα1+Kα2) rays is shown in . This measurement result is the result of separating the diffraction pattern into a Kα1 component and a Kα2 component and removing the Kα2 component. Figure 2The horizontal axis is the diffraction angle 2θ of the peak position. The vertical axis is the diffraction intensity. The strongest peaks of FeO and Fe2SiO4 were observed at the following positions respectively.
[0069] ·The strongest peak of FeO…Diffraction angle 2θ=42.0°±0.2°
[0070] ·The strongest peak of Fe2SiO4…Diffraction angle 2θ=35.9°±0.2°
[0071] (5) Effect of Alloy Particle 5
[0072] The value of the peak intensity ratio (IA / IB) of the alloy particles 5 disclosed in the present invention is less than 0.2. This indicates that the content ratio of FeO in the covering portion 3 is lower than that of Fe2SiO4. Therefore, the powder core 7 containing the alloy particles 5 contains a large amount of Fe2SiO4 with high insulation resistivity in the covering portion 3, and does not contain a large amount of FeO with low insulation resistivity. Therefore, the eddy current loss of the powder core 7 is suppressed to a small extent. In addition, the powder core 7 containing the alloy particles 5 can thin the covering portion 3, so the relative magnetic permeability of the powder core 7 is improved. In addition, for the powder core 7 containing the alloy particles 5 disclosed in the present invention, the melting point (1205°C) of Fe2SiO4 contained in the covering portion 3 is lower than the melting point (1371°C) of FeO, so the covering portions 3 are easily sintered to each other, which can improve the strength.
[0073] 2.Powder core 7
[0074] The powder magnetic core 7 contains a plurality of the above-mentioned alloy particles 5 .
[0075] 3. Method for manufacturing alloy particles 5 and pressed powder core 7
[0076] An example of a method for producing the alloy particles 5 and the powder magnetic core 7 is shown below.
[0077] A. Example of a preferred production method (one)
[0078] (1) Preparation of coating powder
[0079] The core 1 is coated with ferrite by plating. The coating may be formed by grinding, spraying, sol-gel, coprecipitation, etc. in addition to plating. Ferrite may be Ni ferrite, Zn ferrite, Mn ferrite, MnZn ferrite, NiZn ferrite, etc. in addition to the magnet Fe3O4.
[0080] In the plating method, an oxidizing agent (nitrite) is added to an aqueous solution containing the core 1 and divalent ions such as iron ions while controlling the pH to form a ferrite coating. The prepared aqueous solution is filtered and dried to obtain a coated powder.
[0081] (2) Molding (press molding)
[0082] The obtained covered powder is subjected to pressure molding to obtain a molded body. Pressure molding is performed by, for example, applying a surface pressure of 0.5 GPa to 2.0 GPa for molding. In order to improve the moldability, a small amount of organic binder (resin binder) and internal lubricant (stearate, etc.) may also be mixed. In addition, a release agent such as stearate may also be applied to the mold. In addition to uniaxial pressure molding, CIP (cold isostatic pressing) molding may also be performed.
[0083] (3) Annealing (heat treatment)
[0084] By annealing the compact, a powder magnetic core 7 including a plurality of alloy particles 5 is obtained.
[0085] During the annealing process, the ferrite coating reacts with the silicon in the core 1 to form Fe2SiO4.
[0086] Annealing of the covered powder after molding is performed in a non-oxidizing atmosphere (N2 atmosphere, Ar atmosphere or H2 atmosphere). The maximum annealing temperature is preferably 700°C-1050°C. This is because the formation reaction of Fe2SiO4 is promoted, which can reduce eddy current loss. In addition, by annealing, the strain in the core 1 becomes smaller, so the hysteresis loss can be reduced.
[0087] The maximum annealing temperature is more preferably 900°C-1050°C. This is because the strain in the core 1 is further reduced, and the hysteresis loss can be further reduced. By setting the maximum annealing temperature to below 1050°C, the sintering of the alloy particles 5 can be suppressed, and the eddy current loss can be reduced. The annealing temperature is preferably maintained for more than 1 hour. This is because the formation reaction of Fe2SiO4 is promoted, which can reduce the eddy current loss. During the cooling process from 600°C to 300°C, it is preferably cooled at a cooling rate of more than 2°C / min. This is because, when a trace amount of FeO is dissolved in Fe2SiO4, the increase in eddy current loss due to the eutectic phase transformation of FeO is suppressed.
[0088] B. Example of a preferred production method (Part 2)
[0089] (1) Preparation of coating powder
[0090] The coated powder is produced by the method described in the column "(1) Production of coated powder" in the above-mentioned "A. Example (one) of preferred production method".
[0091] (2) Annealing (heat treatment)
[0092] The coated powder is annealed to obtain alloy particles 5. During the annealing process, the ferrite coating reacts with silicon in the core 1 to generate Fe2SiO4.
[0093] Annealing is performed in a non-oxidizing atmosphere (N2 atmosphere, Ar atmosphere or H2 atmosphere). The maximum annealing temperature is preferably 700°C-1050°C. This is because the formation reaction of Fe2SiO4 is advanced, which can reduce eddy current loss. In addition, by annealing, the strain in the core 1 becomes smaller, so the hysteresis loss can be reduced.
[0094] The maximum annealing temperature is more preferably 900°C-1050°C. This is because the strain in the core 1 is further reduced, and the hysteresis loss can be further reduced. By setting the maximum annealing temperature to below 1050°C, the sintering of the alloy particles 5 can be suppressed, and the eddy current loss can be reduced. The annealing temperature is preferably maintained for more than 1 hour. This is because the formation reaction of Fe2SiO4 is promoted, which can reduce the eddy current loss. During the cooling process from 600°C to 300°C, it is preferably cooled at a cooling rate of more than 2°C / min. This is because, when a trace amount of FeO is dissolved in Fe2SiO4, the increase in eddy current loss due to the eutectic phase transformation of FeO is suppressed.
[0095] (3) Molding (press molding)
[0096] The obtained alloy particles 5 are subjected to pressure molding to obtain a powdered magnetic core 7. Pressure molding is performed by, for example, applying a surface pressure of 0.5 GPa-2.0 GPa. In order to improve the moldability, a small amount of an organic binder (resin binder) or an internal lubricant (stearate, etc.) may also be mixed. In addition, a release agent such as stearate may also be applied to the mold. In addition to uniaxial pressure molding, CIP (cold isostatic pressing) molding may also be performed. It should be noted that during molding, a heat treatment for curing the resin binder may also be performed.
[0097] 4. Application examples of powder core 7
[0098] The above-mentioned powder magnetic core 7 is suitable for use in electronic components. Examples of the electronic components include inductors, choke coils, noise filters, reactors, transformers, etc. The electronic component includes, for example, the powder magnetic core 7 and a coil.
[0099] Figure 3-Figure 5 The inductors 10 , 20 , and 30 shown are examples of electronic components of the present disclosure. Figure 3 The inductor 10 shown includes a powder magnetic core 11 and a coil 13 . Figure 4 The inductor 20 shown includes a powder magnetic core 21 and a coil 23 . Figure 5 The inductor 30 shown includes a powder magnetic core 31 and a coil 33. The powder magnetic cores 11, 21, and 31 have the same structure as the powder magnetic core 7.
[0100] Figure 6The noise filter 40 shown is an example of the electronic component of the present disclosure. The noise filter 40 includes a powder magnetic core 41 and a pair of coils 43 and 45. The powder magnetic core 41 has the same structure as the powder magnetic core 7.
[0101] Figure 7 The reactor 50 shown is an example of the electronic component of the present disclosure. The reactor 50 includes a powder magnetic core 51 and a coil 53. The powder magnetic core 51 has the same structure as the powder magnetic core 7.
[0102] Figure 8 The transformer 60 shown is an example of the electronic component of the present disclosure. The transformer 60 includes a powder magnetic core 61 and a pair of coils 63 and 65. The powder magnetic core 61 has the same structure as the powder magnetic core 7 described above.
[0103] The powder magnetic core 7 is preferably used in electronic devices. The electronic devices include electronic components. Examples of the electronic components include the electronic components described above.
[0104] Fig. 9 The noise filter 70 shown is an example of an electronic device of the present disclosure. The noise filter 70 includes an element 71 and capacitors 73, 75, and 77. The element 71 is, for example, Figure 6 The noise filter 40 shown is a component having the same structure.
[0105] The powder magnetic core 7 is preferably used in an electric motor. Examples of the electric motor include a motor and a linear motion actuator.
[0106] Fig.10 The motor 80 shown is an example of the electric motor of the present disclosure. The motor 80 includes a rotor 80A and a stator 80B. The stator 80B includes a powder magnetic core 81 and a coil 83. The powder magnetic core 81 has the same structure as the powder magnetic core 7 described above.
[0107] Fig.11 The generator 90 shown is an example of the generator of the present disclosure. The generator 90 includes a rotor 90A and a stator 90B. The stator 90B includes a powder magnetic core 91 and a coil 93. The powder magnetic core 91 has the same structure as the powder magnetic core 7 described above.
[0108] Example
[0109] Hereinafter, the present invention will be described in more detail based on examples.
[0110] 1. Production of pressed powder core
[0111] (1) Examples 1-4
[0112] In Example 1-4, a core (Fe-6.5% Si) containing 6.5 mass % silicon and the balance consisting of iron and inevitable impurities was used for the raw material powder, and the core was coated with ferrite (Fe3O4) by a plating method.
[0113] In Example 1, an oxidizing agent (nitrite) is added to an aqueous solution containing a core and iron ions (divalent ions) to cover the surface of the core with ferrite. The pH of the aqueous solution when covering the core is adjusted to 10 by a plating method. The plating time is carried out within 30 minutes. After covering the core, pressure molding is carried out at 1 GPa and annealing is maintained at 900°C for 1.5 hours. During the cooling process, cooling is carried out from 600°C to 300°C at a cooling rate of 2°C / min to obtain the powder core of Example 1. It should be noted that Table 1 shows the pH (abbreviated as "pH" in Table 1) and the plating time when covered by the plating method in each embodiment and comparative example.
[0114] [Table 1]
[0115]
[0116] In Example 2, an oxidizing agent (nitrite) is added to an aqueous solution containing a core and iron ions (divalent ions), thereby covering the surface of the core with ferrite. The pH of the aqueous solution when covering the core is adjusted to 6 by a plating method. The plating time is carried out within 30 minutes. After covering the core, pressure molding is performed at 1 GPa and annealing is performed at 900°C for 1.5 hours. During the cooling process, cooling is performed from 600°C to 300°C at a cooling rate of 2°C / min to obtain the powder core of Example 2.
[0117] In Example 3, an oxidant (nitrite) is added to an aqueous solution containing a core and iron ions (divalent ions) to cover the surface of the core with ferrite. The pH of the aqueous solution when covering the core is adjusted to 10 by a plating method. The plating time is within 30 minutes.
[0118] The obtained coated powder was annealed by being kept at 900° C. for 1.5 hours. In the cooling process, the powder was cooled from 600° C. to 300° C. at a cooling rate of 2° C. / min, thereby obtaining alloy particles of Example 3.
[0119] Then, an acrylic resin binder was mixed with the alloy particles, pressure molding was performed at 1 GPa, and heat curing treatment was performed at 120° C. for 1 hour, thereby obtaining the powder magnetic core of Example 3.
[0120] In Example 4, an oxidizing agent (nitrite) is added to an aqueous solution containing a core and iron ions (divalent ions) to cover the surface of the core with ferrite. The pH of the aqueous solution when covering the core is adjusted to 10 by a plating method. The plating time is carried out within 5 minutes. After covering the core, pressure molding is performed at 1 GPa and annealing is performed at 900°C for 1.5 hours. During the cooling process, cooling is performed from 600°C to 300°C at a cooling rate of 2°C / min to obtain the powder core of Example 4.
[0121] (2) Comparative Example 1
[0122] Comparative Example 1: Similar to Example 1-4, a core containing 6.5 mass % of silicon and the balance consisting of iron and inevitable impurities was used as a raw material powder, and the core was coated with ferrite (Fe3O4) by a plating method.
[0123] Comparative Example 1 is as follows: An oxidizing agent (nitrite) is added to an aqueous solution containing a core and iron ions (divalent ions) to cover the surface of the core with ferrite. The pH of the aqueous solution when covering the core is adjusted to 11 by a plating method. The plating time is carried out within 30 minutes. After covering the core, pressure molding is performed at 1 GPa and annealing is performed at 900°C for 1.5 hours. During the cooling process, cooling is performed from 600°C to 300°C at a cooling rate of 2°C / min to obtain the powder core of Comparative Example 1. Comparative Example 1 is the same as Example 1 except that the pH of the aqueous solution when covering the core is adjusted to 11.
[0124] 2. Measurement of peak intensity of the coating portion by XRD (X-ray diffraction)
[0125] The obtained sample was finely pulverized in a mortar, and the finely pulverized sample was filled in a sample holder so as to be at the same height as the edge of the sample holder.
[0126] The powder sample filled in the sample holder was measured using an X-ray diffraction apparatus under the following conditions.
[0127] ·Device: Rigaku SmartLab
[0128] X-ray: CuKα
[0129] X-ray wavelength: (Kα1), (Kα2)
[0130] Tube voltage: 40kV
[0131] Tube current: 30mA
[0132] Scanning speed: 5° / min
[0133] Sampling amplitude: 0.02°
[0134] ·Measurement range (2θ): 10°-80°
[0135] Entrance slit: 1 / 2°
[0136] · Light receiving slit 1: 15.000mm
[0137] · Light receiving slit 2: 20.000mm
[0138] Figure 2 The results of X-ray diffraction measurements using an X-ray diffraction device (Rigaku SmartLab) with CuKα (Kα1+Kα2) rays are shown in the figure. In the diffraction pattern of the powder core obtained by XRD measurement, the Kα2 component is removed, and the peaks originating from the core, the measurement cuvette, etc. are removed, and the peaks of Fe2SiO4 and FeO originating from the covering are obtained.
[0139] The strongest peak intensity IA of FeO is recorded as the intensity of the diffraction peak at a diffraction angle of 2θ=42.0°.
[0140] The strongest peak intensity IB of Fe2SiO4 is recorded as the diffraction peak intensity at a diffraction angle of 2θ=35.9°.
[0141] 3. Evaluation method of eddy current loss
[0142] The eddy current loss of the powder magnetic core was evaluated using a measuring device (BH Analyzer, Iwasaki Communication Co., Ltd., Model SY-8218) under the conditions of 0.1 T and 10 kHz using the following modified Steinmetz equation regarding iron loss.
[0143]
[0144] P CV : Iron loss
[0145] Hysteresis loss term
[0146] K C (B m f) 2 : Eddy current loss term
[0147] K e (B m f) 1.5 :Residual loss term
[0148] 4. Strength evaluation method
[0149] A test piece (50 mm×4 mm×3 mm thick) of the powder core was prepared and subjected to a three-point bending test to obtain an index of strength.
[0150] 5. Evaluation method of relative magnetic permeability
[0151] The relative magnetic permeability of the powder core was measured using a measuring device (BH Analyzer, Iwasaki Communication Co., Ltd., Model SY-8218). The relative magnetic permeability was evaluated under the conditions of 0.1 T and 10 kHz.
[0152] 6. Evaluation results
[0153] Table 1 shows the evaluation results.
[0154] Examples 1-4 satisfy the following conditions (a)-(c).
[0155] Condition (a): The alloy particles have a core portion formed of an alloy containing iron and silicon and a coating portion covering the core portion.
[0156] Condition (b): The coating portion contains Fe2SiO4.
[0157] Condition (c): When the coating portion is measured by X-ray diffraction, with the strongest peak intensity of FeO being IA and the strongest peak intensity of Fe2SiO4 being IB, the peak intensity ratio (IA / IB) is 0.2 or less.
[0158] On the other hand, Comparative Example 1 does not satisfy the above condition (c). That is, in Comparative Example 1, the value of the peak intensity ratio (IA / IB) is larger than 0.2.
[0159] The eddy current losses of Examples 1-4 satisfying the above conditions (a)-(c) are 1.7 kW / m 3 , 1.6kW / m 3 , 1.8kW / m 3 , 1.9kW / m 3 In Comparative Example 1 which does not satisfy the above condition (c), the eddy current loss is 5.4 kW / m 3 . Examples 1-4 are as follows: the coating of the alloy particles contains a large amount of Fe2SiO4 with high insulation resistivity, but does not contain much FeO, so it is believed that the insulation between the alloy particles is high and the eddy current loss can be suppressed. On the other hand, Comparative Example 1 is as follows: the coating of the alloy particles contains a large amount of FeO with high insulation resistivity, but does not contain much Fe2SiO4, so it is believed that the eddy current loss becomes larger.
[0160] In Examples 1-4 that satisfy the above conditions (a)-(c), the strengths of the three-point bending test are 61 MPa, 59 MPa, 71 MPa, and 58 MPa, all of which are good. In Comparative Example 1 that does not satisfy the above condition (c), the strength of the three-point bending test is 55 MPa, which is a result worse than that of the examples. Examples 1-4 are as follows: The covering portion of the alloy particles contains Fe2SiO4, which has a lower melting point than iron oxide, so the covering portions are easily sintered to each other, and it is believed that the strength is improved. Example 3 is as follows: An acrylic resin is mixed in the alloy powder, and it is believed that the strength is particularly improved.
[0161] In Examples 1 to 4 and Comparative Example 1, the relative magnetic permeabilities were 64, 67, 35, 86, and 74, all of which were good results. In particular, Example 4 showed that the relative magnetic permeability became good by setting the plating time to 5 minutes.
[0162] It is suggested that the peak intensity ratio becomes 0.2 or less by adjusting the pH of the aqueous solution to 6-10 when forming the coating portion.
[0163] 7. Effects of the Embodiments
[0164] The powder magnetic core of this embodiment has small eddy current loss and high strength.
[0165] The present invention is not limited to the above-described detailed embodiments, and various modifications and changes can be made within the scope of the claims of the present invention.
[0166] Industrial Applicability
[0167] The powder magnetic core of the present invention is particularly suitable for use in motors, transformers, reactors, inductors, noise filters and the like.
[0168] Description of Reference Numerals
[0169] 1…Core
[0170] 3… Covering
[0171] 5… Alloy particles
[0172] 7, 11, 21, 31, 41, 51, 61, 81, 91… pressed powder core
[0173] 10, 20, 30...Inductor (electronic component)
[0174] 13, 23, 33, 43, 45, 53, 63, 65, 83, 93… coils
[0175] 40…Noise filter (electronic components)
[0176] 50… Reactor (electronic component)
[0177] 60...Transformer (electronic component)
[0178] 70…Noise filter (electronic equipment)
[0179] 80…Motor (electric motor)
[0180] 90…Generator.
Claims
1. An alloy particle comprising: a core portion formed of an alloy containing iron and silicon and a covering portion covering the core portion, The covering portion contains Fe2SiO4, The coating is measured by X-ray diffraction, The strongest peak intensity of FeO is set as IA, When the strongest peak intensity of Fe2SiO4 is set to IB, The value of the peak intensity ratio (IA / IB) is 0.2 or less.
2. A powder magnetic core comprising a plurality of alloy particles according to claim 1. 3 . An electronic component comprising the powder magnetic core according to claim 2 . The electronic component according to claim 3 , comprising the powder magnetic core and a coil. 5 . An electronic device comprising the electronic component according to claim 3 or 4 . 6 . An electric motor comprising the powder magnetic core according to claim 2 .
7. A generator comprising the powder magnetic core according to claim 2.