Recovery method of polyester / wool blended fabric

By using a composite catalyst system in polyester/wool blend fabric for gentle depolymerization, the problem of degradation of temperature-sensitive wool fibers is solved, and the complete separation and efficient recycling of polyester and wool fibers is achieved, and the recovery rate is improved. Fiber properties.

CN118893079APending Publication Date: 2024-11-05QINGDAO AMINO MATERIAL TECH CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410959188.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The prior art is difficult to improve the depolymerization recovery rate of polyester/wool blended fabrics while ensuring the performance of wool fibers, especially due to the problem of degradation in performance caused by temperature sensitivity and low temperature depolymerization rate.

Method used

The composite catalyst system is adopted, including the main catalyst being piperazine compounds and the auxiliary catalyst being a mixture of lactam compounds and ionic liquids. The depolymerization reaction is carried out under mild conditions of 40-70°C to weaken the interaction between polyester and wool fibers. Force to ensure non-destructive retention of wool fibers and complete depolymerization of polyester.

Benefits of technology

Complete separation of polyester and wool fibers is achieved, recovery rate is improved, mechanical properties and chemical stability of wool fibers are ensured, and 100% depolymerization of polyester is achieved, achieving efficient recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118893079A_ABST
    Figure CN118893079A_ABST
Patent Text Reader

Abstract

The invention discloses a polyester / wool blended fabric recovery method, which comprises: S1, drying a washed polyester / wool blended fabric, adding into an alcoholic solution of a composite catalyst, and carrying out a depolymerization reaction at a temperature of 40-70 DEG C to obtain wool fibers and a slurry; the composite catalyst comprises a main catalyst and an auxiliary catalyst; the main catalyst is a piperazine compound, and the auxiliary catalyst is a mixture of a lactam compound and an ionic liquid; s2, washing the wool fibers with alcohol to obtain a cleaning solution, mixing the cleaning solution with the slurry, and carrying out solid-liquid separation to obtain polyester-hydrolyzed polyester monomers and filtrate; through the depolymerization reaction of the composite catalyst in the solvent, complete depolymerization of polyester is ensured, and the reaction temperature is low, so that temperature-sensitive wool components can be retained in a lossless manner, the mechanical property and chemical stability of the wool components are not influenced, meanwhile, complete separation of polyester and wool fibers at the temperature of 75 DEG C or below can be realized, the polyester is completely depolymerized, and the recovery rate is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textiles, and in particular to a method for recycling polyester / wool blended fabrics. Background Art

[0002] Polyester has many excellent textile properties. It can be spun purely or blended with natural fibers such as wool, wool, silk, linen and other chemical fibers to make imitation wool, imitation wool, imitation silk and imitation linen fabrics of various colors. However, clothing made of these polyester fibers is often disposed of by landfill and incineration at the end of consumption, which not only wastes a lot of resources, but also causes serious secondary pollution.

[0003] To prevent secondary pollution, relevant technologies have recycled polyester / wool blended fabrics. However, due to the temperature sensitivity of wool, high temperatures (>75°C) will cause the performance of the recycled wool component to decline, such as a decrease in fiber strength or elongation. This makes the separation and recycling of polyester / wool blended fabrics extremely difficult. At the same time, under conditions below 75°C, the recovery rate of depolymerized polyester is low.

[0004] Therefore, it is necessary to provide a recycling scheme for polyester / wool blended fabrics, which can improve the recovery rate of depolymerized polyester while ensuring the performance of the recycled wool component. Summary of the invention

[0005] In view of this, the present application provides a method for recycling polyester / wool blended fabrics, which is used to solve the problem of how to improve the recovery rate of depolymerized polyester while ensuring the performance of the recycled wool component.

[0006] In order to achieve the above technical objectives, this application adopts the following technical solutions: In a first aspect, the present application provides a method for recycling polyester / wool blended fabrics, comprising the following steps: S1. The washed polyester / wool blended fabric is dried, and then added to an alcohol solution of a composite catalyst, and depolymerized at 40-70° C. to obtain wool fibers and slurry; the composite catalyst includes a main catalyst and an auxiliary catalyst; the main catalyst is a piperazine compound, and the auxiliary catalyst is a mixture of a lactam compound and an ionic liquid; S2. Wash the wool fiber with alcohol to obtain a washing liquid, mix the washing liquid with the slurry, separate the solid and the liquid, and obtain polyester monomers and a filtrate.

[0007] Preferably, the amount of the composite catalyst is 1-20% of the mass of the polyester / wool blended fabric; the mass ratio of the main catalyst to the auxiliary catalyst is 1:2-15, and the mass ratio of the lactam compound to the ionic liquid is 1:0.1-10.

[0008] Preferably, the main catalyst includes one or more of 1,4-dimethylpiperazine, N,N',N''-trimethylaminoethylpiperazine, N,N'-dihydroxyethylpiperazine, N-methyl-N'-hydroxyethylpiperazine, and 1-(2-dimethylaminoethyl)-4-methylpiperazine.

[0009] Preferably, the lactam compound includes one or more of N-methylpyrrolidone, 2-pyrrolidone, 1-octyl-2-pyrrolidone, and N-ethyl-2-pyrrolidone.

[0010] Preferably, the ionic liquid includes one or more of 1-butyl-3-methylimidazolium tetrafluoroborate, 1,3-dimethylimidazolium dimethyl phosphate, 1-ethyl-3-methylimidazolium acetate, 1-hexyl-3-methylimidazolium hexafluorophosphate, 1-hexyl-3-methylimidazolium hexafluorophosphate, N-ethylpyridinium tetrafluoroborate, 1-butyl-3-methylimidazolium bistrifluoromethanesulfonyl imide, 1-dodecyl-3-methylimidazolium tetrafluoroborate, and 1-benzyl-3-methylimidazolium tetrafluoroborate.

[0011] Preferably, in step S1, the step of washing the polyester / wool blended fabric is: washing the polyester / wool blended fabric with a mixed system of alcohol and sodium sulfite at 40-70° C. for 20-60 min.

[0012] Preferably, the polyester content in the polyester / wool blended fabric is 5-95%.

[0013] Preferably, the method further comprises subjecting the filtrate to atmospheric pressure distillation to recover alcohol, and then subjecting the filtrate to vacuum distillation or extraction to recover the diol monomer of the polyester, as well as the piperazine compound and the lactam compound.

[0014] Preferably, the auxiliary catalyst is prepared by stirring the lactam compound and the ionic liquid at 30-50°C.

[0015] In a second aspect, the present application provides wool fibers and polyester depolymerization monomers obtained by a recycling method.

[0016] The beneficial effects of this application are as follows: The present application uses a composite catalyst to react with a solvent to weaken the interaction between the polyester component and the wool component by using an ionic liquid in the auxiliary catalyst, thereby enabling the piperazine main catalyst with moderate alkalinity (pH 10-12) to effectively catalyze the alcoholysis of the polyester with methanol. At the same time, the lactam compound can stabilize the organic base main catalyst cation formed during the catalytic process, thereby increasing the activity of the main catalyst and ensuring the complete depolymerization of the polyester. Since the catalyst used has moderate alkalinity and the reaction temperature is relatively low, the temperature-sensitive wool component can be retained intact, and the mechanical properties and chemical stability of the wool component are not affected. At the same time, the polyester and wool fibers can be completely separated below 75°C, and the polyester is completely depolymerized with a high recovery rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The hydrogen nuclear magnetic resonance spectrum of the polyester monomer dimethyl terephthalate (DMT) recovered after depolymerization provided in Example 6 of the present invention ( 1 H NMR); Figure 2 The separated and recycled polyester and wool blended fabric provided in Example 6 of the present invention. DETAILED DESCRIPTION

[0018] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0019] The present application provides a method for recycling polyester / wool blended fabrics, comprising the following steps: S1. The washed polyester / wool blended fabric is dried, and then added to an alcohol solution of a composite catalyst, and depolymerized at 40-70° C. for 2-8 hours to obtain wool fibers and slurry; the composite catalyst includes a main catalyst and an auxiliary catalyst; the main catalyst is a piperazine compound, and the auxiliary catalyst is a mixture of a lactam compound and an ionic liquid; S2. Wash the wool fiber with alcohol to obtain a washing liquid, mix the washing liquid with the slurry, separate the solid and the liquid, and obtain polyester monomers and a filtrate.

[0020] The present invention adopts a composite catalyst system to achieve complete depolymerization of polyester under mild conditions. In the composite catalyst system, the ionic liquid weakens the interaction between the polyester component and the wool component, so that the piperazine main catalyst with moderate alkalinity effectively catalyzes the methanol decomposition of the polyester, and at the same time, strengthens the separation of the wool component and the polyester component, and improves the separation degree of the two; at the same time, the lactam compound can stabilize the organic base main catalyst cation formed in the catalytic process, improve the activity of the main catalyst, and ensure the complete depolymerization of the polyester. Since the alkalinity of the catalyst used is moderate and the reaction temperature is low, the temperature-sensitive wool component can be retained intact, and the fiber strength of the wool component finally obtained is high and the expansion rate is low.

[0021] The dosage of the composite catalyst is 1-20% of the mass of the polyester / wool blended fabric. Too high a dosage will damage the wool component, while too low a dosage will lead to incomplete depolymerization of the polyester; the mass ratio of the main catalyst to the auxiliary catalyst is 1:2-15. Too low a dosage will lead to incomplete depolymerization of the polyester, while too high a dosage will cause waste of resources and reduced economic efficiency; the mass ratio of the lactam compound to the ionic liquid is 1:0.1-10. Too low a dosage will lead to incomplete depolymerization of the polyester, while too high a dosage will cause waste of resources.

[0022] In this application, polyester depolymerization refers to the depolymerization of polyester into monomers, thereby falling off and separating from blended fabrics, and then realizing the separation and recovery of polyester components. The polyester in this technology is a polymer containing ester chemical bonds, such as polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), polybutylene terephthalate (PBT), polyethylene 2,5-furandicarboxylate (PEF), polytrimethylene 2,5-furandicarboxylate (PTF), polybutylene 2,5-furandicarboxylate (PBF), polylactic acid (PLA), polyhydroxyalkanoic acid (PHA), polybutylene glycol succinate (PBS), low melting point polyester copolymer; wool fiber includes fibers spun from wool and cashmere; polyester depolymerization polyester monomers include DMT.

[0023] In some embodiments, the main catalyst includes one or more of 1,4-dimethylpiperazine, N,N',N''-trimethylaminoethylpiperazine, N,N'-dihydroxyethylpiperazine, N,N',-diethyl-2-methylpiperazine, and N-methyl-N'-hydroxyethylpiperazine.

[0024] In some embodiments, the lactam compound includes one or more of N-methylpyrrolidone, 2-pyrrolidone, 1-octyl-2-pyrrolidone, and N-ethyl-2-pyrrolidone.

[0025] In some embodiments, the ionic liquid includes one or more of 1-butyl-3-methylimidazolium tetrafluoroborate, 1,3-dimethylimidazolium dimethyl phosphate, 1-ethyl-3-methylimidazolium acetate, 1-hexyl-3-methylimidazolium hexafluorophosphate, 1-hexyl-3-methylimidazolium hexafluorophosphate, N-ethylpyridinium tetrafluoroborate, 1-butyl-3-methylimidazolium bistrifluoromethanesulfonyl imide, 1-dodecyl-3-methylimidazolium tetrafluoroborate, and 1-benzyl-3-methylimidazolium tetrafluoroborate.

[0026] In some embodiments, in step S1, the step of washing the polyester / wool blended fabric is: washing the polyester / wool blended fabric with a mixed system of alcohol and sodium sulfite at 40-70° C. for 20-60 minutes. Sodium sulfite has reducing properties, which can weaken the interaction between proteins in the wool component to a certain extent, and is more conducive to the decolorization of the fabric (dyed fabric).

[0027] In some embodiments, the polyester content in the polyester / wool blended fabric is 5-95%.

[0028] In some embodiments, the filtrate is further subjected to atmospheric distillation to recover alcohol, and then subjected to vacuum distillation or extraction to recover the diol monomer of the polyester, as well as the piperazine compound and the lactam compound.

[0029] In some embodiments, the auxiliary catalyst is prepared by stirring a lactam compound and an ionic liquid at 30-50° C.

[0030] The present application provides wool fibers and polyester depolymerization monomers obtained by a recycling method.

[0031] The catalyst system used in the present invention can achieve 100% depolymerization of polyester under low temperature conditions, and at the same time achieve complete separation of polyester and wool components in polyester / wool blended fabrics, with a high recovery rate. Moreover, the reaction separation process in the present invention is gentle and efficient, and the wool fiber can obtain 100% pure components and the fibers are almost not damaged, and can be directly spun into silk threads or used as raw materials to produce regenerated wool fibers. The recovered polyester depolymerization monomers can also be used for the synthesis of new polyester, thereby realizing the closed-loop recycling of the two fiber components in the polyester / wool blended waste.

[0032] The present solution is further described below through specific embodiments.

[0033] Source of raw materials: The polyester / wool blended fabric used in the embodiments of the present application is a blended fabric of PET and wool, wherein the PET content is 50 wt %, the wool content is 50 wt %, and the fabric is cut into a 4 cm*4 cm square shape.

[0034] The enumerated embodiments are not limited to fabrics of this type of components, and other types of blended fabrics of polyester and wool in different proportions are also applicable.

[0035] Examples 1-5 A method for recycling polyester / wool blended fabrics comprises the following steps: S1. 10 g of polyester / wool blended fabric was washed with methanol at 50°C for 60 minutes. During the washing process, 0.2 g of sodium sulfite was added for washing. After washing, the fabric was dried at 60°C for 1 hour. The dried blended fabric, 40 g of methanol, 1 g of 1,4-dimethylpiperazine and 2 g of auxiliary catalyst were added to a reactor. The reactor was then heated to 70°C. After reacting for 3 hours, the reactor was cooled to room temperature. The remaining block solid in the reactor was taken out. The block solid was an undamaged wool fiber frame, and the liquid was a slurry. The type and amount of the auxiliary catalyst in Examples 1-5 are shown in Table 1. S2. The wool fiber frame was washed twice with methanol and dried to obtain 5.0 g of the wool fiber frame. All the wool fiber components were retained. The washing liquid was combined with the slurry in the kettle, and the solid part and the liquid part in the slurry were separated by filtration. The solid part was the depolymerized polyester monomer dimethyl terephthalate (DMT, see Figure 1 ); the filtrate is distilled and vacuum distilled to recover methanol, ethylene glycol, 1,4-dimethylpiperazine and lactam compounds.

[0036] Table 1 Composite components of the catalyst in Examples 1-5

[0037] Example 6 A method for recycling polyester / wool blended fabrics comprises the following steps: S1. 10 g of polyester / wool blended fabric was washed with methanol at 60°C for 20 minutes. During the washing process, 0.2 g of sodium sulfite was added for washing. After washing, the fabric was dried at 60°C for 1 hour. The dried blended fabric was added into a reactor with 40 g of methanol, 2 g of N,N′, N′′-trimethylaminoethylpiperazine, 2 g of N-methylpyrrolidone, and 2 g of 1-ethyl-3-methylimidazole acetate. The reactor was then heated to 40°C. After reacting for 6 hours, the reactor was cooled to room temperature. The block solid remaining in the reactor was taken out. The block solid was an undamaged wool fiber frame, and the liquid was a slurry. S2. The wool fiber framework was washed twice with methanol and dried to obtain 5.0 g of the wool fiber framework. All wool fiber components were retained. The washing liquid was combined with the slurry in the kettle. The solid part and the liquid part in the slurry were separated by filtration. The solid part was the depolymerized polyester monomer DMT. The filtrate was distilled and vacuum distilled to recover methanol, ethylene glycol, N, N′, N′′-trimethylaminoethylpiperazine and N-methylpyrrolidone.

[0038] Figure 1 The hydrogen nuclear magnetic resonance spectrum of the polyester monomer dimethyl terephthalate (DMT) recovered after depolymerization provided in Example 6 of the present invention ( 1 1H NMR).

[0039] Figure 2 The separated and recovered polyester and wool blended fabric provided in Example 6 of the present invention; wherein A is the blended fabric before the separation reaction; and B is the pure wool fabric after the separation reaction, in which the wool fibers are not damaged.

[0040] Example 7 A method for recycling polyester / wool blended fabrics comprises the following steps: S1. 10 g of polyester / wool blended fabric was washed with methanol at 60°C for 20 minutes. During the washing process, 0.2 g of sodium sulfite was added for washing. After washing, the fabric was dried at 60°C for 1 hour. The dried blended fabric was added into a reactor with 40 g of methanol, 0.1 g of N,N′-diethylpiperazine, 1 g of 2-pyrrolidone and 1 g of N-ethylpyridine tetrafluoroborate. The reactor was then heated to 70°C. After reacting for 4 hours, the reactor was cooled to room temperature. The block solid remaining in the reactor was taken out. The block solid was the undamaged wool fiber framework, and the liquid was the slurry. S2. The wool fiber framework was washed twice with methanol and dried to obtain 5.0 g of the wool fiber framework. All wool fiber components were retained. The washing liquid was combined with the slurry in the kettle. The solid part and the liquid part in the slurry were separated by filtration. The solid part was the depolymerized polyester monomer DMT. The filtrate was distilled and vacuum distilled to recover methanol, ethylene glycol, N, N′-diethylpiperazine and 2-pyrrolidone.

[0041] Example 8 A method for recycling polyester / wool blended fabrics comprises the following steps: S1. 10 g of polyester / wool blended fabric was washed with methanol at 60°C for 50 minutes. During the washing process, 0.2 g of sodium sulfite was added for washing. After washing, the fabric was dried at 60°C for 1 hour. The dried blended fabric was added into a reactor with 40 g of methanol, 1 g of N,N′,-diethyl-2-methylpiperazine, 1 g of 1-octylpyrrolidone, and 1 g of 1-benzyl-3-methylimidazole tetrafluoroborate. The reactor was then heated to 60°C. After reacting for 2 hours, the reactor was cooled to room temperature. The block solid remaining in the reactor was taken out. The block solid was the undamaged wool fiber framework, and the liquid was the slurry. S2. The wool fiber framework was washed twice with methanol and dried to obtain 5.0 g of the wool fiber framework. All wool fiber components were retained. The washing liquid was combined with the slurry in the kettle. The solid part and the liquid part in the slurry were separated by filtration. The solid part was the depolymerized polyester monomer DMT. The filtrate was distilled and vacuum distilled to recover methanol, ethylene glycol, N, N′,-diethyl-2-methylpiperazine and 1-octylpyrrolidone.

[0042] Example 9 A method for recycling polyester / wool blended fabrics comprises the following steps: S1. 10 g of polyester / wool blended fabric was washed with methanol at 70°C for 40 minutes. During the washing process, 0.2 g of sodium sulfite was added for washing. After washing, the fabric was dried at 60°C for 1 hour. The dried blended fabric was added into a reactor with 40 g of methanol, 0.5 g of N-methyl-N′-hydroxyethylpiperazine, 1 g of N-ethyl-2-pyrrolidone, and 1 g of 1-hexyl-3-methylimidazole hexafluorophosphate. The reactor was then heated to 60°C. After reacting for 4 hours, the reactor was cooled to room temperature. The block solid remaining in the reactor was taken out. The block solid was the undamaged wool fiber frame, and the liquid was the slurry. S2. The wool fiber frame was washed twice with methanol and dried to obtain 5.0 g of the wool fiber frame. All the wool fiber components were retained. The washing liquid was combined with the slurry in the kettle. The solid part and the liquid part in the slurry were separated by filtration. The solid part was the depolymerized polyester monomer DMT. The filtrate was distilled and vacuum distilled to recover methanol, ethylene glycol, N-methyl-N′-hydroxyethylpiperazine and N-ethyl-2-pyrrolidone.

[0043] Example 10 A method for recycling polyester / wool blended fabrics comprises the following steps: S1. 1 kg of polyester / wool blended fabric is washed with methanol at 60°C for 50 minutes. During the washing process, 20 g of sodium sulfite is added for washing. After washing, the fabric is dried at 60°C for 1 hour. The dried blended fabric is added into a reactor with 4 kg of methanol, 100 g of N,N′,-diethyl-2-methylpiperazine, 100 g of 1-octylpyrrolidone, and 100 g of 1-benzyl-3-methylimidazole tetrafluoroborate. The reactor is then heated to 80°C. After reacting for 2 hours, the reactor is cooled to room temperature. The block solid remaining in the reactor is taken out. The block solid is an undamaged wool fiber framework, and the liquid is a slurry. S2. The wool fiber frame is washed twice with methanol and dried to obtain 450 g of the wool fiber frame. All wool fiber components are retained. The washing liquid is combined with the slurry in the kettle. The solid part and the liquid part in the slurry are separated by filtration. The solid part is the depolymerized polyester monomer DMT. The filtrate is distilled and vacuum distilled to recover methanol, ethylene glycol, N, N′,-diethyl-2-methylpiperazine and 1-octylpyrrolidone.

[0044] Comparative Example 1 A method for recycling polyester / wool blended fabrics, the other contents are the same as those of Example 1, except that the catalyst used is 1g of 1,4-dimethylpiperazine.

[0045] Comparative Example 2 A method for recycling polyester / wool blended fabrics, the other contents of which are the same as those of Example 1, except that the catalyst used is 2g of N-methyl-2-pyrrolidone.

[0046] Comparative Example 3 A method for recycling polyester / wool blended fabrics, the other contents of which are the same as those of Example 1, except that the catalyst used is 2g of 1-butyl-3-methylimidazole tetrafluoroborate.

[0047] Comparative Example 4 A method for recycling polyester / wool blended fabrics, other contents are the same as those in Example 1, except that the depolymerization temperature is 75°C.

[0048] Test and Evaluation The depolymerization efficiency of the polyester in the test examples and comparative examples, as well as the recovery rate of the DMT monomer and the recovery rate of the wool component, are shown in Table 2.

[0049] Among them, the depolymerization efficiency (E) can be calculated from the amount of solids remaining after the reaction. The calculation formula is as follows: Depolymerization efficiency (E) = (polyester fiber content in textile fabric - amount of undepolymerized polyester) / polyester fiber content in textile fabric.

[0050] Table 2 Component recovery results

[0051] The wool components obtained in the examples and comparative examples were opened by an opener to form wool fibers. The recycled wool fibers were made into regenerated wool yarns, and the physical properties were tested according to GB / T 13835.5 and GB / T 13835.6, etc. The physical properties are shown in Table 3. The wool components obtained in comparative examples 1-3 could not be regenerated into wool fibers.

[0052] Table 3 Physical properties of regenerated wool yarn

[0053] The polyester monomer DMT obtained in Example 6 and Comparative Examples 1-4 was polymerized in vacuum at 290° C. for 3 hours using antimony trioxide as a catalyst to generate polyester. The obtained polyester was repeatedly polymerized, depolymerized and polymerized. The parameters of each depolymerization and polycondensation are shown in Table 4.

[0054] Table 4 Parameters of repeated polymerization and depolymerization of polyester depolymerization monomers

[0055] The above results indicate that the present application uses a composite catalyst to carry out a depolymerization reaction in a solvent, and the ionic liquid in the auxiliary catalyst weakens the interaction between the polyester component and the wool component, so that the piperazine main catalyst with moderate alkalinity can effectively catalyze methanol and alcoholyze the polyester. At the same time, the lactam compound can stabilize the organic base main catalyst cation formed in the catalytic process, improve the activity of the main catalyst, and ensure the complete depolymerization of the polyester. Since the alkalinity of the catalyst used is moderate and the reaction temperature is relatively low, the temperature-sensitive wool component can be retained intact, and the mechanical properties and chemical stability of the wool component are not affected. At the same time, the complete separation of polyester and wool fibers below 75°C can be achieved, and the polyester is completely depolymerized with a high recovery rate.

[0056] The above are only preferred specific implementations of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A method for recycling polyester / wool blended fabrics, characterized in that: The following steps are involved: S1. Drying the washed polyester / wool blended fabric, and then adding it to an alcohol solution of a composite catalyst, performing a depolymerization reaction at 40-70° C. to obtain wool fibers and slurry; the composite catalyst comprises a main catalyst and an auxiliary catalyst; the main catalyst is a piperazine compound, and the auxiliary catalyst is a mixture of a lactam compound and an ionic liquid; S2. Wash the wool fiber with alcohol to obtain a washing liquid, mix the washing liquid with the slurry, separate the solid from the liquid, and obtain polyester monomers and a filtrate.

2. The method for recycling polyester / wool blended fabric according to claim 1, characterized in that: The dosage of the composite catalyst is 1-20% of the mass of the polyester / wool blended fabric; the mass ratio of the main catalyst to the auxiliary catalyst is 1:2-15, and the mass ratio of the lactam compound to the ionic liquid is 1:0.1-10.

3. The method for recycling polyester / wool blended fabric according to claim 1, characterized in that: The main catalyst includes one or more of 1,4-dimethylpiperazine, N,N',N''-trimethylaminoethylpiperazine, N,N'-dihydroxyethylpiperazine, N-methyl-N'-hydroxyethylpiperazine, and 1-(2-dimethylaminoethyl)-4-methylpiperazine.

4. The method for recycling polyester / wool blended fabric according to claim 1, characterized in that: The lactam compound includes one or more of N-methylpyrrolidone, 2-pyrrolidone, 1-octyl-2-pyrrolidone, and N-ethyl-2-pyrrolidone.

5. The method for recycling polyester / wool blended fabric according to claim 1, characterized in that: The ionic liquid includes one or more of 1-butyl-3-methylimidazolium tetrafluoroborate, 1,3-dimethylimidazolium dimethyl phosphate, 1-ethyl-3-methylimidazolium acetate, 1-hexyl-3-methylimidazolium hexafluorophosphate, 1-hexyl-3-methylimidazolium hexafluorophosphate, N-ethylpyridinium tetrafluoroborate, 1-butyl-3-methylimidazolium bistrifluoromethanesulfonyl imide, 1-dodecyl-3-methylimidazolium tetrafluoroborate, and 1-benzyl-3-methylimidazolium tetrafluoroborate.

6. The method for recycling polyester / wool blended fabric according to claim 1, characterized in that: In step S1, the step of washing the polyester / wool blended fabric is: washing the polyester / wool blended fabric with a mixed system of alcohol and sodium sulfite at 40-70° C. for 20-60 minutes.

7. The method for recycling polyester / wool blended fabric according to claim 1, characterized in that: The polyester content in the polyester / wool blended fabric is 5-95%.

8. The method for recycling polyester / wool blended fabric according to claim 1, characterized in that: The method also includes subjecting the filtrate to atmospheric pressure distillation to recover alcohol, and then subjecting the filtrate to vacuum distillation or extraction to recover the diol monomer of the polyester, as well as the piperazine compound and the lactam compound.

9. The method for recycling polyester / wool blended fabric according to claim 1, characterized in that: The preparation method of the auxiliary catalyst is as follows: stirring the lactam compound and the ionic liquid at 30-50° C. to obtain the auxiliary catalyst.

10. Wool fiber and polyester monomers obtained by the recovery method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Directed degradation method of waste polyurethane material

    CN110105621A

  • Method for catalyzing methanol alcoholysis of waste PET polyester by choline and terephthalic acid nonmetal ionic liquid

    CN112851502A

  • Preparation of pyrrolidone eutectic solvent and method for efficiently catalyzing alcoholysis of PET by using pyrrolidone eutectic solvent

    CN113717047A

  • Method for recovering polyester fabric by using ionic liquid catalyst

    CN115724738A

  • Recycling method of polyester blended fabric

    CN116655465A