Core roller structure and ring rolling forming method for rare earth magnesium alloy ring piece

By using core roller structure with trapezoidal protrusions and multi-directional forging technology during the rolling and expansion of rare earth magnesium alloy, the problems of poor plasticity and texture tendency of magnesium alloy ring forgings are solved, and the three-dimensional crystal grains of magnesium alloy materials are realized Orientation regulation and mechanical performance improvement.

CN118893166AActive Publication Date: 2024-11-05SHANGHAI JIAOTONG UNIV +2
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411091099.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-05
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

The poor plasticity of magnesium alloy and the strong constraints on material flow during rolling and forming process make it difficult to stabilize the structural dimensions of rare earth magnesium alloy ring forgings, and the mechanical properties are large discrete, and traditional core rollers cannot effectively eliminate texture tendencies and improve crystallization. Grain refinement ability.

Method used

Adopting a core roller structure with trapezoidal convexity, the dislocation constraint shear effect is generated along the thickness direction of the blank to enhance the grain refinement effect, and the three-dimensional grain orientation of magnesium alloy material is realized through multi-directional forging and homogenization heat treatment. Regulate and improve formability and mechanical properties.

Benefits of technology

It significantly improves the structural refining ability of magnesium alloy materials, eliminates strong texture, improves the mechanical properties consistency of rare earth magnesium alloy ring forgings, improves the formingability and grain refining ability, and realizes isotropy of ring forgings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118893166A_ABST
    Figure CN118893166A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of ring rolling forming, and discloses a core roller structure which is characterized by comprising a core roller body and trapezoid protrusions arranged at intervals in the axial direction of the outer wall of the core roller body. Meanwhile, the invention discloses a rare earth magnesium alloy ring piece ring rolling forming method suitable for the core roller structure, and the method comprises the steps that when a core roller is fed every time, a blank is subjected to compression deformation, and meanwhile a staggered constraint shear effect is generated in the thickness direction of the blank; by means of the design, the refining capacity of the structure can be enhanced, and the isotropic capacity of the rare earth magnesium alloy ring forge piece can be improved. The profile characteristics of the core roller are changed, the trapezoidal convex structures are added to form a sawtooth structure, the shear strain of a ring piece in the thickness direction is increased by utilizing the dislocation deformation principle, and grain refinement in the ring rolling process is more facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of roll forming, and more specifically relates to a core roller structure and a rare earth magnesium alloy ring roll forming method. Background Art

[0002] Magnesium alloy has a close-packed hexagonal structure, a relatively large c / a axis, lacks sufficient slip systems, and is mainly based on basal slip, resulting in too strong basal texture of magnesium alloy, small single-pass deformation, severe anisotropy, low plasticity and relatively poor formability; therefore, weakening the basal texture of magnesium alloy, eliminating or reducing low-melting point and coarse compounds, improving the plasticity of magnesium alloy, and developing high-formability processing technology for magnesium alloy are the main technical challenges facing the large-scale application of magnesium alloys. In recent years, the team of Academician Pan Fusheng of Chongqing University and the team of Academician Ding Wenjiang of Shanghai Jiaotong University have successfully developed a batch of high-plasticity rare earth magnesium alloy materials by adopting new alloy design ideas such as solid solution strengthening and plasticization; currently, magnesium rare earth alloy castings have been used as non-load-bearing components in engine casings, new missile cabins, aerospace vehicles, etc., achieving the goal of 20% weight reduction and greatly improving the combat and technical indicators of strategic and tactical weapons and equipment, so they are highly valued;

[0003] In order to further improve the key performance indicators such as the carrying capacity, speed, and range of new-generation strategic and tactical missiles and other weapons and equipment, its main load-bearing structure is planned to use heat-resistant rare earth magnesium alloy thin-walled ring forgings. Its overall forming technology is highly valued. However, due to the poor plasticity of magnesium alloy and the strong constraints on material flow caused by rolling forming, its overall forming is difficult, which is specifically manifested in the difficulty in stable control of structural dimensions, large discreteness of mechanical properties (large differences in radial strength, circumferential strength and axial strength), poor quality stability and other problems, which directly affect the delivery cycle of new-generation model products;

[0004] The material flow mode of the traditional rolling forming process of aluminum alloy, titanium alloy and nickel-based alloy leads to a strong texture tendency of magnesium alloy along the circumference of the ring forging during the deformation process. This strong texture is difficult to control through subsequent deformation or heat treatment, which ultimately leads to large differences in the mechanical properties of the ring forging in all directions, and the product performance does not meet the standards. In addition, the existing cylindrical core roller only produces compressive strain along the thickness direction of the ring blank, and cannot produce shear deformation effect along the thickness direction of the ring forging, and the grain refinement effect is very weak;

[0005] Therefore, studying a core roller structure that can improve the refinement ability of the organization, eliminate texture tendencies, and improve the isotropic performance of rare earth magnesium alloy ring forgings, as well as developing an integral rolling forming technology for heat-resistant rare earth magnesium alloy ring forgings that meets the shape / property control requirements are key technical challenges faced by the lightweight manufacturing of aerospace equipment. Summary of the invention

[0006] In view of this, the present invention provides a core roller structure and a rare earth magnesium alloy ring rolling forming method using the core roller structure, which can, on the one hand, significantly improve the microstructure refinement capability of the magnesium alloy material; on the other hand, can achieve three-dimensional regulation of the grain orientation of the magnesium alloy material, so that the grain orientation is not parallel to the circumference of the ring forging, which can greatly eliminate the strong texture of the magnesium alloy formed during the deformation process, while improving the grain refinement capability of the rolling forming and the overall mechanical properties of the ring forging.

[0007] In order to achieve the above object, the present invention adopts the following technical solution:

[0008] A core roller structure is characterized by comprising: a core roller body, and trapezoidal protrusions arranged at intervals along the axial direction of the outer wall of the core roller body.

[0009] The technical effects produced by adopting the above-mentioned technical scheme include at least: each time the core roller structure feeds the blank, a dislocated constrained shear effect is generated along the thickness direction of the blank, thereby enhancing the grain refinement effect; and this rolling deformation in the non-uniform stress field can significantly weaken the base surface texture of the rare earth magnesium alloy, significantly improve the formability, and significantly improve the anisotropy.

[0010] Furthermore, an angle θ between the hypotenuse of the trapezoidal protrusion and a tangent line at a connection between the hypotenuse and the outer wall of the core roller body satisfies 30° to 60°.

[0011] Furthermore, the distance between the two sides of the top of the trapezoidal protrusion and the vertical projection distance corresponding to the hypotenuse of the trapezoidal protrusion are both a, and a satisfies 0.75mm to 1.5mm.

[0012] Furthermore, the trapezoidal protrusions are evenly distributed axially along the outer wall of the core roller body, and the spacing b between the trapezoidal protrusions satisfies 0.75 mm to 1.5 mm.

[0013] The above technical scheme produces at least the following technical effects: some current technologies use upper and lower rollers for rolling of special-shaped cross-section materials, and the roller surfaces have grooves with small depth and width, so they can only suppress the elongation in the length direction, so that the fluctuation of the rolled parts is reduced. However, the present invention strictly limits the angle and size of the trapezoidal protrusions, and the values ​​are much larger than those of the prior art. The trapezoidal protrusions produce a shear effect within a limited range, and can penetrate the deformed material, thereby making the grain orientation of the ring forging after deformation realize the characteristics of three-dimensional distribution in space, avoiding the formation of a strong texture distribution along the circumference of the ring forging, thereby suppressing or eliminating anisotropy. Furthermore, within the limited range of the present invention, by changing the inclination angle and width of the core roller trapezoidal protrusion, the orientation of the rare earth magnesium alloy grains can be adjusted according to the actual situation, thereby optimizing the mechanical properties of the ring forgings, all of which have good mechanical property consistency and meet the actual use requirements.

[0014] The present invention also provides a rare earth magnesium alloy ring rolling forming method using the core roller structure, comprising the following steps:

[0015] S1: First, multi-directional forging is performed on the rare earth magnesium alloy (Mg-Gd-Y-Zn-Zr can be selected) ingot, the initial forging temperature does not exceed 450°C, the cumulative strain of multi-directional forging reaches 2.5-3.5, and each deformation is ensured to reach the critical deformation amount for dynamic recrystallization of the rare earth magnesium alloy, and the cumulative deformation amount of multi-directional forging reaches the critical deformation amount for geometric recrystallization of the material;

[0016] S2: The rare earth magnesium alloy forging is subjected to homogenization heat treatment at a temperature range of 420-450°C for ≥20h after blanking, and the blank after homogenization treatment is subjected to two roughening and drawing processes to prepare a round cake-shaped blank, and is punched to prepare a thick-walled ring blank; after two roughening and drawing processes, it is ensured that there are no coarse grains and mixed grains inside the forging, the uniformity of the grains is ≥95%, and there are no obvious hole-type defects;

[0017] S3: Before rolling forming, the main roller and core roller structure are preheated at 340-360℃, and the thick-walled ring blank is heated to 380-390℃, and kept warm for ≥2h to ensure that the temperature of the rare earth magnesium alloy ring forging plate is evenly distributed along the thickness direction;

[0018] S4: The entire core roller is a shearing zone. Assume that the circumference of the core roller is x, the size of the shearing unit is a, and the inner circumference of the blank is y. Then when y=nx+(2n+1)×a (n is an integer), the area sheared during the first deformation will be flattened during the second deformation. Correspondingly, the area flattened during the first deformation will be sheared during the second deformation, and this cycle will repeat alternately.

[0019] S5: The core roller is fed linearly at a speed of 0.5 mm / s to 1.2 mm / s in the direction close to the main roller. The trapezoidal protrusion of the core roller is used as a shearing unit to shear the blank. The size of the core roller shearing unit is a = 0.75 mm to 1.5 mm, the angle θ = 30 to 60°, and b = 0.75 mm to 1.5 mm, ensuring that the shear strain along the thickness direction can penetrate the central area of ​​the deformed material during each deformation process;

[0020] S6: When the total linear motion feed amount of the core roller reaches the required ring blank thickness reduction, that is, the total linear motion feed amount of the core roller is equal to the ring blank thickness reduction, the rare earth magnesium alloy ring is subjected to multi-stage quenching treatment to reduce the cracking tendency, wherein the deformed thin-walled rare earth magnesium alloy ring is first placed in 50-80°C water as a whole, kept warm for 20-30 minutes, and then transferred to room temperature water for cooling;

[0021] The rare earth magnesium alloy ring is subjected to aging treatment at 210-220°C for ≥20h; the ring after aging treatment is subjected to cold bulging treatment, the deformation is controlled within 1%, and the internal stress of the ring is eliminated;

[0022] According to GJB, samples were taken at intervals of 90 degrees on the upper and lower end surfaces of the rare earth magnesium alloy ring to measure the high and low magnification structures, mechanical properties and limit hardness.

[0023] The beneficial effects of adopting the above technical solution include at least:

[0024] The grain orientation of the formed rings in the prior art is always parallel to the circumference, and the mechanical properties in each direction differ by about 50MPa, resulting in anisotropy of the rings, and poor stability and safety in specific applications. The present invention proposes a rare earth magnesium alloy ring forging rolling forming process with constrained shear effect, in which each step cooperates with each other, and multi-directional forging and blanking makes the cumulative deformation reach the critical deformation for geometric recrystallization of the material. The homogenization heat treatment and roughing and drawing effectively improve the uniformity of the grains and avoid internal defects. The core roller preheating makes the temperature evenly distributed, and the core roller produces a dislocated constrained shear effect along the thickness direction of the blank. The orientation of the grains is no longer parallel to the circumference of the ring forging, which greatly reduces the strong texture of the magnesium alloy formed during the deformation process, and realizes the three-dimensional regulation of the grain orientation of the magnesium alloy material.

[0025] It can be seen from the above technical solutions that, compared with the prior art, the present invention provides a core roller structure and a rare earth magnesium alloy ring rolling forming method, which have the following technical effects and advantages:

[0026] The present invention proposes a rare earth magnesium alloy ring forging rolling forming process with constrained shear effect. On the one hand, it can significantly improve the microstructure refinement capability of the magnesium alloy material, with the initial microstructure ≥80μm and the fine-grained microstructure ≤8μm after rolling forming. On the other hand, it can realize three-dimensional regulation of the grain orientation of the magnesium alloy material. The deformation introducing the shear effect can greatly weaken the basal texture and improve the mechanical properties of the rare earth magnesium alloy ring forging. Even if the grain orientation is not parallel to the circumference of the ring forging, the strong texture of the magnesium alloy formed during the deformation process can be largely eliminated, while improving the grain refinement capability of the rolling forming and the overall mechanical properties of the ring forging.

[0027] A core roller structure designed according to the present invention changes the profile characteristics of the core roller, adds a trapezoidal protrusion structure to form a sawtooth structure, and utilizes the principle of dislocation deformation to increase the shear strain of the ring along the thickness direction, which is more conducive to grain refinement during the ring rolling process; and the core roller designed by the present invention is mainly used for the ring rolling forming of rare earth magnesium alloys, that is, the deformation of composite metals, that is, bimetallic rings. The dislocation effect formed by the trapezoidal protrusion structure on the surface of the core roller is an asymmetric deformation, which is conducive to eliminating the base surface texture tendency and improving the mechanical properties of the magnesium alloy ring. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0029] Figure 1 It is a schematic diagram of the structure of the magnesium alloy ring rolling of the present invention;

[0030] Figure 2 A top view of the magnesium alloy ring rolled according to the present invention;

[0031] Figure 3 It is a schematic diagram of the surface structure of the core roller structure of the present invention;

[0032] Figure 4 for Figure 3 Middle AA section;

[0033] Figure 5 It is a schematic diagram of the trapezoidal protrusion structure of the core roller structure of the present invention;

[0034] Figure 6 This is a schematic diagram of the first shear deformation principle of the magnesium alloy ring-shaped rolling forming process of the present invention, wherein the right side is an enlarged view of the C area;

[0035] Figure 7 The schematic diagram of the second shear deformation principle of the magnesium alloy ring-shaped rolling forming process of the present invention; the right side is an enlarged view of the C area, and from left to right are the dislocation effect, deformation effect, and final effect;

[0036] Figure 8 Schematic diagram of the principle of geometric recrystallization triggered by cumulative deformation during the multi-directional forging process of magnesium alloy in the present invention; from left to right, the geometric recrystallization occurs with increasing strain;

[0037] Fig. 9 The strain distribution diagram of the heat-resistant rare earth magnesium alloy ring during the rolling forming process of the present invention, wherein a is a traditional smooth cylindrical core roller, b is a core roller rolling forming with a half-circumferential shear profile feature, and c is a core roller rolling forming with a full-circumferential shear profile feature;

[0038] Fig.10 Schematic diagram of the initial fine-grained structure of magnesium alloy;

[0039] Fig.11 This is a schematic diagram of the fine grain structure of magnesium alloy after rolling;

[0040] Fig.12The schematic diagram of ring sampling is shown in Figure 1, where d is the sampling range;

[0041] Among them, 1 is a thick-walled ring blank; 2 is a core roller body; 3 is a main roller; and 4 is a trapezoidal protrusion. DETAILED DESCRIPTION

[0042] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] As attached Figure 3-5 As shown, the present invention proposes a core roller structure, which is characterized by comprising: a core roller body 2, and trapezoidal protrusions 4 axially spaced apart along the outer wall of the core roller body 2.

[0044] Each time the core roller structure of the present invention feeds, the blank is compressed and deformed, and a dislocated constrained shear effect is generated along the thickness direction of the blank, thereby enhancing the grain refinement effect. At the same time, the shear effect brought by the trapezoidal protrusions of the core roller structure can penetrate the deformed material, thereby enabling the grain orientation of the ring forging to achieve a three-dimensional distribution feature in space after deformation, thereby avoiding the formation of a strong texture distribution along the circumference of the ring forging, thereby suppressing or eliminating anisotropy; and the rolling deformation of this non-uniform stress field can significantly weaken the base surface texture of the rare earth magnesium alloy, significantly improve the formability, and significantly improve the anisotropy.

[0045] In the present invention, the bottom surface of the trapezoidal protrusion 4 is arc-shaped, consistent with the surface of the core roller body 2, and extends obliquely upward along both sides of the bottom surface parallel to the longitudinal direction of the core roller to form a platform.

[0046] In the present invention, the angle θ between the hypotenuse of the trapezoidal protrusion 4 and the tangent line at the connection between the hypotenuse and the outer wall of the core roller body 2 satisfies 30° to 60°.

[0047] In the present invention, the distance between the two sides of the top of the trapezoidal protrusion 4 and the vertical projection distance corresponding to the hypotenuse of the trapezoidal protrusion 4 are both a, and a satisfies 0.75 mm to 1.5 mm.

[0048] In the present invention, the trapezoidal protrusions 4 are evenly distributed along the axial direction of the outer wall of the core roller body 2, and the interval b between the trapezoidal protrusions 4 meets 0.75 mm to 1.5 mm.

[0049] By adopting the above technical scheme, the technical effects produced include at least: by changing the angle θ, width a and distance b of the core roller trapezoidal protrusion 4, the orientation of the rare earth magnesium alloy grains can be adjusted according to actual conditions, thereby optimizing the mechanical properties of the ring forging and meeting actual use requirements.

[0050] like Figure 1-2 As shown, the present invention provides a rare earth magnesium alloy ring rolling forming method using the core roller structure, comprising the following steps:

[0051] S1: First, multi-directional forging is performed on the rare earth magnesium alloy (Mg-Gd-Y-Zn-Zr can be selected) ingot, the initial forging temperature does not exceed 450°C, the cumulative strain of multi-directional forging reaches 2.5-3.5, and each deformation is ensured to reach the critical deformation amount for dynamic recrystallization of the rare earth magnesium alloy, and the cumulative deformation amount of multi-directional forging reaches the critical deformation amount for geometric recrystallization of the material;

[0052] S2: After blanking, the rare earth magnesium alloy forging is subjected to homogenization heat treatment in the temperature range of 420-450°C for ≥20h, and the blank after homogenization treatment is subjected to two roughening and drawing processes to prepare a round cake-shaped blank, and then punched to prepare a thick-walled ring blank; after two roughening and drawing processes, it is ensured that there are no coarse grains and mixed grains inside the forging, the uniformity of the grains is ≥95%, and there are no obvious hole-type defects;

[0053] S3: Before rolling forming, the main roller and core roller structure are preheated at 340-360℃, and the thick-walled ring blank is heated to 380-390℃ and kept warm for ≥2h to ensure that the temperature of the rare earth magnesium alloy ring forging plate is evenly distributed along the thickness direction;

[0054] S4: The entire core roller is a shearing zone. Assume that the circumference of the core roller is x, the size of the shearing unit is a, and the inner circumference of the blank is y. When y=nx+(2n+1)×a (n is an integer), the area sheared during the first deformation will be flattened during the second deformation. Correspondingly, the area flattened during the first deformation will be sheared during the second deformation, and this cycle will repeat alternately. The specific deformation dislocation principle is as follows: Figure 6-Figure 7 As shown, it is ensured that the magnesium alloy ring forging produces a full-domain shear effect along the thickness direction of the deformation zone every two revolutions. With the same strain as the cylindrical core roller, the shear deformation refinement effect is 5 to 10 times the general compression strain grain refinement effect.

[0055] S5: The core roller is fed linearly at a speed of 0.5 mm / s to 1.2 mm / s in the direction close to the main roller. The trapezoidal protrusion of the core roller is used as a shearing unit to shear the blank. The size of the core roller shearing unit is a = 0.75 mm to 1.5 mm, the angle θ = 30 to 60 degrees, and b = 0.75 mm to 1.5 mm, ensuring that the shear strain along the thickness direction can penetrate the central area of ​​the deformed material during each deformation process;

[0056] S6: When the total linear motion feed of the core roller reaches the process requirement, that is, the required ring blank thickness reduction is achieved, that is, the total linear motion feed of the core roller is equal to the ring blank thickness reduction, the rare earth magnesium alloy ring is subjected to multi-stage quenching treatment to reduce the cracking tendency, that is, the deformed thin-walled rare earth magnesium alloy ring is first placed in hot water at 50-80°C as a whole, kept warm for 20-30 minutes, and then transferred to room temperature water for cooling;

[0057] The rare earth magnesium alloy ring is subjected to aging treatment at 210-220°C for ≥20h; the ring after aging treatment is subjected to cold bulging treatment, the deformation is controlled within 1%, and the internal stress of the ring is eliminated;

[0058] like Fig.12 As shown, according to GJB, samples were taken at intervals of 90 degrees on the upper and lower end surfaces of the rare earth magnesium alloy ring to measure the high and low magnification structures, mechanical properties and limit hardness.

[0059] The specific working process of the core roller and the main roller on the rare earth magnesium alloy ring blank is as follows: the evenly heated ring blank is placed on the horizontal ring rolling equipment with a rolling force ≥ 250 tons, the main roller rotates clockwise at a constant speed of 30-35rpm, and the ring blank is placed on the base so that the ring blank and the core roller are basically concentric; then, the centering roller, the measuring roller and the axial frame are close to the ring blank; at the beginning of the rolling forming, the core roller gradually approaches the main roller through radial linear feed motion, the friction between the core roller and the blank will cause passive rotation, the ring is continuously deformed, and the diameter gradually expands.

[0060] In the rolling forming process of the rare earth magnesium alloy ring forging with constrained shearing effect of the present invention, the grain size of the forging after multi-directional forging in step S1 is ≤34 μm and the hardness is ≥60 HV.

[0061] In the embodiment, after the homogenization treatment in step S2, the average diameter of the nano-precipitated phase on the cylindrical surface of the forging blank is ≤29nm, and the hardness is ≥80HV.

[0062] In the embodiment, after the billet is subjected to two upsetting and drawing processes in step S2, a rare earth magnesium alloy forging billet with a grain size of ≤22 μm is obtained.

[0063] In the embodiment, the main roller is made of H13 hot working die steel, and the core roller is made of 5CrNiMo hot working die steel.

[0064] In the embodiment, in step S5, the global grain size of the ring forging after deformation is ≤8 μm, and the hardness is ≥90 HV.

[0065] In the embodiment, the hardness of the rare earth magnesium alloy ring obtained in step S6 is ≥110 HV.

[0066] In the embodiment, in step S8, the circumferential, axial and radial yield strengths of the ring forging are ≥410 MPa, and the difference in yield strengths in the three directions is ≤10 MPa; the circumferential, axial and radial elongations of the ring forging are ≥11%, and the difference in elongations in the three directions is ≤0.5%.

[0067] In the embodiment, the initial rare earth magnesium alloy ring blank has an inner diameter of 200 mm, an outer diameter of 280 mm, and a height of 150 mm; after the rolling forming, the ring forging has an inner diameter of 385 mm, an outer diameter of 432 mm, and a height of 150 mm. As long as the equipment allows, there is no restriction on the size.

[0068] Example 1

[0069] S1: First, the rare earth magnesium alloy (Mg-Gd-Y-Zn-Zr) ingot is forged by multi-directional forging, the initial forging temperature is 450℃, and the cumulative strain of multi-directional forging reaches 2.5;

[0070] S2: After the blank is opened, the rare earth magnesium alloy forging is subjected to homogenization heat treatment at 420°C for 20 hours, and the blank after homogenization treatment is subjected to two roughing and drawing processes to prepare a round cake-shaped blank, and then subjected to punching treatment to prepare a thick-walled ring blank;

[0071] S3: Before rolling forming, the main roller and the core roller are preheated at 340°C, and the thick-walled ring blank is heated to 390°C and kept warm for 2 hours;

[0072] S4: The entire core roller is a shearing zone. Assume that the circumference of the core roller is x, the size of the shearing unit is a, and the inner circumference of the blank is y. Then when y=nx+(2n+1)×a (n is an integer), the area sheared during the first deformation will be flattened during the second deformation. Correspondingly, the area flattened during the first deformation will be sheared during the second deformation, and this cycle will repeat alternately.

[0073] S5: The core roller makes a linear feed motion at a speed of 0.5 mm / s along the direction close to the main roller, with a total feed amount of 16.5 mm. The core roller shear unit size is a = 0.75 mm, the angle θ = 30 degrees, and the distance b = 0.75 mm;

[0074] S6: The total feed amount of the core roller in linear motion reaches the process requirement, that is, the required ring blank thickness reduction is 16.5 mm. First, the deformed thin-walled rare earth magnesium alloy ring is placed in 50°C water as a whole, kept warm for 20 minutes, and then transferred to room temperature water for cooling;

[0075] The rare earth magnesium alloy ring is subjected to aging treatment at 220°C for 20 hours, and the aging treated ring is subjected to cold bulging treatment;

[0076] According to GJB, samples were taken at intervals of 90 degrees on the upper and lower end surfaces of the rare earth magnesium alloy ring to measure the high and low magnification structures, mechanical properties and limit hardness.

[0077] In the rolling forming process of the rare earth magnesium alloy ring forging with constrained shear effect in this embodiment, the grain size of the forging after multi-directional forging in step S1 is 34 μm and the hardness is 60 HV.

[0078] In this embodiment, after the homogenization treatment in step S2, the average diameter of the nano-precipitated phase on the cylindrical surface of the forging blank is 29 nm and the hardness is 80 HV.

[0079] In this embodiment, after the blank is subjected to two upsetting and drawing processes in step S2, a rare earth magnesium alloy forging blank with a grain size of 22 μm is obtained.

[0080] In this embodiment, the main roller is made of H13 hot working die steel, and the core roller is made of 5CrNiMo hot working die steel.

[0081] In this embodiment, in step S5, the global grain size of the ring forging after deformation is 8 μm and the hardness is 90 HV.

[0082] In this embodiment, the hardness of the rare earth magnesium alloy ring obtained in step S6 is 110 HV.

[0083] In this embodiment, the circumferential, axial and radial yield strengths of the ring forging obtained in step S8 are all greater than 410 MPa, and the yield strengths in the three directions differ by less than 10 MPa; the circumferential, axial and radial elongations of the ring forging are 11%, 11.2% and 11.5% respectively, and the elongations in the three directions differ by 0.5%.

[0084] Example 2

[0085] S1: First, the rare earth magnesium alloy (Mg-Gd-Y-Zn-Zr) ingot is forged by multi-directional forging, the initial forging temperature is 450°C, and the cumulative strain of multi-directional forging reaches 3.5;

[0086] S2: After the blank is opened, the rare earth magnesium alloy forging is subjected to homogenization heat treatment at 450°C for 20 hours, and the blank after homogenization treatment is subjected to two roughing and drawing processes to prepare a round cake-shaped blank, and then subjected to punching treatment to prepare a thick-walled ring blank;

[0087] S3: Before rolling forming, the main roller and the core roller are preheated at 360°C, and the thick-walled ring blank is heated to 390°C and kept warm for 2 hours;

[0088] S4: The entire core roller is a shearing zone. Assume that the circumference of the core roller is x, the size of the shearing unit is a, and the inner circumference of the blank is y. Then when y=nx+(2n+1)×a (n is an integer), the area sheared during the first deformation will be flattened during the second deformation. Correspondingly, the area flattened during the first deformation will be sheared during the second deformation, and this cycle will repeat alternately.

[0089] S5: The core roller makes a linear feed motion at a speed of 1.2 mm / s along the direction close to the main roller. The size of the core roller shearing unit is a = 1.5 mm, the bottom angle θ = 45 degrees, and the distance b = 1.5 mm;

[0090] S6: The total feed amount of the core roller in linear motion meets the process requirements, that is, the required ring blank thickness reduction is 16.5 mm, wherein the deformed thin-walled rare earth magnesium alloy ring is first placed in 80°C water as a whole, kept warm for 20 minutes, and then transferred to room temperature water for cooling;

[0091] The rare earth magnesium alloy ring is subjected to aging treatment at 220°C for 20 hours; the ring after aging treatment is subjected to cold bulging treatment;

[0092] According to GJB, samples were taken at intervals of 90 degrees on the upper and lower end surfaces of the rare earth magnesium alloy ring to measure the high and low magnification structures, mechanical properties and limit hardness.

[0093] In the rolling forming process of the rare earth magnesium alloy ring forging with constrained shear effect in this embodiment, the grain size of the forging after multi-directional forging in step S1 is 29 μm and the hardness is 65 HV.

[0094] In this embodiment, after the homogenization treatment in step S2, the average diameter of the nano-precipitated phase on the cylindrical surface of the forging blank is 22 nm and the hardness is 82 HV.

[0095] In this embodiment, in step S2, after the billet is subjected to two upsetting and drawing processes, a rare earth magnesium alloy forging billet with a grain size of 18 μm is obtained.

[0096] In this embodiment, the main roller is made of H13 hot working die steel, and the core roller is made of 5CrNiMo hot working die steel.

[0097] In this embodiment, in step S5, the global grain size of the ring forging after deformation is 5 μm and the hardness is 95 HV.

[0098] In this embodiment, the hardness of the rare earth magnesium alloy ring obtained in step S6 is 120 HV.

[0099] In this embodiment, the circumferential, axial and radial yield strengths of the ring forging obtained in step S8 are all about 420 MPa; the circumferential, axial and radial elongations of the ring forging are 11.5%, 11.7% and 11.2% respectively, and the elongations in the three directions differ by 0.5%.

[0100] Comparative analysis with the traditional cylindrical core roller rolling forming of rare earth magnesium alloy rings:

[0101] (1) Finite element analysis and calculation were carried out on the rolling forming process of the rare earth magnesium alloy Mg-Gd-Y-Zn-Zr using a traditional cylindrical core roller and a core roller with a profile with dislocation constraint shear effect proposed in the present invention.

[0102] (2) The finite element calculation adopts the Hansel Spittel constitutive model, and the specific formula is as follows:

[0103]

[0104] Where A = 632.61, m1 = -5.07 × 10 -3 , m2=-4.36×10 -2 , m3=7.50×10 -2 , m4=-9.49×10 -3 .

[0105] (3) Set the main roller speed to 30 rpm, the core roller speed to 0.5-0.7 mm / s, the total feed to 16.5 mm (initial wall thickness 40 mm), and no lubrication (friction coefficient 0.4-0.8).

[0106] (4) The characteristic dimensions of the trapezoidal protrusion on the core roller surface: a = 1 mm, θ = 45 degrees, such as Figure 5 shown.

[0107] (5) Specific simulation of the strain distribution of the forming ring forging is as follows Fig. 9 As shown in the figure, it can be seen that the core roller with dislocation constrained shear characteristics produces greater tangential strain during the rolling process, which is more conducive to grain refinement and elimination of rare earth magnesium alloy texture tendency, and improves the comprehensive mechanical properties of rare earth magnesium alloy rings.

[0108] Experimental verification:

[0109] The heat-resistant rare earth magnesium alloy rings were formed by using the core roll mold with profile features and the hot aluminum alloy rolling forming process parameters. The final mechanical properties of the rings in the circumference, axial direction and radial direction were compared with those of the rings formed by the traditional cylindrical core roll, as shown in Table 1. The size and material of the traditional rings are the same as those in Example 2.

[0110] Table 1

[0111]

[0112] As can be seen from Table 1, the mechanical properties of the rare earth magnesium alloy ring formed by the core roller with periodic trapezoidal protrusion features are better, especially the axial and radial yield strengths are improved by about 20%; and the consistency of the circumferential, axial and radial mechanical properties is better, with the deviation within 10MPa; while the mechanical properties of the ring formed by the traditional scheme differ by about 50MPa in each direction, which will lead to anisotropy of the ring, which is not conducive to improving the stability and safety of the rare earth magnesium alloy projectile in flight.

[0113] A core roller structure designed according to the present invention changes the profile characteristics of the core roller, adds a trapezoidal protrusion structure to form a sawtooth structure, and utilizes the principle of dislocation deformation to increase the shear strain of the ring along the thickness direction, which is more conducive to grain refinement during the ring rolling process; and the core roller designed by the present invention is mainly used for the ring rolling forming of rare earth magnesium alloys, that is, the deformation of composite metals, that is, bimetallic rings. The dislocation effect formed by the trapezoidal protrusion structure on the surface of the core roller is an asymmetric deformation, which is conducive to eliminating the base surface texture tendency and improving the mechanical properties of the magnesium alloy ring.

[0114] Parts not described in detail in the embodiments of the present invention can be implemented using existing technologies and will not be described in detail here.

[0115] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0116] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A core roller structure, characterized in that: include: A core roller body and trapezoidal protrusions arranged at intervals along the outer wall of the core roller body in the axial direction.

2. A core roller structure according to claim 1, characterized in that: The angle θ between the hypotenuse of the trapezoidal protrusion and the tangent line at the connection between the hypotenuse and the outer wall of the core roller body is 30° to 60°.

3. A core roller structure according to claim 1, characterized in that: The distance between the two sides of the top of the trapezoidal protrusion and the vertical projection distance corresponding to the hypotenuse of the trapezoidal protrusion are both a, and a satisfies 0.75mm to 1.5mm.

4. A core roller structure according to claim 1, characterized in that: The trapezoidal protrusions are evenly distributed along the axial direction of the outer wall of the core roller body, and the spacing b between the trapezoidal protrusions is 0.75 mm to 1.5 mm.

5. A rare earth magnesium alloy ring rolling forming method, characterized in that: The following steps are involved: S1: multi-directional forging of rare earth magnesium alloy ingot; S2: homogenizing heat treatment, upsetting and stretching the rare earth magnesium alloy forging after blanking to make a round cake-shaped blank, and then punching it to prepare a thick-walled ring blank; S3: Before rolling forming, preheating the main roller and the core roller structure according to any one of claims 1 to 4, heating the thick-walled ring blank, and ensuring that the temperature of the rare earth magnesium alloy ring forging slab is evenly distributed along the thickness direction; S4: The entire core roller is a shearing zone. Assume that the circumference of the core roller is x, the size of the shearing unit is a, and the inner circumference of the blank is y. When y=nx+(2n+1)×a (n is an integer), the area sheared during the first deformation will be flattened during the second deformation. Correspondingly, the area flattened during the first deformation will be sheared during the second deformation, and this cycle will repeat alternately. S5: The core roller is fed linearly at 0.5 mm / s to 1.2 mm / s in a direction close to the main roller, and the trapezoidal protrusion of the core roller is used as a shearing unit to shear the blank; S6: When the total feed amount of the core roller in linear motion reaches the process requirements, the magnesium alloy ring is subjected to multi-stage quenching treatment, aging treatment, and sampling performance measurement.

6. A rare earth magnesium alloy ring rolling forming method according to claim 5, characterized in that: In the step S1, the initial forging temperature of the multi-directional forging blank does not exceed 450° C., and the accumulated strain of the multi-directional forging reaches 2.5 to 3.

5.

7. A rare earth magnesium alloy ring rolling forming method according to claim 5, characterized in that: The homogenization heat treatment in step S2 refers to heat treating the rare earth magnesium alloy forging at 420-450° C. for ≥20 h, and performing two upsetting and drawing operations on the blank.

8. The method for rolling a rare earth magnesium alloy ring according to claim 5, characterized in that: In the step S3, the temperature for preheating the main roller and the core roller structure is 340-360° C., and the temperature for heating the thick-walled ring blank is 380-390° C., and both are kept warm for ≥2 hours.

9. A rare earth magnesium alloy ring rolling forming method according to claim 5, characterized in that: The main roller is made of H13 hot working die steel, and the core roller is made of 5CrNiMo hot working die steel.

10. A rare earth magnesium alloy ring rolling forming method according to claim 5, characterized in that: The multi-stage quenching process in step S6 is to first put the deformed thin-walled rare earth magnesium alloy ring into 50-80°C water as a whole, keep it warm for 20-30 minutes, and then transfer it to room temperature water for cooling; The aging treatment process is to keep the rare earth magnesium alloy ring at 210-220°C for ≥20h; The sampling performance determination method is to sample at intervals of 90 degrees on the upper and lower end surfaces of the rare earth magnesium alloy ring according to GJB, and to determine the high and low magnification structures, mechanical properties and microhardness.

Citation Information

Patent Citations

  • Cold ring rolling forming method for double-flute section ring

    CN101829745A

  • Rolling forming method for bearing steel complex abnormal section annular element

    CN103143658A

  • Rolling and extruding combined forming method for ribbed thin-wall ring components with large height-diameter ratios

    CN106825341A

  • Periodic nonuniform rolling method for weakening texture of magnesium alloy plate

    CN109570233A

  • Preparation method of large-size rare earth magnesium alloy annular part

    CN114346139A