Heat-treatment-free low-pressure casting aluminum alloy, preparation method and application

By using amorphous powders of La, V and B in aluminum alloys to form LaB6 and (V, Al)B2 particles, the quality problems after heat treatment and silicon poisoning problems in low-pressure casting process are solved, and the high mechanics of heat-free aluminum alloys are realized. Performance and stability, suitable for battery pallet materials for new energy vehicles.

CN119020645AActive Publication Date: 2024-11-26KUNSHAN JINGWEI NEW MATERIALS RES INST CO LTD +2

Patent Information

Application Number
CN202411104779.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-26
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

In the existing low-pressure casting process, quality problems such as surface bubbles and product deformation often occur after heat treatment of aluminum alloys, and the use of deteriorating agents can easily lead to "silicon poisoning" and affect the alloy performance.

Method used

Al-2La-3V-3B amorphous particles were prepared by the belt-shrinking method using amorphous powder of La, V and B as a metamorphic agent, and added to an aluminum alloy to avoid silicon poisoning, forming LaB6 and (V, Al)B2. Particles improve the hardness and mechanical properties of the alloy and achieve heat-free treatment.

Benefits of technology

High strength and toughness can be obtained without heat treatment, with yield strength exceeding 160MPa, tensile strength exceeding 300MPa, and elongation exceeding 8%. It is suitable for battery pallet materials for new energy vehicles, meeting the needs of lightweight and avoiding silicon poisoning.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a heat-treatment-free low-pressure casting aluminum alloy, a preparation method and application. Relates to the technical field of low-pressure casting. The heat-treatment-free low-pressure casting aluminum alloy comprises the following components in percentage by weight: 4.0 to 10.5 percent of Si, 0 to 1.0 percent of Fe, 0.1 to 0.8 percent of Mn, 0 to 0.6 percent of Mg, 0.022 to 0.22 percent of La, 0.033 to 0.33 percent of V, 0.033 to 0.33 percent of B and the balance of Al, the mass ratio of La to V to B is 2: 3: 3. The elements La, V and B can prevent the high-silicon aluminum alloy from generating'silicon poisoning ', the nucleation efficacy of LaB6 and (V, Al) B2 particles cannot be affected by the solute Si element, the LaB6 and (V, Al) B2 particles can be directly used as heterogeneous nucleation points of alpha-Al, the degree of supercooling needed by nucleation is reduced, the solidification efficiency of the alloy is improved, grain refinement is promoted, and the mechanical property of the alloy is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of low-pressure casting, and in particular to a heat-treatment-free low-pressure casting aluminum alloy, a preparation method and an application thereof. Background Art

[0002] In the era of energy conservation, emission reduction, low carbon and environmental protection, lightweighting has become the main theme of the development of the global automobile industry. For every 100 kg reduction in fuel vehicles, the fuel consumption per 100 kilometers can be reduced by 0.3-0.6 liters; for every 10 kg reduction in the weight of pure electric vehicles, the cruising range can be increased by 2.5 kilometers; the "carbon reduction" effect brought about by weight reduction is very considerable. "Replacing steel with aluminum" is one of the most effective ways to achieve lightweighting of automobiles, which has also led to an increasing proportion of various parts represented by aluminum alloys in automobiles.

[0003] In addition to high-pressure casting, low-pressure casting is another aluminum alloy casting technology that is widely used in the automotive and aerospace fields. In addition to producing chassis structural parts such as automobile wheels, steering knuckles, and control arms, low-pressure casting can also be used to cast large integrated castings, such as subframes, battery tray brackets, etc. The comprehensive cost of equipment and molds used for large-scale integrated low-pressure casting is only about one-tenth of that of high-pressure casting, which has significant economic advantages. However, large-scale integrated low-pressure castings will produce quality problems such as surface bubbles and product deformation after heat treatment, which increases the defective rate of aluminum castings and causes cost waste.

[0004] At present, in order to prepare aluminum alloy castings that do not require heat treatment, modifiers such as strontium (Sr), scandium (Sc) and aluminum-titanium-boron (Al-Ti-B) are usually added to the alloy composition. These modifiers have a significant effect in improving the properties of aluminum alloys, such as grain refinement and improved mechanical properties. However, in practice, the use of modifiers often leads to the phenomenon of "silicon poisoning". This is because these elements may form stable compounds in alloys with high silicon content, resulting in uneven distribution of silicon phase or grain coarsening, thus affecting the overall performance of the alloy.

[0005] Therefore, it is particularly important to develop a new type of aluminum alloy that does not require heat treatment, avoid the occurrence of silicon poisoning, and achieve the excellence of aluminum alloy castings without compromising the quality of the silicon phase. Summary of the invention

[0006] In view of the technical problems existing in the prior art, the present invention aims to provide a heat-treatment-free low-pressure casting aluminum alloy, a preparation method and an application thereof.

[0007] One of the purposes of the present invention is to provide a heat-treatment-free low-pressure casting aluminum alloy, wherein the heat-treatment-free low-pressure casting aluminum alloy components include, by weight percentage: Si: 4.0-10.5%, Fe: 0~1.0%, Mn: 0.1~0.8%, Mg: 0~0.6%, La: 0.022~0.22%, V: 0.033~0.33%, B: 0.033~0.33%, the balance is Al; Among them, the mass ratio of La, V and B is 2:3:3.

[0008] Preferably, the La, V and B are added to the alloy in the form of Al-2La-3V-3B amorphous powder, and the Al-2La-3V-3B amorphous particle size is 20-30 μm.

[0009] Preferably, the Al-2La-3V-3B amorphous powder is prepared by a belt spinning method, and the preparation method comprises: The Al-2La-3V-3B alloy foil strip was first prepared by a belt spinning machine, and then the alloy foil strip was ball milled by a crusher to obtain Al-2La-3V-3B amorphous powder.

[0010] Preferably, the rotation speed of the strip spinning machine is 2200-2800 r / min, and the thickness of the prepared alloy foil strip is 20-30 μm and the width is 1.8-2.2 mm.

[0011] Preferably, the crusher mills the alloy foil strip under argon gas conditions, and the crusher rotation speed is 2500-3500 r / min.

[0012] A second object of the present invention is to provide a method for preparing a heat-treatment-free low-pressure casting aluminum alloy, the preparation method comprising: S1 alloy smelting: batch the ingredients according to the weight percentage of the components, first melt the pure aluminum ingot, heat the aluminum liquid to 750-760℃, add pure silicon and aluminum-manganese alloy in turn, and keep it for 25 minutes; continue to adjust the aluminum liquid temperature at 720-730℃, add pure magnesium ingot, and melt the aluminum liquid I; S2 refining: using the graphite rotary injection method, adding refining agent and high-purity argon into the aluminum liquid I at 720-730°C to obtain aluminum liquid II; S3 modification treatment: adjust the temperature of aluminum liquid II to 710-720℃, add Al-2La-3V-3B amorphous substance into aluminum liquid II by graphite rotary blowing method, continue to pass argon gas and rotate and stir for 5-8 minutes after adding, and obtain aluminum liquid III; S4 low pressure casting: The pressure is 500-1000mbar to obtain aluminum alloy castings.

[0013] Preferably, the amount of the refining agent is 2% of the total weight of the aluminum liquid II, the blowing time is 6 minutes, and after the refining is completed, it is allowed to stand for 2 to 3 minutes, and the refining process is repeated twice.

[0014] Preferably, the refining agent includes one or more of Rand high aluminum alloy refining agent-AJ2A, Yili aluminum alloy powder spray refining and slag cleaning agent DLJ-5 or Promag refining agent.

[0015] Preferably, during the low-pressure casting process, when the aluminum liquid III enters the mold, the aluminum liquid temperature is 700-710°C, the mold cavity temperature is 300-350°C, and the temperature at the gate and the diverter cone is 450-500°C.

[0016] The third object of the present invention is to provide a heat-treatment-free low-pressure cast aluminum alloy for use in a battery tray for a new energy vehicle.

[0017] Beneficial effects of the present invention: The invention provides a heat treatment-free low-pressure casting aluminum alloy, wherein the components thereof include, by weight percentage, Si: 4.0-10.5%, Fe: 0-1.0%, Mn: 0.1-0.8%, Mg: 0-0.6%, La: 0.022-0.22%, V: 0.033-0.33%, B: 0.033-0.33%, and the balance is Al; wherein the mass ratio of La, V and B is 2:3:3.

[0018] On the one hand, the addition of La, V and B elements can avoid the "silicon poisoning" phenomenon caused by the use of modifiers such as strontium (Sr), scandium (Sc) and aluminum-titanium-boron (Al-Ti-B) in high-silicon aluminum alloys with Si content greater than 8.0%. On the other hand, La reacts with B to form LaB6, and V reacts with Al and B to form (V, Al) B2. These LaB6 and (V, Al) B2 particles are highly stable in the Al-Si alloy melt and have a small lattice mismatch, which means that the particles form a stable interface with the matrix and reduce the interface energy. This characteristic enhances the bonding strength between the particles and the matrix and improves the hardness and strength of the alloy. LaB6 and (V, Al) B2 particles directly serve as heterogeneous nucleation sites for α-Al, reducing the supercooling required for nucleation. This effect not only improves the solidification efficiency of the alloy, but also promotes grain refinement. In addition, the nucleation efficiency of LaB6 and (V, Al) B2 particles will not be affected by the solute Si element, so they have an excellent grain refining effect in high-silicon aluminum alloys to improve the mechanical properties of the alloy.

[0019] Due to the heterogeneous nucleation effect and grain refinement effect of the particles, the low-pressure cast aluminum alloy prepared by the present invention can achieve high strength and toughness without heat treatment, with a yield strength of >160MPa, a tensile strength of >300MPa, and an elongation of >8%. It can replace steel as a battery tray material for new energy vehicles and meet the demand for lightweight new energy vehicles. DETAILED DESCRIPTION

[0020] According to the first aspect of the present invention, a heat treatment-free low-pressure casting aluminum alloy is provided, wherein the heat treatment-free low-pressure casting aluminum alloy components include, by weight percentage: Si: 4.0-10.5%, Fe: 0~1.0%, Mn: 0.1~0.8%, Mg: 0~0.6%, La: 0.022~0.22%, V: 0.033~0.33%, B: 0.033~0.33%, the balance is Al; Among them, the mass ratio of La, V and B is 2:3:3.

[0021] In the present invention, the addition of La, V and B elements can avoid the "silicon poisoning" phenomenon caused by the use of modifiers such as strontium (Sr), scandium (Sc) and aluminum-titanium-boron (Al-Ti-B) in high-silicon aluminum alloys with a Si content greater than 8.0%. La reacts with B to form LaB6, and V reacts with Al and B to form (V, Al) B2. These LaB6 and (V, Al) B2 particles are highly stable in the Al-Si alloy melt and have a small lattice mismatch, which means that the particles form a stable interface with the matrix and reduce the interface energy. This characteristic enhances the bonding strength between the particles and the matrix and improves the hardness and strength of the alloy. LaB6 and (V, Al) B2 particles directly serve as heterogeneous nucleation sites for α-Al, reducing the supercooling required for nucleation. This effect not only improves the solidification efficiency of the alloy, but also promotes grain refinement. In addition, the nucleation efficiency of LaB6 and (V, Al) B2 particles will not be affected by the solute Si element, so they have an excellent grain refining effect in high-silicon aluminum alloys to improve the mechanical properties of the alloy.

[0022] In the present invention, the addition of Mn element can transform the needle-shaped iron-containing phase into a Chinese character-shaped or fine spherical α-Fe phase, greatly improving the adverse effects of Fe and improving the toughness and corrosion resistance of the alloy.

[0023] In the present invention, the weight percentage of Si is, for example, 4.0%, 4.5%, 5.0%, 5.5%, 6.0%, 6.5%, 7.0%, 7.5%, 8.0%, 8.5%, 9.0%, 9.5%, 10.0% or 10.5%; the weight percentage of Fe is, for example, 0.03%, 0.05%, 0.10%, 0.20%, 0.30%, 0.40%, 0.50%, 0.60%, 0.70%, 0.80%, 0.90% or 1.0 %; the weight percentage of Mn is, for example, 0.10%, 0.15%, 0.2%, 0.25%, 0.30%, 0.35%, 0.40%, 0.45%, 0.50%, 0.55%, 0.60%, 0.65%, 0.70%, 0.75% or 0.80%; the weight percentage of Mg is, for example, 0.05%, 0.10%, 0.15%, 0.2%, 0.25%, 0.30%, 0.35%, 0.40%, 0.45%, 0.5 0%, 0.55% or 0.60%; the weight percentage of La is, for example, 0.022%, 0.025%, 0.030%, 0.035%, 0.040%, 0.045%, 0.050%, 0.055%, 0.060%, 0.065%, 0.070%, 0.075%, 0.080%, 0.085%, 0.090%, 0.095%, 0.10%, 0.11%, 0.15%, 0.17%, 0.19%, 0. .20% or 0.22%; the weight percentage of V is, for example, 0.033%, 0.066%, 0.099%, 0.132%, 0.165%, 0.198%, 0.231%, 0.264%, 0.297% or 0.33%; the weight percentage of B is, for example, 0.033%, 0.066%, 0.099%, 0.132%, 0.165%, 0.198%, 0.231%, 0.264%, 0.297% or 0.33%.

[0024] In a preferred embodiment of the present invention, the La, V and B are added to the alloy in the form of Al-2La-3V-3B amorphous powder, and the Al-2La-3V-3B amorphous particle size is 20-30 μm.

[0025] In the present invention, the amorphous material has a low melting point, is easy to cast, and has a uniformly distributed organizational structure and an isotropic internal structure. It is added to the aluminum alloy in the form of amorphous powder to make the aluminum alloy have good mechanical properties and processing properties. The amorphous structure also has higher stability and uniformity, and can better disperse the added elements La, V and B, effectively prevent the aggregation of the added elements in the aluminum alloy, and avoid the formation of local high-concentration areas, thereby achieving a more uniform distribution of components and better performance improvement in the aluminum alloy.

[0026] In a preferred embodiment of the present invention, the Al-2La-3V-3B amorphous powder is prepared by a belt spinning method, and the preparation method comprises: The Al-2La-3V-3B alloy foil was first prepared by a belt spinning machine, and then the alloy foil was ball milled by a crusher to obtain Al-2La-3V-3B amorphous powder.

[0027] In the present invention, the belt-spinning method can achieve rapid cooling and spinning refinement. The LaB6 and (V, Al)B2 particles in the Al-2La-3V-3B amorphous material obtained by this method are more uniform and fine in size, can be quickly added to the aluminum alloy melt, and are more evenly distributed in the matrix, avoiding the problem of La element not being able to be added.

[0028] In a preferred embodiment of the present invention, the rotation speed of the strip spinning machine is 2200-2800 r / min, and the thickness of the prepared alloy foil strip is 20-30 μm and the width is 1.8-2.2 mm; In the present invention, the prepared alloy foil strip has a thickness of, for example, 20 μm, 21 μm, 22 μm, 23 μm, 24 μm, 25 μm, 26 μm, 27 μm, 28 μm, 29 μm or 30 μm; and a width of, for example, 1.8 mm, 1.9 mm, 2.0 mm, 2.1 mm or 2.2 mm.

[0029] In a preferred embodiment of the present invention, the crusher ball mills the alloy foil strip under argon gas conditions, and the crusher rotation speed is 2500-3500 r / min.

[0030] In the present invention, the crusher ball mills the alloy foil under argon conditions, and the crusher rotation speed is 2500r / min, 2600r / min, 2700r / min, 2800r / min, 2900r / min, 3000r / min, 3100r / min, 3200r / min, 3300r / min, 3400r / min or 3500r / min.

[0031] In the present invention, the preparation of Al-2La-3V-3B amorphous powder by the belt spinning method specifically includes: First, pure aluminum ingots, Al-10La, Al-5V and Al-3B master alloys were cut into uniform small pieces and loaded into a customized quartz tube with a φ3mm hole at the bottom. The position of the quartz tube was adjusted so that the master alloy was in the center of the induction coil. The height of the quartz tube from the surface of the copper roller was adjusted to 3-5mm, and the surface of the copper roller was polished to a bright finish using fine sandpaper and metal polishing paste. Then, the chamber of the belt spinning machine was evacuated to a 3×10 -3Pa vacuum state; adjust the copper roller speed to 2200~2800 r / min, control the pressure difference between the cavity and the spray gun to 20~40Pa, start the high-frequency induction power supply, adjust the induction coil current to 20A, and adjust the melting temperature to 1050℃; after the alloy is completely melted, keep it warm for 30 minutes, turn on the injection switch, use the pressure difference to spray the melt on the copper roller, and form an alloy foil strip under rapid cooling and high speed. The prepared alloy foil strip samples are collected by the collection tube. Under this working condition, the thickness of the alloy foil strip samples prepared by the belt spinning machine is generally about 20~30μm and the width is 1.8~2.2mm. The alloy foil strip samples prepared by the belt spinning machine are placed in a crusher in a glove box filled with argon gas, and the powder is taken out by ball milling at a speed of 2500~3500r / min for 15 minutes, thereby obtaining Al-2La-3V-3B amorphous.

[0032] According to a second aspect of the present invention, a method for preparing a heat-treatment-free low-pressure casting aluminum alloy is provided, the preparation method comprising: S1 alloy smelting: batch the ingredients according to the weight percentage of the components, first melt the pure aluminum ingot, heat the aluminum liquid to 750-760℃, add pure silicon and aluminum-manganese alloy in turn, and keep it for 25 minutes; continue to adjust the aluminum liquid temperature at 720-730℃, add pure magnesium ingot, and melt the aluminum liquid I; S2 refining: using the graphite rotary injection method, adding refining agent and high-purity argon into the aluminum liquid I at 720-730°C to obtain aluminum liquid II; S3 modification treatment: adjust the temperature of aluminum liquid II to 710-720℃, add Al-2La-3V-3B amorphous substance into aluminum liquid II by graphite rotary blowing method, continue to pass argon gas and rotate and stir for 5-8 minutes after adding, and obtain aluminum liquid III; S4 low pressure casting: The pressure is 500-1000mbar to obtain aluminum alloy castings.

[0033] In a preferred embodiment of the present invention, the amount of the refining agent is 2% of the total weight of the aluminum liquid II, the blowing time is 6 minutes, and after the refining is completed, it is allowed to stand for 2 to 3 minutes, and the refining process is repeated twice.

[0034] In a preferred embodiment of the present invention, the refining agent includes one or more of Rand high aluminum alloy refining agent-AJ2A, Yili aluminum alloy powder spray refining and slag cleaning agent DLJ-5 or Promag refining agent.

[0035] In the present invention, the refining agent includes, for example, RAND high aluminum alloy refining agent-AJ2A, Yili aluminum alloy powder spray refining and slag cleaning agent DLJ-5, Promag refining agent, RAND high aluminum alloy refining agent-AJ2A and Yili aluminum alloy powder spray refining and slag cleaning agent DLJ-5, RAND high aluminum alloy refining agent-AJ2A and Promag refining agent, or a combination of Yili aluminum alloy powder spray refining and slag cleaning agent DLJ-5 and Promag refining agent.

[0036] In a preferred embodiment of the present invention, during the low-pressure casting process, when the aluminum liquid III enters the mold, the aluminum liquid temperature is 700-710°C, the mold cavity temperature is 300-350°C, and the temperature at the gate and the diverter cone is 450-500°C.

[0037] In the present invention, the method for preparing the heat-treatment-free low-pressure casting aluminum alloy specifically comprises: (1) Preparation of Al-2La-3V-3B amorphous powder First, pure aluminum ingots, Al-10La, Al-5V and Al-3B master alloys were cut into uniform small pieces and loaded into a customized quartz tube with a φ3mm hole at the bottom. The position of the quartz tube was adjusted so that the master alloy was in the center of the induction coil. The height of the quartz tube from the copper roller surface was adjusted to 4mm, and the copper roller surface was polished to a bright finish using fine sandpaper and metal polishing paste. Then, the chamber of the belt spinning machine was evacuated to a 3×10 -3 Pa vacuum state; adjust the copper roller speed to 2500 r / min, control the pressure difference between the cavity and the spray gun to 30Pa, start the high-frequency induction power supply, adjust the induction coil current to 20A, and adjust the melting temperature to 1050℃; after the alloy is completely melted, keep it warm for 30 minutes, turn on the injection switch, use the pressure difference to spray the melt on the copper roller, and form an alloy foil strip under rapid cooling and high speed. The prepared alloy foil strip samples are collected by the collection tube. Under this working condition, the thickness of the alloy foil strip sample prepared by the belt spinning machine is generally about 25μm and the width is 2.0mm. The alloy foil strip sample prepared by the belt spinning machine is placed in a crusher in a glove box filled with argon gas, and the powder is taken out at a speed of 3000r / min for 15 minutes to obtain Al-2La-3V-3B amorphous.

[0038] (2) Alloy smelting: ① According to the material components and weight percentage of each component of the heat treatment-free low-pressure casting aluminum alloy material, industrial pure aluminum, industrial crystalline silicon, pure magnesium ingot, aluminum-manganese alloy, and Al-2La-3V-3B amorphous are weighed as raw materials to prepare the aluminum alloy.

[0039] ② Check the materials and tools to ensure they are clean and dry, then place the pure aluminum ingot into the crucible and heat it with electricity.

[0040] ③After all the pure aluminum ingots are melted, heat it to 730℃ and scrape off the scum on the surface.

[0041] ④ Raise the temperature of aluminum liquid to 750~760℃, add pure silicon, aluminum-manganese and other alloys in batches, and maintain for 25 minutes. During this period, continue stirring to accelerate the melting and diffusion of alloy elements.

[0042] ⑤ Adjust the temperature of the aluminum liquid to 720~730℃, add pure magnesium ingot, and press it under the aluminum liquid to melt.

[0043] ⑥After all the above ingredients are melted, the aluminum liquid temperature is 730℃, and the slag is stirred and removed.

[0044] (3) Melt treatment: ① The first refining: The aluminum liquid temperature is 720-730℃, and graphite rotary spraying and powder blowing are used to purify the aluminum liquid. The refining gas is high-purity argon. The amount of refining agent is 2% of the total weight of the aluminum liquid. The refining time is 6 minutes. After the refining is completed, let it stand for 2-3 minutes and completely remove the slag.

[0045] ② Second refining: The temperature of the aluminum liquid is 720-730℃. Graphite rotary spraying and powder blowing are used to purify the aluminum liquid. High-purity argon is used as the refining gas. The amount of refining agent is 2% of the total weight of the aluminum liquid. The refining time is 6 minutes. After the refining is completed, let it stand for 2-3 minutes and completely remove the slag.

[0046] ③ The aluminum liquid temperature is 710~720℃, and Al-2La-3V-3B amorphous powder is added by graphite rotary blowing. After the amorphous powder is added, continue to rotate and stir with argon for 5~8 minutes to accelerate the melting and diffusion of the alloy elements.

[0047] ④ Check the composition of the aluminum liquid. If it passes the test, let the aluminum liquid stand for 20 minutes.

[0048] (4) Casting production ① Mold preparation: The surface of the mold cavity needs to be cleaned and placed in a mold heating furnace for 2 hours at a temperature of 250°C. After the mold is taken out of the furnace, spray insulation coating on the aluminum liquid runner and riser, spray thermal conductive coating in the product cavity, and then put it into the mold heating furnace for insulation for 30 minutes.

[0049] ② Casting production: The temperature of the casting aluminum liquid is controlled at 700~710℃, and the mold is heated with a professional mold baking device. The mold cavity temperature is controlled at 300~350℃, and the mold inlet and diverter cone are heated to 450~500℃; when the mold is opened for production for the first time, all cooling water pipes are closed. When the fifth mold is produced, two 20-mesh filters are placed at the riser position, all cooling water pipes are opened, and the cooling water temperature is controlled at 28~30℃, the cooling water pressure is 0.4~0.55MPa, and the cooling gas pressure is 0.6~0.8MPa; the pressure of the low-pressure casting machine is set to 700mbar, the pressurization time is 30S, and the low-pressure aluminum alloy casting is obtained after holding the pressure for 120S.

[0050] ③ Post-processing: Place the produced low-pressure aluminum alloy castings into a 30~35℃ cooling water pool for cooling for 15S, then take them out and remove the pouring riser and flash.

[0051] (5) Tensile test: After the treated low-pressure aluminum alloy castings are placed for 24 hours, test bars are prepared for tensile testing.

[0052] The third object of the present invention is to provide an application of the heat-treatment-free low-pressure cast aluminum alloy as described above in a battery tray for new energy vehicles.

[0053] Example 1 (1) Alloy smelting: ① According to the material composition of the heat treatment-free low-pressure casting aluminum alloy material and the weight percentage of each component, Si: 8.5%, Fe < 0.05%, Mn: 0.5%, Mg: 0.35%, La: 0.11%, V: 0.165% and B: 0.165%, the balance is Al, industrial pure aluminum, industrial crystalline silicon, pure magnesium ingot, aluminum-manganese alloy, Al-2La-3V-3B amorphous material are weighed as raw materials to prepare the aluminum alloy.

[0054] ② Check the materials and tools to ensure they are clean and dry, then place the pure aluminum ingot into the crucible and heat it with electricity.

[0055] ③After all the pure aluminum ingots are melted, heat it to 730℃ and scrape off the scum on the surface.

[0056] ④ Raise the temperature of aluminum liquid to 750~760℃, add pure silicon, aluminum-manganese and other alloys in batches, and maintain for 25 minutes. During this period, continue stirring to accelerate the melting and diffusion of alloy elements.

[0057] ⑤ Adjust the temperature of the aluminum liquid to 720~730℃, add pure magnesium ingot, and press it under the aluminum liquid to melt.

[0058] ⑥After all the above ingredients are melted, the aluminum liquid temperature is 730℃, and the slag is stirred and removed.

[0059] (2) Melt treatment: ① The first refining: The aluminum liquid temperature is 720-730℃, and graphite rotary spraying and powder blowing are used to purify the aluminum liquid. The refining gas is high-purity argon. The amount of refining agent is 2% of the total weight of the aluminum liquid. The refining time is 6 minutes. After the refining is completed, let it stand for 2-3 minutes and completely remove the slag.

[0060] ② Second refining: The temperature of the aluminum liquid is 720-730℃. Graphite rotary spraying and powder blowing are used to purify the aluminum liquid. High-purity argon is used as the refining gas. The amount of refining agent is 2% of the total weight of the aluminum liquid. The refining time is 6 minutes. After the refining is completed, let it stand for 2-3 minutes and completely remove the slag.

[0061] ③ The aluminum liquid temperature is 710~720℃, and Al-2La-3V-3B amorphous powder is added by graphite rotary blowing. After the amorphous powder is added, continue to rotate and stir with argon for 5-8 minutes to accelerate the melting and diffusion of the alloy elements.

[0062] ④ Check the composition of the aluminum liquid. If it passes the test, let the aluminum liquid stand for 20 minutes.

[0063] (3) Casting production ① Mold preparation: The surface of the mold cavity needs to be cleaned and placed in a mold heating furnace for 2 hours at a temperature of 250°C. After the mold is taken out of the furnace, spray insulation coating on the aluminum liquid runner and riser, spray thermal conductive coating in the product cavity, and then put it into the mold heating furnace for insulation for 30 minutes.

[0064] ② Casting production: The temperature of the casting aluminum liquid is controlled at 700~710℃, and the mold is heated with a professional mold baking device. The mold cavity temperature is controlled at 300~350℃, and the mold inlet and diverter cone are heated to 450~500℃; when the mold is opened for production for the first time, all cooling water pipes are closed. When the fifth mold is produced, two 20-mesh filters are placed at the riser position, all cooling water pipes are opened, and the cooling water temperature is controlled at 28~30℃, the cooling water pressure is 0.4~0.55MPa, and the cooling gas pressure is 0.6~0.8MPa; the pressure of the low-pressure casting machine is set to 700mbar, the pressurization time is 30S, and the low-pressure aluminum alloy casting is obtained after holding the pressure for 120S.

[0065] ③ Post-processing: Place the produced low-pressure aluminum alloy castings into a 30~35℃ cooling water pool for cooling for 15S, then take them out and remove the pouring riser and flash.

[0066] (5) Tensile test: After the treated low-pressure aluminum alloy castings are placed for 24 hours, test bars are prepared for tensile testing.

[0067] Example 2 ① According to the material composition of the heat treatment-free low-pressure casting aluminum alloy material and the weight percentage of each component, Si: 6.0%, Fe < 0.05%, Mn: 0.35%, Mg: 0.35%, La: 0.022%, V: 0.033% and B: 0.033%, the balance is Al, industrial pure aluminum, industrial crystalline silicon, pure magnesium ingot, aluminum-manganese alloy, Al-2La-3V-3B amorphous material are weighed as raw materials to prepare the aluminum alloy.

[0068] The remaining steps and parameters are consistent with those in Example 1.

[0069] Example 3 According to the material composition of the heat-treatment-free low-pressure casting aluminum alloy material and the weight percentage of each component, Si: 10.5%, Fe < 0.05%, Mn: 0.60%, Mg: 0.35%, La: 0.22%, V: 0.33% and B: 0.33%, and the balance is Al, industrial pure aluminum, industrial crystalline silicon, pure magnesium ingot, aluminum-manganese alloy, and Al-2La-3V-3B amorphous are weighed as raw materials to prepare the aluminum alloy.

[0070] The remaining steps and parameters are consistent with those in Example 1.

[0071] Comparative Example 1 According to the material composition of the heat-treatment-free low-pressure casting aluminum alloy material and the weight percentage of each component, Si: 8.5%, Fe < 0.05%, Mn: 0.50% and Mg: 0.35% with the remainder being Al, industrial pure aluminum, industrial crystalline silicon, pure magnesium ingot and aluminum-manganese alloy are weighed as raw materials to prepare the aluminum alloy.

[0072] The remaining steps and parameters are consistent with those in Example 1.

[0073] Comparative Example 2 According to the material composition of the heat-treatment-free low-pressure casting aluminum alloy material and the weight percentage of each component, Si: 8.5%, Fe < 0.05%, Mn: 0.50%, Mg: 0.35%, Sr: 0.10%, and the balance is Al, the aluminum alloy is formulated.

[0074] The remaining steps and parameters are consistent with those in Example 1.

[0075] Comparative Example 3 According to the material composition of the heat-treatment-free low-pressure casting aluminum alloy material and the weight percentage of each component, Si: 8.5%, Fe < 0.05%, Mn: 0.50% and Mg: 0.35% and Al-Ti-B: 0.10%, and the balance is Al, the aluminum alloy is formulated.

[0076] The remaining steps and parameters are consistent with those in Example 1.

[0077] Comparative Example 4 A common commercial A356 low-pressure casting aluminum alloy material is prepared according to the material composition of the heat-treatment-free low-pressure casting aluminum alloy material and the weight percentage of each component: Si: 7.0%, Fe < 1.5%, Ti: 0.10% and Mg: 0.30%, and the balance is Al.

[0078] The remaining steps and parameters are consistent with those in Example 1.

[0079] Performance Testing The performance test is carried out in accordance with GB / T 228.1 "Tensile test of metallic materials Part 1: Room temperature test method Tensile test of metallic materials".

[0080] Table 1 Mechanical properties of die-cast aluminum alloys of Examples 1 to 3 and Comparative Examples 1 to 4

Claims

1. A heat-treatment-free low-pressure casting aluminum alloy, characterized in that: The heat treatment-free low-pressure casting aluminum alloy components include, by weight percentage: Si: 4.0-10.5%, Fe: 0-1.0%, Mn: 0.1-0.8%, Mg: 0-0.6%, La: 0.022-0.22%, V: 0.033-0.33%, B: 0.033-0.33%, the balance is Al; Among them, the mass ratio of La, V and B is 2:3:

3.

2. The heat treatment-free low-pressure casting aluminum alloy according to claim 1, characterized in that: The La, V and B are added into the alloy in the form of Al-2La-3V-3B amorphous powder, and the Al-2La-3V-3B amorphous particle size is 20-30 μm.

3. The heat treatment-free low-pressure casting aluminum alloy according to claim 2, characterized in that: The preparation method of the Al-2La-3V-3B amorphous powder comprises: firstly preparing an Al-2La-3V-3B alloy foil strip by a belt spinning method, and then ball milling the alloy foil strip by a crusher to obtain the Al-2La-3V-3B amorphous powder.

4. The heat treatment-free low-pressure casting aluminum alloy according to claim 3, characterized in that: The rotating speed of the strip spinning machine is 2200-2800 r / min, and the thickness of the prepared alloy foil strip is 20-30 μm and the width is 1.8-2.2 mm.

5. The heat treatment-free low-pressure casting aluminum alloy according to claim 3, characterized in that: The crusher ball-mills the alloy foil strip under argon gas conditions, and the crusher speed is 2500-3500r / min.

6. A method for preparing a heat-treatment-free low-pressure casting aluminum alloy as claimed in any one of claims 1 to 5, characterized in that: The preparation method comprises: S1 alloy smelting: the ingredients are prepared according to the weight percentage of the components. First, the pure aluminum ingot is melted, the aluminum liquid is heated to 750-760℃, and pure silicon and aluminum-manganese alloy are added in sequence, and kept for 25 minutes; the aluminum liquid temperature is further adjusted to 720-730℃, and pure magnesium ingot is added to melt aluminum liquid I; S2 refining: using the graphite rotary injection method, adding refining agent and high-purity argon into the aluminum liquid I at 720-730°C to obtain aluminum liquid II; S3 modification treatment: adjust the temperature of aluminum liquid II to 710-720°C, add Al-2La-3V-3B amorphous substance into aluminum liquid II by graphite rotary blowing method, continue to pass argon gas and rotate and stir for 5-8 minutes after adding, and obtain aluminum liquid III; S4 low pressure casting: The pressure is 500-1000mbar to obtain aluminum alloy castings.

7. The method for preparing a heat-treatment-free low-pressure casting aluminum alloy according to claim 6, characterized in that: The amount of the refining agent used is 2% of the total weight of the aluminum liquid II, the blowing time is 6 minutes, and after the refining is completed, it is left to stand for 2 to 3 minutes, and the refining process is repeated twice.

8. The method for preparing a heat treatment-free low-pressure casting aluminum alloy according to claim 6, characterized in that: The refining agent includes one or more of Rand high aluminum alloy refining agent-AJ2A, Yili aluminum alloy powder spray refining and slag cleaning agent DLJ-5 or Promag refining agent.

9. The method for preparing a heat-treatment-free low-pressure casting aluminum alloy according to claim 6, characterized in that: During the low-pressure casting process, when the aluminum liquid III enters the mold, the aluminum liquid temperature is 700-710°C, the mold cavity temperature is 300-350°C, and the temperature at the gate and the diverter cone is 450-500°C.

10. Use of the heat-treatment-free low-pressure cast aluminum alloy as claimed in any one of claims 1 to 5 in a battery tray for new energy vehicles.

Citation Information

Patent Citations

  • Heat-treatment-free high-toughness die-casting aluminum alloy as well as preparation method and product thereof

    CN115961183A

  • Non-heat-treated high-toughness die-casting aluminum alloy for new energy automobile and preparation method thereof

    CN116065061A

  • Heat-treatment-free die-casting aluminum alloy for electric bicycle and preparation method thereof

    CN116121605A

  • Brazable heat-treatment-free die-casting aluminum alloy material and preparation method and application thereof

    CN116334454A

  • Die-casting aluminum alloy without heat-treatment and preparation method and application thereof

    US20240139803A1

Cited By

  • Heat-treatment-free aluminum alloy material for low-pressure casting and preparation method thereof

    CN120290946A