Method for brazed connection of Y2O3-MgO nano-composite ceramic and titanium alloy

Through the connection of AgCuTi or AgCu solder in Y2O3-MgO nanocomposite ceramics and titanium alloy, metallurgical connections and intermetallic compounds are formed by the reaction of Ti and Cu elements, which solves the metallurgical bonding and residual stress problems when the ceramics and alloys are connected. Improves the mechanical and high temperature resistance of the joints.

CN118893264APending Publication Date: 2024-11-05HARBIN INST OF TECH

Patent Information

Application Number
CN202411099838.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-06-11
Filing Date
2024-08-12
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

It is difficult to form a metallurgical bond between Y2O3-MgO nano-composite ceramics and titanium alloys when brazed, and the brazed joints are prone to generate residual stress, reducing the mechanical properties of the joints.

Method used

AgCuTi or AgCu brazing material is used for brazing connection, TiO2 is generated by reacting Ti element with Y2O3 in ceramics, and CuO is formed by reacting Cu element with TiO2, diffusing to the surface of the ceramic to form Cu2Y2O5 reaction layer, forming metallurgical connection, and AgCu The Cu element in the solder reacts with the titanium alloy to form Cu-Ti intermetallic compounds, which are distributed in the brazing joints to improve high temperature resistance, and use Ag as a matrix to relieve residual stress of the joint.

Benefits of technology

Reliable brazing connection between Y2O3-MgO nano-complex ceramics and titanium alloys is achieved, which improves the mechanical properties and high temperature resistance of the joints and reduces the residual stress of the joints.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118893264A_ABST
    Figure CN118893264A_ABST
Patent Text Reader

Abstract

The invention discloses a method for brazed connection of Y2O3-MgO nano-composite ceramic and titanium alloy, and relates to a method for brazed connection of Y2O3-MgO ceramic and titanium alloy. In order to solve the problems that metallurgical bonding is difficult to form and the residual stress of a brazed joint is large during welding of the Y2O3-MgO nano-composite ceramic, reliable brazed connection of the Y2O3-MgO nano-composite ceramic and the titanium alloy is realized, and the joint with relatively high mechanical properties is obtained. When the Y2O3-MgO nano-composite ceramic and the titanium alloy are connected through brazing, a Cu2Y2O5 reaction layer is generated on the surface of the ceramic, metallurgical connection is formed, a Cu-Ti-O compound is further generated in the reaction layer, the Cu-Ti intermetallic compound in a brazing seam has excellent high-temperature resistance, Ag serves as a matrix of the whole brazing seam, joint residual stress can be relieved, and the mechanical property of the brazing seam is improved. And reliable brazing connection of the Y2O3-MgO nano-composite ceramic and the metal is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for brazing Y2O3-MgO ceramics and titanium alloy. Background Art

[0002] In order to enable the aviation platform to navigate accurately in a more severe environment, its navigation system needs to have a strong infrared detection capability. Since the infrared sensor is exposed to the outside of the aviation platform, it will face harsh aerodynamic heat, aerodynamic force, thermal shock, and wind and sand impact, which will damage the infrared sensor. Therefore, it is necessary to equip an infrared window to isolate the infrared sensor from the external environment and transmit the infrared signal while protecting the internal infrared sensor. This inevitably requires the infrared window to have good mechanical properties and wave transmission performance. However, during the flight, high temperature conditions will reduce the transmittance of traditional infrared window materials such as sapphire and enhance self-radiation, resulting in a sharp drop in detection sensitivity. In contrast, Y2O3-MgO nanocomposite ceramics is a new type of infrared window material with high high-temperature transmittance, low self-radiation coefficient, strong thermal shock resistance, and good mechanical properties. It can maintain relatively stable performance at high temperatures, so it has become a key application material for high-precision and high-stability infrared windows. Titanium alloys generally have the characteristics of low density and high specific strength, and are widely used in aerospace, national defense science and technology and other fields with excellent fatigue resistance and corrosion resistance. Therefore, achieving reliable connection between Y2O3-MgO nanocomposite ceramics and titanium alloy is of great significance for the production of lightweight, good mechanical properties, excellent high-temperature performance, and precise and stable infrared window modules.

[0003] Up to now, there are many methods that can be used to connect metals and ceramics, including mechanical, diffusion, self-propagating high-temperature synthesis, and brazing. These connection methods have their own advantages and disadvantages. For example, the advantages of self-propagating high-temperature synthesis connection are low energy consumption, high production efficiency, and small thermal impact on the parent material. However, due to the fast self-propagating reaction rate, it is difficult to control the welding time, and thus the interface reaction is difficult to control. In brazing, it is divided into direct brazing and indirect brazing. It uses the melting of the brazing material to achieve wetting and interface reaction with the parent material, thereby achieving reliable connection of complex components. The advantages are low cost, simple process, small restrictions on joint size and shape, and strong adaptability. Compared with other connection methods, brazing can be used in more metal and ceramic connection scenarios.

[0004] Y2O3-MgO nanocomposite ceramics are made by mixing chemically stable Y2O3 and MgO nanopowders in a 50:50 ratio and then sintering at high temperature. Therefore, Y2O3-MgO nanocomposite ceramics are chemically stable ceramics and are difficult to react chemically with general alloy brazing materials to form a metallurgical bond. In addition, for the brazing connection between Y2O3-MgO nanocomposite ceramics and metals, due to the large difference in thermal expansion coefficients between the two, it is easy to generate large residual stress in the brazed joint, which reduces the mechanical properties of the joint. Summary of the invention

[0005] In order to solve the problem that it is difficult to form metallurgical bonding and the residual stress of the brazed joint is large when Y2O3-MgO nanocomposite ceramics are welded, the present invention provides a method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloys to achieve reliable brazing connection between Y2O3-MgO nanocomposite ceramics and titanium alloys and obtain a joint with higher mechanical properties.

[0006] The method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy of the present invention is carried out according to the following steps:

[0007] 1. Cut, grind and clean the Y2O3-MgO nanocomposite ceramics and titanium alloy before welding:

[0008] 2. Pre-welding treatment of AgCuTi solder:

[0009] Taking powdered AgCuTi active solder or foil-shaped AgCuTi active solder, cutting, double-sided grinding and cleaning the foil-shaped AgCuTi active solder;

[0010] The content of Ti in the powdered AgCuTi active solder or the foil-shaped AgCuTi active solder is 0.5-5%, and the rest is Ag-Cu eutectic component;

[0011] 3. Assembly of the test piece to be welded: Place the titanium alloy with the surface to be welded facing upward, place powdered AgCuTi active brazing filler metal or foil-shaped AgCuTi active brazing filler metal at the center of the surface to be welded of the titanium alloy, and finally place the Y2O3-MgO nanocomposite ceramic with the surface to be welded facing downward in contact with the powdered AgCuTi active brazing filler metal or foil-shaped AgCuTi active brazing filler metal to obtain an assembly;

[0012] 4. Vacuum brazing connection: Place the assembly on a flat graphite table and place a round graphite block on the assembly to ensure that the Y2O3-MgO nanocomposite ceramic, AgCuTi active brazing filler metal and titanium alloy are in close contact, and then put them into the furnace together for brazing;

[0013] The brazing process is as follows: vacuumizing the furnace until the vacuum degree reaches 5×10-3 Pa, and heat to 800℃~1000℃ at a heating rate of 5~15℃ / min. After keeping warm for 10min, cool to below 150℃ at a cooling rate of ≤5℃ / min. Finally, take out the specimen and it is done.

[0014] The principles and beneficial effects of the present invention are:

[0015] The present invention adopts AgCuTi active solder for brazing connection. Ti element is an active element and reacts with Y2O3 in the ceramic to generate TiO2 in the initial stage of reaction. Then, Cu element in the solder reacts with TiO2 to be oxidized to CuO. CuO diffuses into the ceramic to react with Y2O3 to generate Cu2Y2O5 reaction layer on the surface of the ceramic to form metallurgical connection. Cu-Ti-O compound is also generated in the reaction layer. Meanwhile, Y2O3 in the ceramic close to the reaction layer also reacts with CuO to generate Cu2Y2O5. The remaining Cu element in the AgCuTi active solder reacts with Ti element diffused into the brazing seam by the titanium alloy to generate Cu-Ti intermetallic compound distributed in the brazing seam. The Cu-Ti intermetallic compound in the brazing seam has excellent high temperature resistance. Ag, as the matrix of the entire brazing seam, helps to relieve the residual stress of the joint. Therefore, the present invention realizes the reliable brazing connection between Y2O3-MgO nanocomposite ceramic and metal.

[0016] Another method of brazing Y2O3-MgO nanocomposite ceramics and titanium alloy using AgCu solder is carried out in the following steps:

[0017] 1. Cut, grind and clean the Y2O3-MgO nanocomposite ceramics and titanium alloy before welding:

[0018] During the cutting process, the area of ​​the Y2O3-MgO nanocomposite ceramic to be welded is smaller than the area of ​​the titanium alloy to be welded.

[0019] The cleaning process comprises: placing the polished Y2O3-MgO nanocomposite ceramic and titanium alloy into a cleaning agent respectively, performing ultrasonic cleaning in a 100kHz ultrasonic cleaning machine for 5 minutes, replacing a new cleaning agent, repeating the cleaning 2-3 times, placing the cleaned titanium alloy into acetone for liquid sealing for standby use; placing the cleaned Y2O3-MgO nanocomposite ceramic into an evaporation device for Ti evaporation, the evaporation time being 60 seconds, and forming a Ti coating on the surface of the Y2O3-MgO nanocomposite ceramic;

[0020] In the grinding process, 400-3000 mesh sandpaper is used to grind the Y2O3-MgO nanocomposite ceramic surface to be welded and the titanium alloy surface to be welded step by step; sandpaper grinding can remove surface impurities and ensure that the surface to be welded is smooth and flat;

[0021] The cleaning agent is anhydrous ethanol or acetone;

[0022] 2. Pre-welding treatment of AgCu solder:

[0023] Taking powdered AgCu solder or foil-shaped AgCu solder, cutting, double-sided grinding and cleaning the foil-shaped AgCu solder;

[0024] The foil-shaped AgCu solder is cut to a size larger than the surface of the Y2O3-MgO nanocomposite ceramic to be welded but smaller than the surface of the titanium alloy to be welded; before brazing, two clamps with flat surfaces are used to clamp the foil-shaped AgCu solder, and a pressure of 5 to 10 MPa is applied to flatten the foil;

[0025] The foil-shaped AgCu solder is polished using 3000-5000 mesh sandpaper;

[0026] The cleaning process is as follows: putting the polished AgCu solder foil into a cleaning agent, ultrasonically cleaning it in a 100kHz ultrasonic cleaning machine for 5 minutes, replacing the cleaning agent with a new one, repeating the cleaning 2-3 times, and putting the cleaned AgCu solder foil into acetone for liquid sealing for standby use; the cleaning agent is anhydrous ethanol or acetone;

[0027] The powdered AgCu solder or foil-shaped AgCu solder is an Ag-Cu eutectic component;

[0028] 3. Assembly of the test piece to be welded: Place the titanium alloy with the surface to be welded facing upward, place powdered AgCu solder or foil-shaped AgCu solder in the center of the surface to be welded, and finally place the Y2O3-MgO nanocomposite ceramic with the surface to be welded facing downward in contact with the powdered AgCu solder or foil-shaped AgCu solder to obtain an assembly;

[0029] 4. Vacuum brazing connection: Place the assembly on a flat graphite table and place a round graphite block on the assembly to ensure that the Y2O3-MgO nanocomposite ceramic, AgCu brazing filler metal and titanium alloy are in close contact, and then put them into a furnace together for brazing;

[0030] The brazing process is as follows: vacuumizing the furnace until the vacuum degree reaches 5×10 -3 Pa, and heat to 800℃~1000℃ at a heating rate of 5~15℃ / min. After keeping warm for 10min, cool to below 150℃ at a cooling rate of ≤5℃ / min. Finally, take out the specimen and it is done.

[0031] The principles and beneficial effects of the present invention are:

[0032] The present invention adopts AgCu solder for brazing connection. When the brazing temperature rises to the liquidus temperature of the AgCu solder, the TC4 titanium alloy begins to dissolve into the liquid solder, and then elements such as Ti and Al in the TC4 titanium alloy diffuse into the weld. The Ti element is an active element and diffuses to the ceramic side at the initial stage of the reaction to preferentially react with Y2O3 in the ceramic to generate TiO2. Subsequently, the Cu element in the solder reacts with TiO2 to be oxidized to CuO. The CuO diffuses into the ceramic and reacts with Y2O3 to generate a Cu2Y2O5 reaction layer on the ceramic surface to form a metallurgical connection. A Cu-Ti-O compound is also generated in the reaction layer, and Y2O3 in the ceramic close to the reaction layer also reacts with CuO to generate Cu2Y2O5. The remaining Cu element in the AgCu active brazing filler metal reacts with the Ti element diffused from the titanium alloy into the brazing seam to form a Cu-Ti intermetallic compound distributed in the brazing seam. The Cu-Ti intermetallic compound in the brazing seam has excellent high temperature resistance, and Ag, as the matrix of the entire brazing seam, helps to relieve the residual stress of the joint. Therefore, the present invention realizes a reliable brazing connection between Y2O3-MgO nanocomposite ceramics and metals. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a microstructure picture of the brazed joint of the Y2O3-MgO nanocomposite ceramic and TC4 titanium alloy in Example 1;

[0034] Figure 2 This is a microstructure picture of the brazed joint of the Y2O3-MgO nanocomposite ceramic and TC4 titanium alloy in Example 2;

[0035] Figure 3 This is a microstructure picture of the brazed joint of the Y2O3-MgO nanocomposite ceramic and TC4 titanium alloy in Example 3;

[0036] Figure 4 This is a microstructure picture of the brazed joint of the Y2O3-MgO nanocomposite ceramic and TC4 titanium alloy in Example 4;

[0037] Figure 5 This is a microstructure picture of the brazed joint of the Y2O3-MgO nanocomposite ceramic and TC4 titanium alloy in Example 5;

[0038] Figure 6 This is a microstructure picture of the brazed joint of the Y2O3-MgO nanocomposite ceramic and TC4 titanium alloy in Example 6;

[0039] Figure 7 The transmission observation image of the microstructure of the ceramic side of the brazed joint between Y2O3-MgO nanocomposite ceramic and TC4 titanium alloy in Example 3 and its element surface distribution image;

[0040] Figure 8 The relationship curve between the thickness of the ceramic side reaction layer and the connection temperature in the brazed connection joints of the Y2O3-MgO nanocomposite ceramic and TC4 titanium alloy obtained in Examples 1 to 4. DETAILED DESCRIPTION

[0041] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any reasonable combination of the specific implementation modes.

[0042] Specific implementation method 1: The method of brazing Y2O3-MgO nanocomposite ceramics and titanium alloy in this implementation method is carried out according to the following steps:

[0043] 1. Cut, grind and clean the Y2O3-MgO nanocomposite ceramics and titanium alloy before welding:

[0044] 2. Pre-welding treatment of AgCuTi solder:

[0045] Taking powdered AgCuTi active solder or foil-shaped AgCuTi active solder, cutting, double-sided grinding and cleaning the foil-shaped AgCuTi active solder;

[0046] The content of Ti in the powdered AgCuTi active solder or the foil-shaped AgCuTi active solder is 0.5-5%, and the rest is Ag-Cu eutectic component;

[0047] 3. Assembly of the test piece to be welded: Place the titanium alloy with the surface to be welded facing upward, place powdered AgCuTi active brazing filler metal or foil-shaped AgCuTi active brazing filler metal at the center of the surface to be welded of the titanium alloy, and finally place the Y2O3-MgO nanocomposite ceramic with the surface to be welded facing downward in contact with the powdered AgCuTi active brazing filler metal or foil-shaped AgCuTi active brazing filler metal to obtain an assembly;

[0048] 4. Vacuum brazing connection: Place the assembly on a flat graphite table and place a round graphite block on the assembly to ensure that the Y2O3-MgO nanocomposite ceramic, AgCuTi active brazing filler metal and titanium alloy are in close contact, and then put them into the furnace together for brazing;

[0049] The brazing process is as follows: vacuumizing the furnace until the vacuum degree reaches 5×10 -3 Pa, and heat to 800℃~1000℃ at a heating rate of 5~15℃ / min. After keeping warm for 10min, cool to below 150℃ at a cooling rate of ≤5℃ / min. Finally, take out the specimen and it is done.

[0050] This implementation has the following beneficial effects:

[0051] This embodiment adopts AgCuTi active solder for brazing connection. Ti element is an active element. In the initial stage of the reaction, it preferentially reacts with Y2O3 in the ceramic to generate TiO2. Then, Cu element in the solder reacts with TiO2 to be oxidized to CuO. CuO diffuses into the ceramic and reacts with Y2O3 to generate a Cu2Y2O5 reaction layer on the ceramic surface, forming a metallurgical connection. Cu-Ti-O compound is also generated in the reaction layer. At the same time, Y2O3 in the ceramic close to the reaction layer will also react with CuO to generate Cu2Y2O5. The remaining Cu element in the AgCuTi active solder reacts with the Ti element diffused into the brazing seam by the titanium alloy to generate Cu-Ti intermetallic compound distributed in the brazing seam. The Cu-Ti intermetallic compound in the brazing seam has excellent high temperature resistance. Ag, as the matrix of the entire brazing seam, helps to relieve the residual stress of the joint. Therefore, this embodiment realizes a reliable brazing connection between Y2O3-MgO nanocomposite ceramic and metal.

[0052] Specific implementation method 2: The difference between this implementation method and specific implementation method 1 is that during the cutting process in step 1, the area of ​​the Y2O3-MgO nanocomposite ceramic to be welded is smaller than the area of ​​the titanium alloy to be welded.

[0053] Specific implementation method three: This implementation method is different from specific implementation methods one or two in that: the cleaning process described in step one is: the polished Y2O3-MgO nanocomposite ceramics and titanium alloy are respectively placed in the cleaning agent, ultrasonically cleaned in a 100kHz ultrasonic cleaning machine for 5 minutes, replaced with a new cleaning agent, and repeated cleaning 2 to 3 times, and the cleaned Y2O3-MgO nanocomposite ceramics and titanium alloy are respectively placed in acetone for liquid sealing for standby use.

[0054] Specific implementation method four: The difference between this implementation method and any one of specific implementation methods one to three is that: during the polishing process described in step one, 400-3000 mesh sandpaper is used to polish the welding surface of the Y2O3-MgO nano-composite ceramic and the welding surface of the titanium alloy step by step; sandpaper polishing can remove surface impurities and ensure that the welding surface is smooth and flat.

[0055] Specific implementation method five: This implementation method is different from any one of specific implementation methods one to four in that: it is characterized in that: the cleaning agent in step one is anhydrous ethanol or acetone.

[0056] Specific embodiment six: This embodiment differs from any one of specific embodiments one to five in that: in step two, the foil-like AgCuTi active solder is cut to a foil size that is larger than the surface of the Y2O3-MgO nanocomposite ceramic to be welded and smaller than the surface of the titanium alloy to be welded; before brazing, two clamps with flat surfaces are used to clamp the foil-like AgCuTi active solder, and a pressure of 5 to 10 MPa is applied to flatten the foil.

[0057] Specific implementation method 7: This implementation method is different from any one of specific implementation methods 1 to 6 in that: in step 2, the foil-shaped AgCuTi active solder is polished using 3000-5000 mesh sandpaper.

[0058] Specific embodiment eight: This embodiment differs from any one of specific embodiments one to seven in that: the cleaning process described in step two is: placing the polished AgCuTi foil in a cleaning agent, ultrasonically cleaning it in a 100kHz ultrasonic cleaning machine for 5 minutes, replacing the new cleaning agent, repeating the cleaning 2 to 3 times, and placing the cleaned AgCuTi foil in acetone for liquid sealing for standby use.

[0059] Specific implementation method 9: This implementation method is different from any one of specific implementation methods 1 to 8 in that: the cleaning agent in step 2 is anhydrous ethanol or acetone.

[0060] Specific embodiment 10: This embodiment is different from the first to ninth embodiments in that the method of brazing Y2O3-MgO nanocomposite ceramics and titanium alloy using AgCu brazing filler metal is carried out according to the following steps:

[0061] 1. Cut, grind and clean the Y2O3-MgO nanocomposite ceramics and titanium alloy before welding:

[0062] During the cutting process, the area of ​​the Y2O3-MgO nanocomposite ceramic to be welded is smaller than the area of ​​the titanium alloy to be welded.

[0063] The cleaning process comprises: placing the polished Y2O3-MgO nanocomposite ceramic and titanium alloy into a cleaning agent respectively, performing ultrasonic cleaning in a 100kHz ultrasonic cleaning machine for 5 minutes, replacing a new cleaning agent, repeating the cleaning 2-3 times, placing the cleaned titanium alloy into acetone for liquid sealing for standby use; placing the cleaned Y2O3-MgO nanocomposite ceramic into an evaporation device for Ti evaporation, the evaporation time being 60 seconds, and forming a Ti coating on the surface of the Y2O3-MgO nanocomposite ceramic;

[0064] In the grinding process, 400-3000 mesh sandpaper is used to grind the Y2O3-MgO nanocomposite ceramic surface to be welded and the titanium alloy surface to be welded step by step; sandpaper grinding can remove surface impurities and ensure that the surface to be welded is smooth and flat;

[0065] The cleaning agent is anhydrous ethanol or acetone;

[0066] 2. Pre-welding treatment of AgCu solder:

[0067] Taking powdered AgCu solder or foil-shaped AgCu solder, cutting, double-sided grinding and cleaning the foil-shaped AgCu solder;

[0068] The foil-shaped AgCu solder is cut to a size larger than the surface of the Y2O3-MgO nanocomposite ceramic to be welded but smaller than the surface of the titanium alloy to be welded; before brazing, two clamps with flat surfaces are used to clamp the foil-shaped AgCu solder, and a pressure of 5 to 10 MPa is applied to flatten the foil;

[0069] The foil-shaped AgCu solder is polished using 3000-5000 mesh sandpaper;

[0070] The cleaning process is as follows: putting the polished AgCu solder foil into a cleaning agent, ultrasonically cleaning it in a 100kHz ultrasonic cleaning machine for 5 minutes, replacing the cleaning agent with a new one, repeating the cleaning 2-3 times, and putting the cleaned AgCu solder foil into acetone for liquid sealing for standby use; the cleaning agent is anhydrous ethanol or acetone;

[0071] The powdered AgCu solder or foil-shaped AgCu solder is an Ag-Cu eutectic component;

[0072] 3. Assembly of the test piece to be welded: Place the titanium alloy with the surface to be welded facing upward, place powdered AgCu solder or foil-shaped AgCu solder in the center of the surface to be welded, and finally place the Y2O3-MgO nanocomposite ceramic with the surface to be welded facing downward in contact with the powdered AgCu solder or foil-shaped AgCu solder to obtain an assembly;

[0073] 4. Vacuum brazing connection: Place the assembly on a flat graphite table and place a round graphite block on the assembly to ensure that the Y2O3-MgO nanocomposite ceramic, AgCu brazing filler metal and titanium alloy are in close contact, and then put them into a furnace together for brazing;

[0074] The brazing process is as follows: vacuumizing the furnace until the vacuum degree reaches 5×10 -3 Pa, and heat to 800℃~1000℃ at a heating rate of 5~15℃ / min. After keeping warm for 10min, cool to below 150℃ at a cooling rate of ≤5℃ / min. Finally, take out the specimen and it is done.

[0075] This embodiment uses AgCu solder for brazing connection. When the brazing temperature rises to the liquidus temperature of the AgCu solder, the TC4 titanium alloy begins to dissolve into the liquid solder, and then the Ti, Al and other elements in the TC4 titanium alloy diffuse into the weld. The Ti element is an active element and will diffuse to the ceramic side at the initial stage of the reaction to preferentially react with the Y2O3 in the ceramic to generate TiO2. Subsequently, the Cu element in the solder reacts with TiO2 to be oxidized to CuO. CuO diffuses into the ceramic and reacts with Y2O3 to generate a Cu2Y2O5 reaction layer on the ceramic surface, forming a metallurgical connection. Cu-Ti-O compounds are also generated in the reaction layer, and at the same time, the Y2O3 in the ceramic close to the reaction layer will also react with CuO to generate Cu2Y2O5. The remaining Cu element in the AgCu active brazing filler metal reacts with the Ti element diffused from the titanium alloy into the brazing seam to form a Cu-Ti intermetallic compound distributed in the brazing seam. The Cu-Ti intermetallic compound in the brazing seam has excellent high temperature resistance, and Ag, as the matrix of the entire brazing seam, helps to relieve the residual stress of the joint. Therefore, this embodiment realizes a reliable brazing connection between Y2O3-MgO nanocomposite ceramics and metal.

[0076] Example 1

[0077] The method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy in this embodiment is carried out according to the following steps:

[0078] 1. Cut, grind and clean the Y2O3-MgO nanocomposite ceramics and titanium alloy before welding:

[0079] During the cutting process, the Y2O3-MgO nanocomposite ceramic is cut to a welding surface area of ​​3mm×3mm, and the titanium alloy is cut to a welding surface area of ​​15mm×10mm;

[0080] The cleaning process comprises: placing the polished Y2O3-MgO nanocomposite ceramic and titanium alloy in a cleaning agent respectively, performing ultrasonic cleaning in a 100kHz ultrasonic cleaning machine for 5 minutes, replacing the cleaning agent with a new one, repeating the cleaning twice, and placing the cleaned Y2O3-MgO nanocomposite ceramic and titanium alloy in acetone for liquid sealing for standby use;

[0081] In the grinding process, 400 mesh, 600 mesh, 1200 mesh, and 3000 mesh sandpapers are used to grind the Y2O3-MgO nanocomposite ceramic surface to be welded and the titanium alloy surface to be welded step by step; sandpaper grinding can remove surface impurities and ensure that the surface to be welded is smooth and flat;

[0082] The cleaning agent is acetone;

[0083] 2. Pre-welding treatment of AgCuTi solder:

[0084] Taking the AgCuTi active solder in foil form, cutting, double-sided grinding and cleaning the AgCuTi active solder in foil form;

[0085] The AgCuTi active solder in foil form is cut to a foil size of 4 mm×4 mm; before brazing, two clamps with flat surfaces are used to clamp the AgCuTi active solder in foil form, and a pressure of 10 MPa is applied to flatten the foil;

[0086] The foil-shaped AgCuTi active solder is polished using 3000-mesh sandpaper;

[0087] The cleaning process is as follows: putting the polished AgCuTi foil into a cleaning agent, ultrasonically cleaning it in a 100kHz ultrasonic cleaning machine for 5 minutes, replacing the cleaning agent with a new one, repeating the cleaning twice, and putting the cleaned AgCuTi foil into acetone for liquid sealing for standby use; the cleaning agent is anhydrous ethanol;

[0088] The Ti content in the foil-shaped AgCuTi active solder is 3.5%, and the rest is Ag-Cu eutectic component (AgCuTi3.5);

[0089] 3. Assembly of the test piece to be welded: Place the titanium alloy with the surface to be welded facing upward, place the foil-shaped AgCuTi active solder in the center of the titanium alloy surface to be welded, and finally place the Y2O3-MgO nanocomposite ceramic with the surface to be welded facing downward in contact with the foil-shaped AgCuTi active solder to obtain an assembly;

[0090] 4. Vacuum brazing connection: Place the assembly on a flat graphite table and place a round graphite block on the assembly to ensure that the Y2O3-MgO nanocomposite ceramic, AgCuTi active brazing filler metal and titanium alloy are in close contact, and then put them into the furnace together for brazing;

[0091] The brazing process is as follows: vacuumizing the furnace until the vacuum degree reaches 5×10 -3 Heating was started at 0.05°C Pa, and the temperature was increased to 840°C at a heating rate of 10°C / min. After keeping the temperature for 10 min, the temperature was cooled to below 150°C at a cooling rate of ≤5°C / min. The specimen was taken out and the process was completed.

[0092] The shear test was carried out using an electronic universal testing machine with a loading speed of 0.5 mm / min. In this embodiment, AgCuTi foil was used as an intermediate layer to braze Y2O3-MgO nanocomposite ceramic and TC4 titanium alloy at 840°C, and the resulting connection joint had a room temperature shear strength of 22 MPa.

[0093] Example 2

[0094] The method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy in this embodiment is carried out according to the following steps:

[0095] 1. Cut, grind and clean the Y2O3-MgO nanocomposite ceramics and titanium alloy before welding:

[0096] During the cutting process, the Y2O3-MgO nanocomposite ceramic is cut to a welding surface area of ​​3mm×3mm, and the titanium alloy is cut to a welding surface area of ​​15mm×10mm;

[0097] The cleaning process comprises: placing the polished Y2O3-MgO nanocomposite ceramic and titanium alloy in a cleaning agent respectively, performing ultrasonic cleaning in a 100kHz ultrasonic cleaning machine for 5 minutes, replacing the cleaning agent with a new one, repeating the cleaning twice, and placing the cleaned Y2O3-MgO nanocomposite ceramic and titanium alloy in acetone for liquid sealing for standby use;

[0098] In the grinding process, 400 mesh, 600 mesh, 1200 mesh, and 3000 mesh sandpapers are used to grind the Y2O3-MgO nanocomposite ceramic surface to be welded and the titanium alloy surface to be welded step by step; sandpaper grinding can remove surface impurities and ensure that the surface to be welded is smooth and flat;

[0099] The cleaning agent is acetone;

[0100] 2. Pre-welding treatment of AgCuTi solder:

[0101] Taking the AgCuTi active solder in foil form, cutting, double-sided grinding and cleaning the AgCuTi active solder in foil form;

[0102] The AgCuTi active solder in foil form is cut to a foil size of 4 mm×4 mm; before brazing, two clamps with flat surfaces are used to clamp the AgCuTi active solder in foil form, and a pressure of 10 MPa is applied to flatten the foil;

[0103] The foil-shaped AgCuTi active solder is polished using 3000-mesh sandpaper;

[0104] The cleaning process is as follows: putting the polished AgCuTi foil into a cleaning agent, ultrasonically cleaning it in a 100kHz ultrasonic cleaning machine for 5 minutes, replacing the cleaning agent with a new one, repeating the cleaning twice, and putting the cleaned AgCuTi foil into acetone for liquid sealing for standby use; the cleaning agent is anhydrous ethanol;

[0105] The Ti content in the foil-shaped AgCuTi active solder is 3.5%, and the rest is Ag-Cu eutectic component (AgCuTi3.5);

[0106] 3. Assembly of the test piece to be welded: Place the titanium alloy with the surface to be welded facing upward, place the foil-shaped AgCuTi active solder in the center of the titanium alloy surface to be welded, and finally place the Y2O3-MgO nanocomposite ceramic with the surface to be welded facing downward in contact with the foil-shaped AgCuTi active solder to obtain an assembly;

[0107] 4. Vacuum brazing connection: Place the assembly on a flat graphite table and place a round graphite block on the assembly to ensure that the Y2O3-MgO nanocomposite ceramic, AgCuTi active brazing filler metal and titanium alloy are in close contact, and then put them into the furnace together for brazing;

[0108] The brazing process is as follows: vacuumizing the furnace until the vacuum degree reaches 5×10 -3 Heating was started at 0.05°C Pa, and the temperature was increased to 860°C at a heating rate of 10°C / min. After keeping the temperature for 10 min, the temperature was cooled to below 150°C at a cooling rate of ≤5°C / min. The specimen was taken out and the process was completed.

[0109] In this embodiment, AgCuTi foil is used as an intermediate layer to braze Y2O3-MgO nanocomposite ceramic and TC4 titanium alloy at 860°C, and the resulting connection joint has a room temperature shear strength of 41 MPa.

[0110] Example 3

[0111] The method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy in this embodiment is carried out according to the following steps:

[0112] 1. Cut, grind and clean the Y2O3-MgO nanocomposite ceramics and titanium alloy before welding:

[0113] During the cutting process, the Y2O3-MgO nanocomposite ceramic is cut to a welding surface area of ​​3mm×3mm, and the titanium alloy is cut to a welding surface area of ​​15mm×10mm;

[0114] The cleaning process comprises: placing the polished Y2O3-MgO nanocomposite ceramic and titanium alloy in a cleaning agent respectively, performing ultrasonic cleaning in a 100kHz ultrasonic cleaning machine for 5 minutes, replacing the cleaning agent with a new one, repeating the cleaning twice, and placing the cleaned Y2O3-MgO nanocomposite ceramic and titanium alloy in acetone for liquid sealing for standby use;

[0115] In the grinding process, 400 mesh, 600 mesh, 1200 mesh, and 3000 mesh sandpapers are used to grind the Y2O3-MgO nanocomposite ceramic surface to be welded and the titanium alloy surface to be welded step by step; sandpaper grinding can remove surface impurities and ensure that the surface to be welded is smooth and flat;

[0116] The cleaning agent is acetone;

[0117] 2. Pre-welding treatment of AgCuTi solder:

[0118] Taking the AgCuTi active solder in foil form, cutting, double-sided grinding and cleaning the AgCuTi active solder in foil form;

[0119] The AgCuTi active solder in foil form is cut to a foil size of 4 mm×4 mm; before brazing, two clamps with flat surfaces are used to clamp the AgCuTi active solder in foil form, and a pressure of 10 MPa is applied to flatten the foil;

[0120] The foil-shaped AgCuTi active solder is polished using 3000-mesh sandpaper;

[0121] The cleaning process is as follows: putting the polished AgCuTi foil into a cleaning agent, ultrasonically cleaning it in a 100kHz ultrasonic cleaning machine for 5 minutes, replacing the cleaning agent with a new one, repeating the cleaning twice, and putting the cleaned AgCuTi foil into acetone for liquid sealing for standby use; the cleaning agent is anhydrous ethanol;

[0122] The Ti content in the foil-shaped AgCuTi active solder is 3.5%, and the rest is Ag-Cu eutectic component (AgCuTi3.5);

[0123] 3. Assembly of the test piece to be welded: Place the titanium alloy with the surface to be welded facing upward, place the foil-shaped AgCuTi active solder in the center of the titanium alloy surface to be welded, and finally place the Y2O3-MgO nanocomposite ceramic with the surface to be welded facing downward in contact with the foil-shaped AgCuTi active solder to obtain an assembly;

[0124] 4. Vacuum brazing connection: Place the assembly on a flat graphite table and place a round graphite block on the assembly to ensure that the Y2O3-MgO nanocomposite ceramic, AgCuTi active brazing filler metal and titanium alloy are in close contact, and then put them into the furnace together for brazing;

[0125] The brazing process is as follows: vacuumizing the furnace until the vacuum degree reaches 5×10 -3 Pa, heating was started at a heating rate of 10°C / min to 880°C, and after keeping warm for 10 min, cooling was performed to below 150°C at a cooling rate of ≤5°C / min, and the specimen was taken out.

[0126] The shear test was carried out using an electronic universal testing machine with a loading speed of 0.5 mm / min. In this embodiment, AgCuTi foil was used as an intermediate layer to braze the Y2O3-MgO nanocomposite ceramic and TC4 titanium alloy at 880°C, and the resulting connection joint had a room temperature shear strength of 46 MPa. Figure 7The transmission observation image of the microstructure on the ceramic side of the Y2O3-MgO nanocomposite ceramic and TC4 titanium alloy brazing joint in Example 3 and its element surface distribution image; it can be seen from the figure that the reaction layer on the ceramic side is mainly composed of Cu2Y2O5 and Cu-Ti-O compounds, and the Cu-Ti-O compounds are mainly distributed on the ceramic surface, and the Y2O3 in the ceramic area close to the reaction layer also generates Cu2Y2O5 compounds due to the diffusion of Cu element and its reaction with TiO2.

[0127] Example 4

[0128] The method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy in this embodiment is carried out according to the following steps:

[0129] 1. Cut, grind and clean the Y2O3-MgO nanocomposite ceramics and titanium alloy before welding:

[0130] During the cutting process, the Y2O3-MgO nanocomposite ceramic is cut to a welding surface area of ​​3mm×3mm, and the titanium alloy is cut to a welding surface area of ​​15mm×10mm;

[0131] The cleaning process comprises: placing the polished Y2O3-MgO nanocomposite ceramic and titanium alloy in a cleaning agent respectively, performing ultrasonic cleaning in a 100kHz ultrasonic cleaning machine for 5 minutes, replacing the cleaning agent with a new one, repeating the cleaning twice, and placing the cleaned Y2O3-MgO nanocomposite ceramic and titanium alloy in acetone for liquid sealing for standby use;

[0132] In the grinding process, 400 mesh, 600 mesh, 1200 mesh, and 3000 mesh sandpapers are used to grind the Y2O3-MgO nanocomposite ceramic surface to be welded and the titanium alloy surface to be welded step by step; sandpaper grinding can remove surface impurities and ensure that the surface to be welded is smooth and flat;

[0133] The cleaning agent is acetone;

[0134] 2. Pre-welding treatment of AgCuTi solder:

[0135] Taking the AgCuTi active solder in foil form, cutting, double-sided grinding and cleaning the AgCuTi active solder in foil form;

[0136] The AgCuTi active solder in foil form is cut to a foil size of 4 mm×4 mm; before brazing, two clamps with flat surfaces are used to clamp the AgCuTi active solder in foil form, and a pressure of 10 MPa is applied to flatten the foil;

[0137] The foil-shaped AgCuTi active solder is polished using 3000-mesh sandpaper;

[0138] The cleaning process is as follows: putting the polished AgCuTi foil into a cleaning agent, ultrasonically cleaning it in a 100kHz ultrasonic cleaning machine for 5 minutes, replacing the cleaning agent with a new one, repeating the cleaning twice, and putting the cleaned AgCuTi foil into acetone for liquid sealing for standby use; the cleaning agent is anhydrous ethanol;

[0139] The Ti content in the foil-shaped AgCuTi active solder is 3.5%, and the rest is Ag-Cu eutectic component (AgCuTi3.5);

[0140] 3. Assembly of the test piece to be welded: Place the titanium alloy with the surface to be welded facing upward, place the foil-shaped AgCuTi active solder in the center of the titanium alloy surface to be welded, and finally place the Y2O3-MgO nanocomposite ceramic with the surface to be welded facing downward in contact with the foil-shaped AgCuTi active solder to obtain an assembly;

[0141] 4. Vacuum brazing connection: Place the assembly on a flat graphite table and place a round graphite block on the assembly to ensure that the Y2O3-MgO nanocomposite ceramic, AgCuTi active brazing filler metal and titanium alloy are in close contact, and then put them into the furnace together for brazing;

[0142] The brazing process is as follows: vacuumizing the furnace until the vacuum degree reaches 5×10 -3 Heating was started at 0.05°C Pa, and the temperature was increased to 900°C at a heating rate of 10°C / min. After keeping the temperature for 10 min, the temperature was cooled to below 150°C at a cooling rate of ≤5°C / min. The specimen was taken out and the process was completed.

[0143] The shear test was carried out using an electronic universal testing machine with a loading speed of 0.5 mm / min. In this embodiment, AgCuTi foil was used as an intermediate layer to braze Y2O3-MgO nanocomposite ceramic and TC4 titanium alloy at 900°C, and the resulting connection joint had a room temperature shear strength of 32 MPa.

[0144] Figure 1 This is a microstructure picture of the brazed joint of the Y2O3-MgO nanocomposite ceramic and TC4 titanium alloy in Example 1; Figure 2 This is a microstructure picture of the brazed joint of the Y2O3-MgO nanocomposite ceramic and TC4 titanium alloy in Example 2; Figure 3 This is a microstructure picture of the brazed joint of the Y2O3-MgO nanocomposite ceramic and TC4 titanium alloy in Example 3; Figure 4 This is a microstructure picture of the brazed joint of the Y2O3-MgO nanocomposite ceramic and TC4 titanium alloy in Example 4; Figures 1 to 4It can be seen that within the brazing temperature range of 840-900℃, when the temperature is kept for 10min, AgCuTi foil can be used to achieve brazing connection between Y2O3-MgO nanocomposite ceramics and TC4 titanium alloy, and each connection interface can form a strong and defect-free metallurgical bond. During the brazing process, the reaction layer on the ceramic side is mainly composed of the reaction of CuO with Y2O3 in the base material, but there are also Cu-Ti-O compounds, and CuO also diffuses in the ceramic base material and participates in the reaction. Figure 8 The relationship curve between the ceramic side reaction layer thickness and the connection temperature in the brazed joints of Y2O3-MgO nanocomposite ceramic and TC4 titanium alloy obtained in Examples 1 to 4 is shown in the figure. It can be seen from the figure that as the temperature increases, the reaction degree between the Ti element and the ceramic becomes more intense, and the thickness of the ceramic side reaction layer generated becomes larger.

[0145] Example 5

[0146] The method for brazing Y2O3-MgO nanocomposite ceramic and titanium alloy using AgCu solder in this embodiment is carried out according to the following steps:

[0147] 1. Cut, grind and clean the Y2O3-MgO nanocomposite ceramics and titanium alloy before welding:

[0148] During the cutting process, the Y2O3-MgO nanocomposite ceramic to be welded is cut to an area of ​​3mm×3mm; the titanium alloy to be welded is cut to an area of ​​15mm×10mm;

[0149] The cleaning process comprises: placing the polished Y2O3-MgO nanocomposite ceramic and titanium alloy into a cleaning agent respectively, performing ultrasonic cleaning in a 100kHz ultrasonic cleaning machine for 5 minutes, replacing a new cleaning agent, repeating the cleaning twice, placing the cleaned titanium alloy into acetone for liquid sealing for standby use; placing the cleaned Y2O3-MgO nanocomposite ceramic into an evaporation device for Ti evaporation for 60 seconds, and forming a Ti coating on the surface of the Y2O3-MgO nanocomposite ceramic;

[0150] In the grinding process, 400, 600, 1200, and 3000 mesh sandpapers are used to grind the Y2O3-MgO nanocomposite ceramic surface to be welded and the titanium alloy surface to be welded step by step; sandpaper grinding can remove surface impurities and ensure that the surface to be welded is smooth and flat;

[0151] The cleaning agent is anhydrous ethanol;

[0152] 2. Pre-welding treatment of AgCu solder:

[0153] Taking the AgCu solder in foil form, cutting, double-sided grinding and cleaning the AgCu solder in foil form;

[0154] The foil-shaped AgCu solder is cut to a foil size of 4 mm×4 mm; before brazing, two clamps with flat surfaces are used to clamp the foil-shaped AgCu solder, and a pressure of 10 MPa is applied to flatten the foil;

[0155] The foil-shaped AgCu solder is polished using 3000-mesh sandpaper;

[0156] The cleaning process is as follows: putting the polished AgCu solder foil into a cleaning agent, ultrasonically cleaning it in a 100kHz ultrasonic cleaning machine for 5 minutes, replacing the cleaning agent with a new one, repeating the cleaning twice, and putting the cleaned AgCu solder foil into acetone for liquid sealing for standby use; the cleaning agent is anhydrous ethanol;

[0157] The foil-shaped AgCu solder is an Ag-Cu eutectic composition;

[0158] 3. Assembly of the test piece to be welded: Place the titanium alloy with the surface to be welded facing upward, place the foil-shaped AgCu solder in the center of the surface to be welded, and finally place the Y2O3-MgO nanocomposite ceramic with the surface to be welded facing downward in contact with the foil-shaped AgCu solder to obtain an assembly;

[0159] 4. Vacuum brazing connection: Place the assembly on a flat graphite table and place a round graphite block on the assembly to ensure that the Y2O3-MgO nanocomposite ceramic, AgCu brazing filler metal and titanium alloy are in close contact, and then put them into a furnace together for brazing;

[0160] The brazing process is as follows: vacuumizing the furnace until the vacuum degree reaches 5×10 -3 Pa, heating was started at a heating rate of 10°C / min to 880°C, and after keeping warm for 10 min, cooling was performed to below 150°C at a cooling rate of ≤5°C / min, and the specimen was taken out.

[0161] Figure 5 This is a microstructure picture of the brazed joint of the Y2O3-MgO nanocomposite ceramic and the TC4 titanium alloy in Example 5; it can be seen that each connection interface can form a strong, defect-free metallurgical bond. The room temperature shear strength of the resulting connection joint reaches 28MPa.

[0162] Example 6

[0163] The method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy in this embodiment is carried out according to the following steps:

[0164] 1. Cut, grind and clean the Y2O3-MgO nanocomposite ceramics and titanium alloy before welding:

[0165] During the cutting process, the Y2O3-MgO nanocomposite ceramic is cut to a welding surface area of ​​3mm×3mm, and the titanium alloy is cut to a welding surface area of ​​15mm×10mm;

[0166] The cleaning process comprises: placing the polished Y2O3-MgO nanocomposite ceramic and titanium alloy in a cleaning agent respectively, performing ultrasonic cleaning in a 100kHz ultrasonic cleaning machine for 5 minutes, replacing the cleaning agent with a new one, repeating the cleaning twice, and placing the cleaned Y2O3-MgO nanocomposite ceramic and titanium alloy in acetone for liquid sealing for standby use;

[0167] In the grinding process, 400 mesh, 600 mesh, 1200 mesh, and 3000 mesh sandpapers are used to grind the Y2O3-MgO nanocomposite ceramic surface to be welded and the titanium alloy surface to be welded step by step; sandpaper grinding can remove surface impurities and ensure that the surface to be welded is smooth and flat;

[0168] The cleaning agent is acetone;

[0169] 2. Pre-welding treatment of AgCuTi solder:

[0170] Taking the AgCuTi active solder in foil form, cutting, double-sided grinding and cleaning the AgCuTi active solder in foil form;

[0171] The AgCuTi active solder in foil form is cut to a foil size of 4 mm×4 mm; before brazing, two clamps with flat surfaces are used to clamp the AgCuTi active solder in foil form, and a pressure of 10 MPa is applied to flatten the foil;

[0172] The foil-shaped AgCuTi active solder is polished using 3000-mesh sandpaper;

[0173] The cleaning process is as follows: putting the polished AgCuTi foil into a cleaning agent, ultrasonically cleaning it in a 100kHz ultrasonic cleaning machine for 5 minutes, replacing the cleaning agent with a new one, repeating the cleaning twice, and putting the cleaned AgCuTi foil into acetone for liquid sealing for standby use; the cleaning agent is anhydrous ethanol;

[0174] The Ti content in the foil-shaped AgCuTi active solder is 4.5%, and the rest is Ag-Cu eutectic component (AgCuTi4.5);

[0175] 3. Assembly of the test piece to be welded: Place the titanium alloy with the surface to be welded facing upward, place the foil-shaped AgCuTi active solder in the center of the titanium alloy surface to be welded, and finally place the Y2O3-MgO nanocomposite ceramic with the surface to be welded facing downward in contact with the foil-shaped AgCuTi active solder to obtain an assembly;

[0176] 4. Vacuum brazing connection: Place the assembly on a flat graphite table and place a round graphite block on the assembly to ensure that the Y2O3-MgO nanocomposite ceramic, AgCuTi active brazing filler metal and titanium alloy are in close contact, and then put them into the furnace together for brazing;

[0177] The brazing process is as follows: vacuumizing the furnace until the vacuum degree reaches 5×10 -3 Pa, heating was started at a heating rate of 10°C / min to 880°C, and after keeping warm for 10 min, cooling was performed to below 150°C at a cooling rate of ≤5°C / min, and the specimen was taken out.

[0178] Figure 6 This is a microstructure picture of the brazed joint of the Y2O3-MgO nanocomposite ceramic and the TC4 titanium alloy in Example 6; it can be seen that each connection interface can form a strong, defect-free metallurgical bond. The room temperature shear strength of the obtained connection joint reaches 45MPa.

Claims

1. A method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy, characterized in that: The method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy is carried out according to the following steps:

1. Cut, grind and clean the Y2O3-MgO nanocomposite ceramics and titanium alloy before welding:

2. Pre-welding treatment of AgCuTi solder: Taking powdered AgCuTi active solder or foil-shaped AgCuTi active solder, cutting, double-sided grinding and cleaning the foil-shaped AgCuTi active solder; The content of Ti in the powdered AgCuTi active solder or the foil-shaped AgCuTi active solder is 0.5-5%, and the rest is Ag-Cu eutectic component; 3. Assembly of the test piece to be welded: Place the titanium alloy with the surface to be welded facing upward, place powdered AgCuTi active brazing filler metal or foil-shaped AgCuTi active brazing filler metal at the center of the surface to be welded of the titanium alloy, and finally place the Y2O3-MgO nanocomposite ceramic with the surface to be welded facing downward in contact with the powdered AgCuTi active brazing filler metal or foil-shaped AgCuTi active brazing filler metal to obtain an assembly; 4. Vacuum brazing connection: Place the assembly on a flat graphite table and place a round graphite block on the assembly to ensure that the Y2O3-MgO nanocomposite ceramic, AgCuTi active brazing filler metal and titanium alloy are in close contact, and then put them into the furnace together for brazing; The brazing process is as follows: vacuumizing the furnace until the vacuum degree reaches 5×10 -3 Pa, and heat to 800℃~1000℃ at a heating rate of 5~15℃ / min. After keeping warm for 10min, cool to below 150℃ at a cooling rate of ≤5℃ / min. Finally, take out the specimen and it is done.

2. The method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy according to claim 1, characterized in that: During the cutting process in step 1, the area of ​​the Y2O3-MgO nanocomposite ceramic to be welded is cut to be smaller than the area of ​​the titanium alloy to be welded.

3. The method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy according to claim 1, characterized in that: The cleaning process described in step 1 is: put the polished Y2O3-MgO nanocomposite ceramics and titanium alloy into the cleaning agent respectively, ultrasonically clean them in a 100kHz ultrasonic cleaning machine for 5 minutes, replace the new cleaning agent, repeat the cleaning 2 to 3 times, and put the cleaned Y2O3-MgO nanocomposite ceramics and titanium alloy into acetone for liquid sealing for standby use.

4. The method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy according to claim 1, characterized in that: In the grinding process described in step 1, the surfaces to be welded of the Y2O3-MgO nanocomposite ceramic and the surfaces to be welded of the titanium alloy are ground step by step using sandpaper with a mesh size of 400 to 3000.

5. The method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy according to claim 1, characterized in that: The cleaning agent in step 1 is anhydrous ethanol or acetone.

6. The method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy according to claim 1, characterized in that: Step 2: The foil-shaped AgCuTi active solder is cut to a size larger than the Y2O3-MgO nanocomposite ceramic surface to be welded and smaller than the titanium alloy surface to be welded; before brazing, two clamps with flat surfaces are used to clamp the foil-shaped AgCuTi active solder, and a pressure of 5 to 10 MPa is applied to flatten the foil.

7. The method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy according to claim 1, characterized in that: In step 2, the foil-shaped AgCuTi active solder is polished using 3000-5000 mesh sandpaper.

8. The method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy according to claim 1, characterized in that: The cleaning process in step 2 is as follows: placing the polished AgCuTi foil in a cleaning agent, ultrasonically cleaning it in a 100kHz ultrasonic cleaning machine for 5 minutes, replacing the cleaning agent with a new one, repeating the cleaning 2 to 3 times, and placing the cleaned AgCuTi foil in acetone for liquid sealing for standby use.

9. The method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy according to claim 1, characterized in that: The cleaning agent in step 2 is anhydrous ethanol or acetone.

10. A method for brazing Y2O3-MgO nanocomposite ceramics and titanium alloy using AgCu brazing filler metal, characterized in that: The method of brazing Y2O3-MgO nanocomposite ceramics and titanium alloy using AgCu brazing filler metal is carried out in the following steps:

1. Cut, grind and clean the Y2O3-MgO nanocomposite ceramics and titanium alloy before welding: During the cutting process, the area of ​​the Y2O3-MgO nanocomposite ceramic to be welded is smaller than the area of ​​the titanium alloy to be welded. The cleaning process comprises: placing the polished Y2O3-MgO nanocomposite ceramic and titanium alloy into a cleaning agent respectively, performing ultrasonic cleaning in a 100kHz ultrasonic cleaning machine for 5 minutes, replacing a new cleaning agent, repeating the cleaning 2-3 times, placing the cleaned titanium alloy into acetone for liquid sealing for standby use; placing the cleaned Y2O3-MgO nanocomposite ceramic into an evaporation device for Ti evaporation, the evaporation time being 60 seconds, and forming a Ti coating on the surface of the Y2O3-MgO nanocomposite ceramic; In the grinding process, 400-3000 mesh sandpaper is used to grind the Y2O3-MgO nanocomposite ceramic surface to be welded and the titanium alloy surface to be welded step by step; The cleaning agent is anhydrous ethanol or acetone; 2. Pre-welding treatment of AgCu solder: Taking powdered AgCu solder or foil-shaped AgCu solder, cutting, double-sided grinding and cleaning the foil-shaped AgCu solder; The foil-shaped AgCu solder is cut to a size larger than the surface of the Y2O3-MgO nanocomposite ceramic to be welded but smaller than the surface of the titanium alloy to be welded; before brazing, two clamps with flat surfaces are used to clamp the foil-shaped AgCu solder, and a pressure of 5 to 10 MPa is applied to flatten the foil; The foil-shaped AgCu solder is polished using 3000-5000 mesh sandpaper; The cleaning process is as follows: putting the polished AgCu solder foil into a cleaning agent, ultrasonically cleaning it in a 100kHz ultrasonic cleaning machine for 5 minutes, replacing the cleaning agent with a new one, repeating the cleaning 2-3 times, and putting the cleaned AgCu solder foil into acetone for liquid sealing for standby use; the cleaning agent is anhydrous ethanol or acetone; The powdered AgCu solder or foil-shaped AgCu solder is an Ag-Cu eutectic component; 3. Assembly of the test piece to be welded: Place the titanium alloy with the surface to be welded facing upward, place powdered AgCu solder or foil-shaped AgCu solder in the center of the surface to be welded, and finally place the Y2O3-MgO nanocomposite ceramic with the surface to be welded facing downward in contact with the powdered AgCu solder or foil-shaped AgCu solder to obtain an assembly; 4. Vacuum brazing connection: Place the assembly on a flat graphite table and place a round graphite block on the assembly to ensure that the Y2O3-MgO nanocomposite ceramic, AgCu brazing filler metal and titanium alloy are in close contact, and then put them into a furnace together for brazing; The brazing process is as follows: vacuumizing the furnace until the vacuum degree reaches 5×10 -3 Pa, and heat to 800℃~1000℃ at a heating rate of 5~15℃ / min. After keeping warm for 10min, cool to below 150℃ at a cooling rate of ≤5℃ / min. Finally, take out the specimen and it is done.

Citation Information

Patent Citations

  • Welding connection method of oxide ceramic and metal

    CN108546095A

  • Brazing method for ceramic and metal

    CN109734469A

  • AgCu composite brazing filler metal for brazing ceramics and high-temperature alloys

    CN110181196A

  • Composite middle layer and method for brazing boron carbide composite ceramic and titanium alloy through composite middle layer

    CN113600957A

  • Method for brazing Y2O3-MgO composite ceramic and metal by adopting TiZrNiCu active brazing filler metal

    CN117921118A

Cited By

  • Ceramic-metal material composite brazing method with in-situ synthesis reaction

    CN121491464A