Welding process for high-strength non-bearing type vehicle body frame

By optimizing the activator formulation and welding parameters, and using MIG welding technology, the problem of high-strength frame connection was solved, achieving reliable connection and safety of the high-strength body, and meeting the simulation test requirements under various working conditions.

CN118893361APending Publication Date: 2024-11-05CITIC DICASTAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411280971.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing high-strength automotive frames, which use integrated die casting, cannot meet connection requirements, leading to body cracking and high bolt connection costs, thus failing to meet the needs of lightweighting and safety.

Method used

The high-strength non-load-bearing body frame welding process is adopted, and the active agent MIG welding technology is used. By optimizing the active agent formula and welding parameters and designing the bevel angle, the connection between the 4.5mm thick casting and the aluminum alloy profile is achieved, ensuring the welding quality.

Benefits of technology

It achieves a reliable connection of high-strength frame, reduces bolt connection costs, improves the overall performance and safety of the vehicle body, and meets the simulation test requirements under various working conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118893361A_ABST
    Figure CN118893361A_ABST
Patent Text Reader

Abstract

The invention discloses a high-strength non-bearing type vehicle body frame welding process, and relates to the field of frame welding processes, and the welding process comprises design of a high-performance heat-treatment-free aluminum alloy frame, an active agent, MIG welding speed, MIG welding current, MIG welding voltage, argon flow, welding interface and welding layer number. According to the technical requirements of a frame, a welding test piece is welded under the condition of different process parameters, through test analysis, 30-degree Y-shaped grooves are formed in the two sides of the welding test piece, 5-degree reversible deformation is prefabricated, spot welding fixing is adopted, and the welding process is that the current is 125 A, the welding speed is 3 m / h, the voltage is 22 v, the argon flow of the upper layer of the test piece is 20 L / h, and the argon flow of the lower layer of the test piece is 15 L / h. According to the welding process, the 4.5 mm-thick integrally-cast heat-treatment-free alloy can be completely welded at a time, and simulation tests of working conditions such as vertical impact, limit turning, emergency braking, torsion working conditions, whole vehicle torsion durability and whole vehicle vertical durability are adopted for power assembly suspension points.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of vehicle frame welding technology, and particularly relates to a high-strength non-load-bearing vehicle body frame welding technology. Background Art

[0002] The existing high-strength automobile frames are made of integrated die-casting, which cannot solve the connection problem well. The lightweight requirements of automobiles urgently require a high-performance welding process that can ensure the safety of the frame. The purpose of the present invention is to provide a welding process that can penetrate 4.5mm thick integrated casting heat-treatment-free alloy at one time, and simulate the vertical impact, extreme turning, emergency braking, torsion conditions, vehicle torsion durability, vehicle vertical durability and other working conditions of the powertrain suspension point. Summary of the invention

[0003] The invention aims to overcome the existing connection problems of high-strength aluminum alloy frames for commercial vehicles, which lead to cracking of the vehicle body and high bolt connection costs.

[0004] In order to solve the above technical problems, the present invention provides a high-strength non-load-bearing body frame welding process, including a frame unit, an extruded aluminum profile connected to the frame, the frame powertrain device is connected by activator MIG welding, and the powertrain is welded to the aluminum frame crossbeam through the body suspension devices on both sides and a single end thereof; through welding process development, the relevant groove angle and anti-deformation angle are designed, and the activator is brushed on both sides of the groove, and the connection between the 4.5mm thick casting and the profile is realized by one welding, and the activator formula is: Table 1 Active agent ratio

[0005] The orthogonal design test method was used to optimize the composition of the activator, and the best activator ratio was obtained, which was 15% SiO2, 15% Cr2O3, 55% NiO, 10% potassium carbonate, 2.5% titanium aluminum alloy and 2.5% zirconium aluminum alloy. The activator was stirred into a paste with anhydrous ethanol, and the activator was applied on both sides of the groove, with a width of 40mm on each side to cover the color of the metal surface.

[0006] The design of the welding groove uses a 4.5mm heat-treatment-free high-strength aluminum alloy frame on one side and a 4.5mm6082-T6 (aluminum alloy grade) extruded profile on the other side. Butt welding is adopted, and a 30° Y-shaped groove is opened on both sides of the weld, and a 5° reverse deformation is prefabricated.

[0007] Welding process settings: including the welding current, welding voltage, welding speed, and argon flow rate using the orthogonal test method; using the Y-type butt joint method, a 4.5mm thick high-pressure casting specimen was welded through at one time, and the welding specimen was determined through mechanical property tests, metallographic specimens, scanning electron microscopes, and energy spectrum analysis of the fracture to determine the welding specimen with the best performance under the optimal welding process. The final welding process parameters are: current 125A, welding speed 3m / h, voltage 22v, argon flow rate 20L / h on the upper layer of the specimen, and argon flow rate 15L / h on the lower layer of the specimen.

[0008] Furthermore, the weld has the highest mechanical properties under the optimal welding process.

[0009] Furthermore, under the optimal welding process, the metallographic structure of the weld is denser.

[0010] Furthermore, the weld hardness is the highest under the optimal welding process.

[0011] Furthermore, under the optimal welding process, the tensile fracture surface shows a ductile fracture under a scanning electron microscope, and there are significantly fewer pores and shrinkage defects.

[0012] Furthermore, under the optimal welding process, the content of harmful elements in the energy spectrum is relatively low.

[0013] The beneficial effects of the present invention are as follows: the new welding process for high-strength non-load-bearing body frames for automobiles provided by the present invention can weld through a 4.5 mm thick integrated cast heat-treatment-free alloy at one time, and according to the performance requirements of the frame, the powertrain suspension points are subjected to vertical impact, extreme turning, emergency braking, torsional conditions, whole vehicle torsional durability, whole vehicle vertical durability, and upper limit downward 0.8g durability conditions. Through 7 simulation conditions, the body welding structure can well meet customer performance requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a low-magnification metallographic photograph of the weld after the welding process of the present invention is adopted.

[0015] Figure 2 This is a scanning electron microscope photograph of a tensile fracture without using the welding process of the present invention.

[0016] Figure 3 This is a scanning electron microscope photograph of the tensile fracture after the welding process of the present invention is adopted.

[0017] Figure 4 This is a low-magnification panoramic photograph of a tensile fracture without using the welding process of the present invention.

[0018] Figure 5 This is a low-magnification panoramic photograph of the tensile fracture after the welding process of the present invention is adopted.

[0019] Figure 6This is an electron microscope photograph of the tensile fracture of a frame welding specimen that does not adopt the welding process of the present invention.

[0020] Figure 7 for Figure 6 Energy spectrum analysis diagram of the first tensile fracture welding defect.

[0021] Figure 8 for Figure 6 Energy spectrum analysis diagram of welding defect at the second tensile fracture.

[0022] Fig. 9 This is an electron microscope photograph of the tensile fracture of a frame welding specimen after adopting the welding process of the present invention.

[0023] Fig.10 for Fig. 9 Energy spectrum analysis diagram of welding defect of tensile fracture at the middle mark. DETAILED DESCRIPTION

[0024] The preferred embodiments of the present invention will be described in detail below with reference to the accompanying drawings.

[0025] like Figure 1 As shown in the figure, a high-strength non-load-bearing body frame welding process is used. The selection of welding samples is 4.5mm thick 6082-T6 national standard extruded profile on one side and 4.5mm thick sample block taken from heat-treatment-free high-pressure casting frame on the other side. The design of the weld is to open a 30° Y-shaped groove on both sides of the weld and prefabricate a 5° reverse deformation. The activator unit is to apply an activator made of acetone into a paste on both sides of the weld to cover the color of the metal surface. MIG welding is used. The welding process is tested through orthogonal tests. The optimal process finally selected needs to gradually determine the welding current, welding voltage, welding speed, argon gas flow rate on the front of the weld, and argon gas flow rate on the back of the weld. Mechanical property test, tensile test is carried out on the welded specimen to determine the optimal mechanical properties. The metallographic structure of the welding sample is analyzed; the tensile fracture of the welding specimen is analyzed by scanning electron microscope to determine the defect type, size and distribution; the tensile fracture of the welding specimen is analyzed by energy spectrum to determine the influence of pores and slag inclusion defects on the composition; finally, the macroscopic metallographic structure is observed by ultra-deep metallographic microscope. The welding process of the present invention can improve the welding performance of the frame by 20% and reduce the pores of the organizational structure by 10% by adjusting the welding parameters.

[0026] Table 2 Tensile test results

[0027] High performance aluminum alloy frame base material mechanical properties: R p0.2 :180MPa,R m :300MPa,A 50 :8%.

[0028] By utilizing the automobile high-strength aluminum alloy non-load-bearing body frame welding process provided by the present invention, according to the structure of the frame, the design of the activator unit and the weld and the optimization of the welding process parameters are optimized, so that the frame welding connection position is in an optimal stress state to reach more than 65% of the parent material performance to ensure its rigidity and performance. Specifically, according to the actual structure of the frame, by loading loads under 7 working conditions of vertical impact, extreme turning, emergency braking, torsional working conditions, whole vehicle torsional durability, whole vehicle vertical durability, and upper limit downward 0.8g durability, the welding process is optimized to prevent the stress and deformation of the powertrain suspension position from exceeding the standard under the 7 working conditions.

[0029] By comparison Fig. 9 and Figure 6 From the energy spectrum diagram and the element statistics in Table 5, Table 3 and Table 4, it can be seen that the welding process of the present invention improves the quality of the frame welding products.

[0030] Table 3 Figure 7 Element percentage statistics table

[0031] Table 4 Figure 8 Element percentage statistics table

[0032] Table 5 Fig.10 Element percentage statistics table

Claims

1. A high-strength non-load-bearing body frame welding process, It is characterized in that It includes a frame unit, and an extruded aluminum profile connected to the frame forms a frame power assembly device, the frame power assembly device is connected by activator MIG welding, the frame power assembly device includes body suspension devices on both sides and an aluminum frame cross beam, and one end of a single body suspension device is welded to the aluminum frame cross beam; an activator is brushed on both sides of the frame groove, and a 4.5mm thick casting and the profile are connected by one welding.

2. A high-strength non-load-bearing body frame welding process as claimed in claim 1, It is characterized in that Brush activator on the weld surface, applying 40mm width on both sides of the weld to cover the metal surface color.

3. A high-strength non-load-bearing body frame welding process as claimed in claim 2, It is characterized in that The frame groove has a groove of 30° on both sides, and a 5° anti-deformation is reserved to control the welding deformation of the frame.