Low-melting-point SnBiIn-xAg brazing filler metal alloy as well as preparation method and application thereof
By adding 0.5 to 3 wt% silver micron particles to the SnBiIn solder alloy, the rigid Ag2In phase was generated and the InBi phase was refined, the problem of insufficient mechanical properties and wettability of the existing Sn-based solder alloy was solved, and the further improvement was achieved Low melting point and better mechanical properties, suitable for ultra-low temperature packaging and welding of micro electronic components in high-tech fields.
Patent Information
- Application Number
- CN202411200551.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-05
AI Technical Summary
The existing Sn-based solder alloys have insufficient performance problems in meeting low melting point and wettability, and it is difficult to meet the mechanical properties and miniaturization and portability requirements of high-tech products.
Using SnBiIn-xAg solder alloy, by adding 0.5 to 3 wt% silver microparticles to the ternary solder microparticles, the generation of hard Ag2In phase is promoted and the InBi phase is refined, so as to improve the mechanical properties of the solder and at low temperatures. Maintain good wettability at the melting point.
Improve the tensile strength and wetting performance of SnBiIn-xAg solder alloy, so that it can show better structural stability and spreading capabilities in ultra-low temperature packaging and micro electronic components welding, and overcome the relatively good performance of ordinary SnBiIn solder alloys. Poor defect.
Smart Images

Figure CN118893364A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of solder technology, and in particular relates to a low melting point SnBiIn-xAg solder alloy and a preparation method and application thereof. Background Art
[0002] The melting point of solder is lower than that of the welding material, which can realize the combination of two materials (or parts) and is used for the packaging of electronic components. With the improvement of environmental protection requirements, the requirements for lead-free and cadmium-free solders have been put forward. Sn-Cu, Sn-Ag and other Sn-based solders are important lead-free and cadmium-free solders that can meet environmental protection requirements.
[0003] At the same time, with the development of high-tech technologies such as 5G technology, new energy vehicles, aerospace and biochip technology in recent years, the electronic components used internally have also been required to be miniaturized, portable and multifunctional. The third-generation semiconductor materials such as gallium nitride (GaN) and silicon carbide (SiC) have a wider bandgap, higher breakdown electric field, higher thermal conductivity, higher electron saturation rate and higher radiation resistance, which can meet the requirements of high-tech technologies such as new energy vehicles. In addition to the requirements for third-generation semiconductor materials such as gallium nitride (GaN) and silicon carbide (SiC), high-tech also puts forward higher requirements for solder, such as The miniaturization of electronic components also leads to the smaller size of solder joints after soldering, which puts higher requirements on the mechanical properties of the solder after soldering to improve the structural stability of electronic components. Some heat-sensitive electronic components also put higher requirements on the melting point of the solder, and need to be brazed at a lower temperature to avoid damage to heat-sensitive electronic components and reduce energy consumption. In addition, electronic components made of inorganic non-metallic materials such as gallium nitride put higher requirements on the wettability of metal solders, and the solder needs to be spread as much as possible. However, it is difficult for conventional Sn-based solders to simultaneously meet good mechanical properties, low melting points and good wettability.
[0004] At present, some Sn-based solders, such as eutectic In-48Sn solder, eutectic Sn-58Bi solder and other special solders, have a melting point below 150°C. The eutectic In-48Sn solder with a melting point of about 118°C can be used in low-temperature welding scenarios such as step soldering, while the eutectic Sn-58Bi solder with a melting point of about 138°C can also reduce the generation of pores and meet the requirements of low-temperature airtightness. However, it is also found in the application process that eutectic In-48Sn solder, eutectic Sn-58Bi solder and other special solders have low melting points. The defects of the solder are that the In-48Sn alloy exhibits low tensile strength of about 11MPa and low creep resistance. At the same time, In (indium) is a rare metal with low reserves and high price. The brittleness of Bi (bismuth) in the Sn-Bi based alloy is large, and too much Bi (bismuth) will have an adverse effect on the tensile strength and ductility of the Sn-Bi based solder joints. Therefore, it is necessary to develop new types of solder alloys to meet the requirements of mechanical properties, low melting point and wettability of solder alloys with the development of high-tech. Summary of the invention
[0005] In view of this, the present application provides a low melting point SnBiIn-xAg solder alloy and a preparation method and application thereof, which are used to solve the technical problem of poor performance of solder alloys in the prior art.
[0006] In a first aspect, the present application provides a SnBiIn-xAg solder alloy, the raw material composition of which includes ternary solder micron particles and silver micron particles;
[0007] The ternary solder micron particles include tin micron particles, bismuth micron particles and indium micron particles;
[0008] In the SnBiIn-xAg solder alloy, the doping amount of the silver micron particles is 0.5-3wt%.
[0009] Preferably, in the SnBiIn-xAg solder alloy, the doping amount of the silver microparticles is 2 wt %.
[0010] Preferably, the ternary solder micron particles include 30-40 at % of tin micron particles, 30-40 at % of bismuth micron particles and 30-40 at % of indium micron particles.
[0011] Preferably, the particle size of the tin micron particles is 1 to 5 μm;
[0012] The particle size of the bismuth micron particles is 1 to 5 μm;
[0013] The particle size of the indium micron particles is 15 to 20 μm;
[0014] The particle size of the silver micron particles is 1 to 5 μm.
[0015] The second aspect of the present application provides a method for preparing a SnBiIn-xAg solder alloy, which utilizes the raw materials of the SnBiIn-xAg solder alloy described in the first aspect to prepare the SnBiIn-xAg solder alloy, and the preparation method comprises the following steps:
[0016] Step S1, weighing tin micron particles, bismuth micron particles and indium micron particles according to the ratio of 30-40 at. %: 30-40 at. %: 30-40 at. % to obtain ternary solder micron particles;
[0017] Step S2, weighing silver micron particles according to a doping amount of 0.5 to 3 wt%, and mixing with ternary solder micron particles to obtain a raw material of SnBiIn-xAg solder alloy;
[0018] Step S3, melting the raw materials of SnBiIn-xAg solder alloy to obtain SnBiIn-xAg solder alloy.
[0019] Preferably, in step S2, the mixing process is mechanical mixing for 30 to 90 minutes.
[0020] Preferably, in step S3, the smelting process is: smelting at 300-400°C for 10-30 min, smelting at 720°C for 40-80 min, and cooling in the furnace to obtain the SnBiIn-xAg solder alloy.
[0021] Preferably, in step S3, the smelting is performed 1 to 3 times.
[0022] The fourth aspect of the present application provides the application of the SnBiIn-xAg solder alloy described in the first aspect in the field of electronic components.
[0023] Preferably, the electronic components include heat-sensitive electronic components, miniaturized electronic components and electronic components made of non-metallic materials.
[0024] Among them, in this patent application, heat-sensitive electronic components refer to electronic components whose parts are easily damaged under high temperature conditions; miniaturized electronic components refer to miniaturized electronic components with small sizes of parts, overall structures and solder joints between parts; electronic components including non-metallic materials refer to electronic components including non-metallic materials such as ceramics.
[0025] In summary, the present application provides a low melting point SnBiIn-xAg solder alloy and its preparation method and application. In the raw material composition of the SnBiIn-xAg solder alloy provided by the present application, 0.5-3wt% of silver microparticles are added to tin microparticles, bismuth microparticles and indium microparticles. The addition of silver microparticles promotes the hard Ag 2The generation of In phase and refinement of InBi phase can improve the mechanical properties of SnBiIn-xAg solder alloy. The SnBiIn-xAg solder alloy itself has a low melting point, which meets the requirements of ultra-low temperature packaging. At the same time, SnBiIn-xAg solder also has good wettability, thus solving the technical problem of poor performance of solder alloy in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0027] Figure 1 The DSC curve diagram of the SnBiIn solder alloy provided in Comparative Example 1 of the present application;
[0028] Figure 2 A DSC curve diagram of the SnBiIn-0.5wt%Ag solder alloy provided in Example 1 of the present application;
[0029] Figure 3 A DSC curve diagram of the SnBiIn-1wt%Ag solder alloy provided in Example 1 of the present application;
[0030] Figure 4 A DSC curve diagram of the SnBiIn-2wt%Ag solder alloy provided in Example 1 of the present application;
[0031] Figure 5 A DSC curve diagram of the SnBiIn-3wt%Ag solder alloy provided in Example 1 of the present application;
[0032] Figure 6 The wettability result diagram of the SnBiIn solder alloy and the SnBiIn-xAg solder alloy provided in Example 1 and Comparative Example 1 of the present application;
[0033] Figure 7 The SEM image of the SnBiIn solder alloy provided in Comparative Example 1 of the present application;
[0034] Figure 8 This is a SEM image of the SnBiIn-0.5wt%Ag solder alloy provided in Example 1 of the present application;
[0035] Fig. 9 This is a SEM image of the SnBiIn-1wt%Ag solder alloy provided in Example 1 of the present application;
[0036] Fig.10 This is a SEM image of the SnBiIn-2wt%Ag solder alloy provided in Example 1 of the present application;
[0037] Fig.11 This is a SEM image of the SnBiIn-3wt%Ag solder alloy provided in Example 1 of the present application;
[0038] Fig.12 a to d are EDS result diagrams corresponding to Spectrum 1 to 4 in the SEM diagrams of the SnBiIn solder alloy and the SnBiIn-xAg solder alloy provided in Example 1 and Comparative Example 1 of the present application, respectively;
[0039] Fig.13 This is a result diagram of the average width of the InBi phase in the SnBiIn solder alloy and the SnBiIn-xAg solder alloy provided in Example 1 and Comparative Example 1 of the present application;
[0040] Fig.14 A graph showing the tensile strength test results of the InBi phase in the SnBiIn solder alloy and the SnBiIn-xAg solder alloy provided in Example 1 and Comparative Example 1 of the present application;
[0041] Fig.15 The tensile fracture morphology of the SnBiIn solder alloy provided in Comparative Example 1 of the present application, Figure a is magnified 1.00kX times, and Figure b is magnified 4.00kX times;
[0042] Fig.16 The tensile fracture morphology of the SnBiIn-0.5wt%Ag solder alloy provided in Example 1 of the present application, Figure a is magnified 1.00kX times, and Figure b is magnified 4.00kX times;
[0043] Fig.17 This is a tensile fracture morphology of the SnBiIn-1wt%Ag solder alloy provided in Example 1 of the present application, Figure a is magnified 1.00kX times, and Figure b is magnified 4.00kX times;
[0044] Fig.18 The tensile fracture morphology of the SnBiIn-2wt%Ag solder alloy provided in Example 1 of the present application, Figure a is magnified 1.00kX times, and Figure b is magnified 4.00kX times;
[0045] Fig.19 The tensile fracture morphology of the SnBiIn-3wt%Ag solder alloy provided in Example 1 of the present application, Figure a is magnified 1.00kX times, and Figure b is magnified 4.00kX times;
[0046] Fig. 20This is the IMCs morphology of the interface between the SnBiIn solder alloy and the Cu substrate provided in Comparative Example 1 of the present application;
[0047] Fig.21 This is the IMCs morphology of the interface between the SnBiIn-0.5wt%Ag solder alloy and the Cu substrate provided in Example 1 of the present application;
[0048] Fig. 22 This is the IMCs morphology of the interface between the SnBiIn-1wt%Ag solder alloy and the Cu substrate provided in Example 1 of the present application;
[0049] Fig.23 This is the IMCs morphology of the interface between the SnBiIn-2wt%Ag solder alloy and the Cu substrate provided in Example 1 of the present application;
[0050] Fig.24 This is the IMCs morphology of the interface between the SnBiIn-3wt%Ag solder alloy and the Cu substrate provided in Example 1 of the present application;
[0051] Fig.25 This is a graph showing the thickness results of IMCs at the interface of SnBiIn solder alloy, SnBiIn-xAg solder alloy and Cu substrate provided in Example 1 and Comparative Example 1 of the present application. DETAILED DESCRIPTION
[0052] The present application provides a low melting point SnBiIn-xAg solder alloy and a preparation method and application thereof, which are used to solve the technical problem of poor performance of solder alloys in the prior art.
[0053] The technical solution of the present application will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0054] In view of the defect of poor performance of the current SnBiIn solder alloy, the present application provides a SnBiIn-xAg solder alloy. The raw material composition of the SnBiIn-xAg solder alloy includes ternary solder microparticles such as tin microparticles, bismuth microparticles and indium microparticles, and silver microparticles, and the doping amount of the silver microparticles is 0.5-3wt%, for example, 0.5, 1, 2, and 3g of silver microparticles are doped in every 100g of SnBiIn-xAg solder.
[0055] The solder alloy prepared by ordinary SnBiIn solder is prone to have too coarse InBi phase, resulting in poor performance. However, this patent application adds silver microparticles to the ternary solder microparticles. The addition of silver microparticles leads to hard Ag 2 The formation of In phase and the combination of Bi and In to form InBi phase are reduced, and the hard Ag 2 The formation of In phase can play a role of dispersion strengthening on the one hand, and on the other hand, it can refine InBi phase and promote uniform stress distribution, thereby improving the tensile strength and other mechanical properties of SnBiIn-xAg solder alloy; at the same time, SnBiIn-xAg solder alloy has a low melting point and can be combined with copper substrate and other welding materials at about 86℃. The wetting angle of SnBiIn-xAg solder alloy can be reduced to 35°, and the spreading area can reach 68.1mm 2 , which can easily spread to the surface of metal welding materials such as copper substrates and non-metal welding materials such as ceramics. This enables the SnBiIn-xAg solder alloy provided by this patent application to overcome the defect of poor performance of ordinary SnBiIn solder alloys.
[0056] Preferably, for the SnBiIn-xAg solder alloy provided in this patent application, the doping amount of silver microparticles in the SnBiIn-xAg solder alloy, the present application prefers that the doping amount of silver microparticles is 2wt%. Under this silver microparticle doping ratio, the SnBiIn-xAg solder alloy has better tensile strength, wettability and melting point.
[0057] At the same time, for the process of preparing SnBiIn-xAg solder alloy using SnBiIn-xAg solder, the present application uses a vacuum tube furnace, and the evenly mixed raw materials of the SnBiIn-xAg solder alloy are placed in a quartz boat, and then sent into the vacuum tube furnace for smelting. During the smelting, it is first melted at 300-400°C for 10-30 minutes, and then melted at 720°C for 40-80 minutes. After melting, it is cooled to obtain the SnBiIn-xAg solder alloy; and the shape of the SnBiIn-xAg solder alloy can be made into a 1mm×1mm×20mm long strip solder sheet sample through a mold.
[0058] As for the packaging process using SnBiIn-xAg solder alloy and Cu substrate, since the melting point of SnBiIn-xAg solder alloy is relatively low, the present application can achieve ultra-low temperature packaging of SnBiIn-xAg solder alloy and Cu substrate by soldering at a temperature of 86°C for 2 to 10 minutes; the flux used in the packaging process can be the rosin-type flux model Flux 55 produced by Shenzhen Yttrium Chengda Company.
[0059] The SnBiIn-xAg solder alloy provided in the present application will be specifically described below in combination with examples and experimental results.
[0060] Example 1
[0061] Embodiment 1 of the present application provides a method for preparing a SnBiIn-xAg solder alloy, the preparation method comprising: a step of preparing a raw material of the solder alloy, and a step of preparing the solder alloy by melting.
[0062] The steps to prepare the brazing alloy raw material include:
[0063] First, according to the ratio of equal molar mixing, 0.02 mol In particles 2.37g, 0.02 mol Sn particles 4.18g, 0.02 mol Bi particles 2.30g are weighed, and 8.85g of ternary solder micron particles are obtained after mixing. Four portions of the same ternary solder micron particles are weighed; wherein, the particle size of the In particles is 15-20μm, the particle size of the Sn particles is 1-5μm, and the particle size of the Bi particles is 1-5μm;
[0064] Then, according to the doping amount of Ag particles in SnBiIn-xAg solder alloy of 0.5wt%, 1wt%, 2wt%, and 3wt%, 0.045g, 0.09g, 0.18g, and 0.27g of Ag particles (1-5μm) were weighed respectively;
[0065] Then, the ternary solder micron particles and 0.045 g of Ag particles, the ternary solder micron particles and 0.09 g of Ag particles, the ternary solder micron particles and 0.18 g of Ag particles, and the ternary solder micron particles and 0.27 g of Ag particles were mechanically mixed for 60 minutes to obtain four portions of SnBiIn-xAg solder alloy raw materials.
[0066] The steps of melting and preparing the solder alloy include:
[0067] The raw materials of four parts of SnBiIn-xAg solder alloy were transferred to quartz boats respectively, and the quartz boats were sent to a vacuum tube furnace. The solder alloy was melted in an OTF-1200X vacuum tube furnace, and the melting temperature was first raised from room temperature to 350°C for 20 minutes, and then raised to 720°C for 60 minutes. The furnace was cooled to room temperature and remelted twice, and four parts of SnBiIn-xAg solder alloy were obtained by cooling; for the convenience of testing, the solder alloy in this embodiment was a 1mm×1mm×20mm long strip solder sheet sample prepared using a mold.
[0068] Comparative Example 1
[0069] Comparative Example 1 of the present application provides a method for preparing a SnBiIn solder alloy, which comprises: a step of preparing a raw material for the solder alloy, and a step of preparing the solder alloy by melting.
[0070] The steps to prepare the brazing alloy raw material include:
[0071] According to the mixing ratio of equal molar ratio, 2.37g of 0.02mol In particles, 4.18g of 0.02mol Sn particles, and 2.30g of 0.02mol Bi particles were weighed, and 8.85g of ternary solder micron particles were mechanically mixed for 60 minutes to obtain the raw material of SnBiIn solder alloy; wherein, the particle size of In particles is 15-20μm, the particle size of Sn particles is 1-5μm, and the particle size of Bi particles is 1-5μm.
[0072] The steps of melting and preparing the solder alloy include:
[0073] The raw materials of SnBiIn solder alloy are transferred into quartz boats respectively, and the quartz boats are sent into a vacuum tube furnace. The solder alloy is melted in an OTF-1200X vacuum tube furnace, and the melting temperature is first raised from room temperature to 350°C for 20 minutes, and then raised to 720°C for 60 minutes. The furnace is cooled to room temperature and remelted twice, and the SnBiIn solder alloy is cooled to obtain. For the convenience of testing, the solder alloy in this embodiment is a 1mm×1mm×20mm long strip solder sheet sample prepared using a mold.
[0074] Experimental Example 1
[0075] Experimental Example 1 of the present application conducts structural and performance tests on the SnBiIn-xAg solder alloys provided in Example 1 and Comparative Example 1.
[0076] The test process includes: first, evenly applying the flux on the polished and cleaned thin copper sheet, and then placing the four SnBiIn-xAg solder alloys provided in Example 1 and the SnBiIn solder alloy provided in Comparative Example 1 on the thin copper sheet (25mm×25mm×0.2mm), respectively, placing them on the D15 environmentally friendly constant temperature platform, heating them to 150°C and keeping them warm for 5 minutes, then taking them out and air cooling them to obtain five SnBiIn / Cu test samples, and then using instruments to perform structure and performance analysis on the SnBiIn / Cu test samples; the instruments used include: Discovery 250 differential scanning calorimeter, LeiCa optical microscope, Zeiss Supra 55 scanning electron microscope and energy dispersive X-ray spectrometer, STR-1102 strength bonding tester.
[0077] In the test results, the thermal performance results of the differential scanning calorimeter test are as follows Figure 1-5 As shown, from Figure 1-5It can be seen that the melting points of SnBiIn solder alloy and SnBiIn-xAg solder alloy are both around 85°C, and the melting point of SnBiIn-xAg solder alloy is lower. SnBiIn-xAg solder alloy is more suitable for ultra-low temperature packaging and can reduce the risk of damage to some heat-sensitive electronic components. It can also be seen that in the SnBiIn-xAg solder alloy, when the Ag doping amount is 2wt%, its melting point is even lower.
[0078] In the test results, the wettability results of the LeiCa optical microscope and Image J software test are shown in Figure 6. Figure 6 It can be seen that the wetting angle of SnBiIn solder alloy is 43.9° and the spreading area is 53.6mm 2 , while the wetting angle of SnBiIn-xAg solder alloy is smaller and the spreading area is larger, indicating that the wettability of SnBiIn-xAg solder alloy is better, which is conducive to the spreading of the solder alloy and is more suitable for the welding of some non-metallic electronic components; and in the SnBiIn-xAg solder alloy, when the Ag doping amount is 2wt%, its wetting angle is 35° and the spreading area is 68.1mm 2 , which is higher than the wetting angle and spreading area when the Ag doping amount is 3wt%.
[0079] In the test results, the microstructure and mechanical properties of the Zeiss Supra 55 scanning electron microscope, energy dispersive X-ray spectrometer, and STR-1102 strength tester were tested. Figure 7-19 shown; from Figure 7-12 It can be seen that the microstructures of SnBiIn-xAg solder alloy and SnBiIn solder alloy are different. SnBiIn solder alloy is mainly InBi phase and Sn-rich phase with a wider average width, while Ag appears in SnBiIn-xAg solder alloy. 2 In phase, and with the addition of silver microparticles Ag 2 The In phase becomes more and more. When 3wt% silver micron particles are added, a Bi-rich phase appears in the SnBiIn-xAg solder alloy. This is because the binding free energy of Ag and In is smaller than the binding free energy of Bi and In, and part of Bi fails to react with In to form InBi phase.
[0080] In SnBiIn-xAg solder alloy and SnBiIn solder alloy, the average width of InBi phase is as follows Fig.13 As shown, from Fig.13It can be seen that in the SnBiIn solder alloy, the average width of the InBi phase is 7.04μm. With the addition of Ag micronized particles, the microstructure of the solder alloy is also significantly refined. After adding 2wt% Ag micronized particles, the average width of the InBi phase in the solder alloy is refined to 4.19μm, which is 40% lower than that in the SnBiIn solder alloy. However, after adding 3wt% Ag micronized particles, the average width of the InBi phase increases. This may be due to the fact that Ag 2 The aggregation of In phase leads to the weakening of the effect of refining InBi phase.
[0081] from Fig.14 It can be seen that the addition of silver microparticles to the SnBiIn-xAg solder alloy affects the mechanical properties of the solder alloy; the tensile strength of the SnBiIn solder alloy without the addition of silver microparticles is 41.71MPa, and with the increase of the silver microparticle content, the tensile strength of the solder alloy shows a trend of first increasing and then decreasing, which is reflected in that when the addition amount of silver microparticles is 0.5wt%, 1wt% and 2wt%, the tensile strength of the solder alloy is enhanced, and at about 2wt%, a higher tensile strength of 58.90MPa can be achieved; at 3wt%, the tensile strength of the solder alloy decreases; combined with the spectrometer test results of the previous SnBiIn-xAg solder alloy and SnBiIn solder alloy, it can be analyzed that in the 0.5-2wt% stage, with the addition of silver microparticles, Ag 2 In phase is gradually generated, hard Ag 2 The In phase can play a role of dispersion strengthening and refine the InBi phase, promoting uniform stress distribution, thereby improving the tensile strength and other mechanical properties of the SnBiIn-xAg solder alloy. When the addition amount of silver microparticles is 3wt%, the Ag 2 The In phase aggregates, and the effects of dispersion strengthening and refinement of the InBi phase are weakened.
[0082] The tensile fracture morphology test results of SnBiIn-xAg solder alloy and SnBiIn solder alloy are shown in Figure 15-19 As shown, from Fig.15 As can be seen from the ab diagram in the figure, the fracture of the SnBiIn solder alloy is mainly InBi grains, and the fracture mode is intergranular brittle fracture. Figure 16-18 As can be seen from the ab graph in Figure 2, as the amount of silver microparticles added increases, the InBi grains begin to decrease and Ag 2 In phase and pit-shaped Sn-rich phase. When the addition amount of silver microparticles increases to 2wt%, Ag can be observed from the tensile fracture of the solder alloy. 2The In phase protrudes from the InBi phase without breaking, which means that when the dislocation moves to the vicinity of the InBi phase, it cannot cut through it but can only bypass it, thereby enhancing the tensile properties of the solder alloy. Fig.19 It can be seen from the ab diagram that when the addition amount of silver micron particles increases to 3wt%, more InBi phases appear at the fracture, which leads to a decrease in the tensile properties of the solder alloy. The tensile fracture morphology test, microstructure test and tensile strength test results of the SnBiIn-xAg solder alloy and the SnBiIn solder alloy tested by the STR-1102 strength combination tester correspond to each other, indicating that the addition of silver micron particles in the SnBiIn-xAg solder alloy will affect the mechanical properties of the SnBiIn-xAg solder alloy. When the SnBiIn-xAg solder alloy is actually applied, the addition amount of silver micron particles should be controlled to be about 2wt%.
[0083] The microstructure of the interface between SnBiIn-xAg solder alloy and SnBiIn solder alloy and Cu was characterized as follows Figure 20-24 shown; from Figure 20-24 It can be seen that the interface IMCs between SnBiIn-xAg solder alloy and SnBiIn solder alloy and Cu substrate are mainly Cu 3 (Sn,In) phase and Cu 6 (Sn,In) 5 phases, such as prismatic and scalloped Cu 6 Sn 5 Phase; Cu 3 Sn phase and Cu 6 Sn 5 The phase does not appear in the interface IMCs because the atomic radius of In atoms and Sn atoms is very close (the atomic radius of In atoms is 144 pm, and the atomic radius of Sn atoms is 140 pm). 3 Sn phase and Cu 6 Sn 5 Sn atoms in the phase. 6 Sn 5 The phase has the smallest Gibbs free energy in the Cu-Sn system. Sn atoms and Cu atoms first form Cu 6 Sn 5 phase, then Cu 6 Sn 5 The phase continues to react with Cu atoms to form Cu 3 Sn phase; from Fig.25 It can be further seen that the upper layer of the IMCs at the interface between the SnBiIn-xAg solder alloy and the SnBiIn solder alloy and the Cu substrate includes Ag 2In phase, the presence of these phases affects the interface IMCs, causing the thickness of the interface IMCs to decrease, such as Fig.25 As shown in the figure, with the increase of silver doping content in SnBiIn-xAg / Cu, the interface IMCs become thinner and thinner, and the thickness decreases from 3.03μm to 2.01μm. By regulating the interface IMCs, the bonding strength between the solder alloy and the Cu substrate can be further improved, and the structural stability of some microelectronic components that are connected using small-sized solder joints can be improved.
[0084] It can be seen from the test results of Experimental Example 1 that the SnBiIn-xAg solder alloy provided in the present application has a low melting point, can achieve ultra-low temperature packaging, and is not easy to affect the performance of heat-sensitive electronic components; at the same time, it has good wettability and is easy to spread to the surface of the material to be welded. It also has good mechanical properties and can maintain structural stability after welding.
[0085] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A SnBiIn-xAg solder alloy, characterized in that: The raw material composition includes ternary solder micron particles and silver micron particles; The ternary solder micron particles include tin micron particles, bismuth micron particles and indium micron particles; In the SnBiIn-xAg solder alloy, the doping amount of the silver micron particles is 0.5-3wt%.
2. The SnBiIn-xAg solder alloy according to claim 1, characterized in that: The doping amount of the silver microparticles is 2 wt %.
3. The SnBiIn-xAg solder alloy according to claim 1, characterized in that: The ternary solder micron particles include 30-40 at% of tin micron particles, 30-40 at% of bismuth micron particles and 30-40 at% of indium micron particles.
4. The SnBiIn-xAg solder alloy according to claim 1, characterized in that: The particle size of the tin micron particles is 1 to 5 μm; The particle size of the bismuth micron particles is 1 to 5 μm; The particle size of the indium micron particles is 15 to 20 μm; The particle size of the silver micron particles is 1 to 5 μm.
5. A method for preparing a SnBiIn-xAg solder alloy, characterized in that: Includes steps: Step S1, weighing tin micron particles, bismuth micron particles and indium micron particles according to the ratio of 30-40 at. %: 30-40 at. %: 30-40 at. % to obtain ternary solder micron particles; Step S2, weighing silver micron particles according to a doping amount of 0.5 to 3 wt%, and mixing with ternary solder micron particles to obtain a raw material of SnBiIn-xAg solder alloy; Step S3, melting the raw materials of SnBiIn-xAg solder alloy to obtain SnBiIn-xAg solder alloy.
6. The method for preparing a SnBiIn-xAg solder alloy according to claim 5, characterized in that: In step S2, the mixing process is mechanical mixing for 30 to 90 minutes.
7. The method for preparing a SnBiIn-xAg solder alloy according to claim 5, characterized in that: In step S3, the smelting process is: smelting at 300-400°C for 10-30 minutes, smelting at 720°C for 40-80 minutes, and cooling in the furnace to obtain SnBiIn-xAg solder alloy.
8. The method for preparing a SnBiIn-xAg solder alloy according to claim 5, characterized in that: In step S3, the smelting is performed 1 to 3 times.
9. Application of the SnBiIn-xAg solder alloy according to any one of claims 1 to 4 in the field of electronic components.
10. The use according to claim 9, characterized in that: The electronic components include heat-sensitive electronic components, miniaturized electronic components and electronic components made of ceramic materials.