Composite brazing filler metal suitable for low-corrosion brazing of titanium alloy thin-wall structural part and preparation method and application of composite brazing filler metal

By using a composite solder of TiZrHfCuNiCo amorphous high entropy foil and Ti foil, the dissolution defect problem of traditional solder when brazing TC4 titanium alloy thin-walled structural parts is solved, and high-strength brazing under low dissolution conditions is achieved The effect improves the performance and stability of the joint.

CN118893366AActive Publication Date: 2024-11-05HARBIN INST OF TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411071698.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-05
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

Traditional titanium-based brazing materials are prone to dissolution defects when brazing TC4 titanium alloy thin-walled structural parts, resulting in reduced joint strength and fatigue resistance, and it is difficult to achieve both low dissolution and high strength.

Method used

Using composite brazing material composited by two layers of TiZrHfCuNiCo amorphous high entropy foil and one layer of Ti foil, it is prepared by adhesive or resistive spot welding. The phase of Ti foil changes to β-Ti during brazing, thereby increasing Cu and Ni. The diffusion coefficient and solubility of elements such as Co can fully react with the solder, reduce residual solder and improve joint strength.

Benefits of technology

It effectively reduces the dissolution of the base material, improves the strength and performance of the brazed joint, and ensures that high-strength brazing effect is achieved under low dissolution conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118893366A_ABST
    Figure CN118893366A_ABST
Patent Text Reader

Abstract

The invention discloses composite brazing filler metal suitable for low-corrosion brazing of a titanium alloy thin-wall structural part and a preparation method and application of the composite brazing filler metal, and relates to amorphous high-entropy composite brazing filler metal and a preparation method and application of the amorphous high-entropy composite brazing filler metal. And the contradiction that low corrosion and high strength cannot be achieved at the same time is solved. The composite brazing filler metal suitable for low-corrosion brazing of the titanium alloy thin-wall structural part is formed by compounding two layers of TiZrHfCuNiCo amorphous high-entropy foil pieces and a layer of Ti foil, the layer of Ti foil is arranged between the two layers of TiZrHfCuNiCo amorphous high-entropy foil pieces, and the TiZrHfCuNiCo amorphous high-entropy foil pieces and the Ti foil are compounded together through a binding agent or a resistance spot welding method. The composite brazing filler metal can effectively reduce corrosion of base metal while improving the performance of a brazed joint, and the strength of the joint is improved. The main product form of the composite brazing filler metal is a foil, and the composite brazing filler metal is uniform in component, convenient to assemble, capable of well controlling the width of a brazing seam, ideal in brazing filler metal material, more suitable for being put into actual production and capable of greatly improving the joint strength under the condition that base metal is low in corrosion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an amorphous high-entropy composite solder and a preparation method and application thereof. Background Art

[0002] TC4 titanium alloy has been widely used as a structural material due to its excellent specific strength and corrosion resistance. With the continuous development of the manufacturing industry, higher requirements have been placed on the welding process of TC4 titanium alloy. However, traditional titanium-based brazing fillers are prone to corrosion defects when brazing thin-walled structural parts such as TC4 titanium alloy honeycomb panels and heat exchangers. When there is severe corrosion in the thin-walled TC4 brazed joint, the strength and fatigue resistance of the joint will be seriously deteriorated, and it is very easy to fail under high temperature, high pressure and corrosive conditions.

[0003] The main reason for the dissolution of traditional titanium-based brazing filler metals is that elements such as Ni and Cu are often added to the brazing filler metal to reduce its melting point. However, during the brazing process, the Cu and Ni elements will diffuse into the TC4 base material, alloying the base material surface and reducing the melting point, which will lead to dissolution defects. Although the use of low-dissolution amorphous high-entropy foil can inhibit the diffusion of elements of the TC4 base material into the brazing filler metal, thereby achieving the purpose of reducing the dissolution of the base material, at the same time, due to the low dissolution of the base material, the Ti element in the base material diffuses less into the brazing filler metal. At this time, the brazing filler metal does not fully react with the Ti element in the base material, resulting in a large amount of residual brazing filler metal in the joint, which seriously restricts the improvement of the joint strength. Summary of the invention

[0004] In order to solve the contradiction between low corrosion and high strength in TC4 titanium alloy brazing joints, the present invention provides a composite brazing material suitable for low corrosion brazing of titanium alloy thin-walled structural parts, and a preparation method and application thereof.

[0005] The composite brazing filler metal suitable for low-corrosion brazing of titanium alloy thin-walled structural parts is composited by two layers of TiZrHfCuNiCo amorphous high-entropy foils and a layer of Ti foil, wherein the layer of Ti foil is arranged between the two layers of TiZrHfCuNiCo amorphous high-entropy foils, and the TiZrHfCuNiCo amorphous high-entropy foils and the Ti foil are composited together by a binder or a resistance spot welding method.

[0006] Ti in the TiZrHfCuNiCo amorphous high entropy foil of the present invention is a main component element in the titanium alloy, which can make the high entropy solder have good wettability and fluidity on the surface of the base material. Zr and Hf are elements of the same main group as Ti, and can be infinitely soluble in each other, thereby improving the wettability of the solder and the base material, and can significantly reduce the melting point of the solder, and increase the chaos degree of the alloy, thereby increasing the entropy value of the alloy. The three elements of Cu, Ni and Co have similar effects and can be infinitely soluble in each other, thereby further reducing the melting point of the solder, and at the same time increasing the chaos degree of the alloy, thereby increasing the entropy value of the alloy. The reason why Ti foil is included in the composite solder is that when pure Ti is heated to 882°C, an allotropic transformation will occur, and the lattice structure of Ti will change from a close-packed hexagonal structure of α-Ti to a body-centered cubic structure of β-Ti. Since the base material TC4 contains a large amount of Al element, which is an α-Ti stabilizer, it can increase the phase change temperature of α-Ti to about 985-995°C. When the brazing temperature is between 882°C and 985°C, the base material has not yet undergone a phase change and still contains a large amount of α-Ti, while the pure Ti foil in the composite solder has been completely transformed into β-Ti. Since the diffusion coefficient and solubility of melting-reducing elements such as Cu, Ni, and Co in β-Ti are much higher than those of α-Ti, Cu, Ni, and Co will preferentially enter the pure Ti foil during the brazing process and cause the pure Ti foil to melt, so that the Ti element fully reacts with the solder, reducing the residual solder in the brazing seam and improving the joint strength.

[0007] The preparation method of the composite brazing material suitable for low-corrosion brazing of titanium alloy thin-walled structural parts of the present invention is carried out according to the following steps:

[0008] Step 1: weigh the raw materials of TiZrHfCuNiCo amorphous high entropy foil according to atomic percentage;

[0009] The TiZrHfCuNiCo amorphous high entropy foil is composed of 12-30% Ti, 12-30% Zr, 12-30% Hf, 12-30% Cu, 12-30% Ni and 12-30% Co in atomic percentage;

[0010] Step 2: Melting the raw materials weighed in step 1 to obtain a brazing ingot;

[0011] Step 3: preparing the solder ingot obtained in step 2 into a TiZrHfCuNiCo amorphous high entropy foil by a single-roll spinning method;

[0012] Step 4: placing the Ti foil between two layers of TiZrHfCuNiCo amorphous high entropy foils and compounding them together using an adhesive or resistance spot welding method to prepare a low-dissolution, high-strength amorphous high-entropy composite brazing material for TC4 titanium alloy brazing;

[0013] The thickness ratio of the TiZrHfCuNiCo amorphous high entropy foil to the Ti foil is 0.8-3:1.

[0014] The method for brazing TC4 titanium alloy using a composite brazing filler metal suitable for low-corrosion brazing of titanium alloy thin-walled structural parts is carried out in the following steps:

[0015] Step 1: Grind the surface of the TC4 alloy to be welded with fine sandpaper to remove surface oil and oxides, and then put the grinded TC4 alloy and the low-dissolution, high-strength amorphous, high-entropy composite brazing material for TC4 titanium alloy brazing into anhydrous ethanol for ultrasonic cleaning;

[0016] Step 2: Assemble from top to bottom the TC4 alloy, the low-dissolution, high-strength amorphous, high-entropy composite brazing material for TC4 titanium alloy brazing, and the TC4 alloy, and finally put them into a vacuum brazing furnace for brazing, and then complete;

[0017] The brazing process is as follows: heating to 940-960°C at a speed of 10°C / min and keeping the temperature for 10 minutes, then cooling to 150-200°C at a speed of 10-15°C / min, and then cooling to room temperature with the furnace to complete the brazing of the TC4 alloy.

[0018] The technical effects of the present invention are:

[0019] 1. The TiZrHfCuNiCo amorphous high entropy foil in the low-dissolution, high-strength amorphous high-entropy composite brazing material for TC4 titanium alloy brazing of the present invention has good wettability with the base material, and has many types of components, high content, and the content of each component is relatively close, and the atomic arrangement is relatively chaotic, so the mixing entropy of the atomic arrangement is very high, thereby inhibiting the formation of intermetallic compounds. At the same time, the atomic sizes of various elements in the high-entropy alloy differ greatly, especially when the mixing entropy of the alloy is high, the coordinated diffusion between the main elements of the alloy becomes difficult, and the differences in atomic size, bond type and lattice potential energy between the main elements cause the crystal structure of the high-entropy alloy to be distorted, which also hinders the movement of atoms and makes it difficult to diffuse in the high-entropy alloy, thereby inhibiting the diffusion rate of atoms, and being able to improve the performance of the brazed joint while effectively reducing the corrosion of the base material.

[0020] 3. The pure Ti foil in the composite solder of the present invention can be transformed into β-Ti during brazing, thereby increasing the diffusion coefficient and solubility of melting-reducing elements such as Cu, Ni, and Co in the pure Ti foil, causing the pure Ti foil to melt before the TC4 base material, allowing the Ti element to fully react with the solder, thereby increasing the joint strength.

[0021] 4. The main product form of the composite solder of the present invention is foil, which has uniform composition, is easy to assemble, and can better control the width of the soldering seam. It is an ideal solder material, more suitable for actual production, and can greatly improve the joint strength under the condition of low dissolution of the base material. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The interface microstructure diagram of the TC4 / TiZrHfCuNiCo / pure Ti / TiZrHfCuNiCo / TC4 brazed joint obtained under the brazing condition of 940°C / 10min in Example 1;

[0023] Figure 2 This is the interface structure diagram of the TC4 / TiZrHfCuNiCo / TC4 brazed joint obtained under the brazing conditions of 940℃ / 10min in the comparative example. DETAILED DESCRIPTION

[0024] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any reasonable combination of the specific implementation modes.

[0025] Specific implementation method 1: This implementation method is suitable for the composite brazing filler metal for low-corrosion brazing of titanium alloy thin-walled structural parts, which is composed of two layers of TiZrHfCuNiCo amorphous high-entropy foils and a layer of Ti foil. The layer of Ti foil is arranged between the two layers of TiZrHfCuNiCo amorphous high-entropy foils, and the TiZrHfCuNiCo amorphous high-entropy foil and the Ti foil are composited together by an adhesive or resistance spot welding.

[0026] This embodiment has the following beneficial effects:

[0027] 1. The TiZrHfCuNiCo amorphous high entropy foil in the low-dissolution, high-strength amorphous high-entropy composite brazing material for TC4 titanium alloy brazing in this embodiment has good wettability with the base material, and has many types of components, high content, and relatively close content of each component. The atomic arrangement is relatively chaotic, so the mixing entropy of the atomic arrangement is very high, thereby inhibiting the formation of intermetallic compounds. At the same time, the atomic sizes of various elements in the high-entropy alloy vary greatly, especially when the mixing entropy of the alloy is high, the coordinated diffusion between the main elements of the alloy becomes difficult, and the differences in atomic size, bond type and lattice potential energy between the main elements cause the crystal structure of the high-entropy alloy to be distorted, which will hinder the movement of atoms and make it difficult to diffuse in the high-entropy alloy, thereby inhibiting the diffusion rate of atoms, which can improve the performance of the brazed joint while effectively reducing the corrosion of the base material.

[0028] 3. The pure Ti foil in the composite solder of this embodiment can be transformed into β-Ti during brazing, which increases the diffusion coefficient and solubility of melting-reducing elements such as Cu, Ni, and Co in the pure Ti foil, causing the pure Ti foil to melt before the TC4 base material, allowing the Ti element to fully react with the solder and improve the joint strength.

[0029] 4. The main product form of the composite solder in this embodiment is foil, which has uniform composition, is easy to assemble, and can better control the width of the soldering seam. It is an ideal solder material, more suitable for actual production, and can greatly improve the joint strength under the condition of low dissolution of the base material.

[0030] Specific embodiment 2: This embodiment is different from specific embodiment 1 in that: the purity of the Ti foil is 99.9wt.%.

[0031] Specific embodiment three: This embodiment is different from specific embodiment one or two in that the TiZrHfCuNiCo amorphous high entropy foil is composed of 12-30% Ti, 12-30% Zr, 12-30% Hf, 12-30% Cu, 12-30% Ni and 12-30% Co in atomic percentage.

[0032] Specific embodiment 4: This embodiment is suitable for the preparation method of the composite brazing material for low-corrosion brazing of titanium alloy thin-walled structural parts according to the following steps:

[0033] Step 1: weigh the raw materials of TiZrHfCuNiCo amorphous high entropy foil according to atomic percentage;

[0034] The TiZrHfCuNiCo amorphous high entropy foil is composed of 12-30% Ti, 12-30% Zr, 12-30% Hf, 12-30% Cu, 12-30% Ni and 12-30% Co in atomic percentage;

[0035] Step 2: Melting the raw materials weighed in step 1 to obtain a brazing ingot;

[0036] Step 3: preparing the solder ingot obtained in step 2 into a TiZrHfCuNiCo amorphous high entropy foil by a single-roll spinning method;

[0037] Step 4: placing the Ti foil between two layers of TiZrHfCuNiCo amorphous high entropy foils and compounding them together using an adhesive or resistance spot welding method to prepare a low-dissolution, high-strength amorphous high-entropy composite brazing material for TC4 titanium alloy brazing;

[0038] The thickness ratio of the TiZrHfCuNiCo amorphous high entropy foil to the Ti foil is 0.8-3:1.

[0039] Specific implementation mode 5: This implementation mode is different from specific implementation mode 4 in that the smelting in step 2 is carried out in an arc melting furnace or an induction melting furnace.

[0040] Specific implementation method six: This implementation method is different from specific implementation methods four or five in that the smelting atmosphere in step two is a vacuum or inert gas protective atmosphere.

[0041] Specific implementation method 7: This implementation method is different from any one of specific implementation methods 4 to 6 in that: the thickness of the TiZrHfCuNiCo amorphous high entropy foil in step 3 is 30 to 100 μm.

[0042] Specific implementation eight: This implementation differs from any one of specific implementations four to seven in that: the binder in step four is an aqueous solution of carboxymethyl cellulose with a mass fraction of 20 to 50%.

[0043] Specific embodiment 9: In this embodiment, the method for brazing TC4 titanium alloy using a composite brazing filler metal suitable for low-corrosion brazing of titanium alloy thin-walled structural parts is carried out according to the following steps:

[0044] Step 1: Grind the surface of the TC4 alloy to be welded with fine sandpaper to remove surface oil and oxides, and then put the grinded TC4 alloy and the low-dissolution, high-strength amorphous, high-entropy composite brazing material for TC4 titanium alloy brazing into anhydrous ethanol for ultrasonic cleaning;

[0045] Step 2: Assemble from top to bottom the TC4 alloy, the low-dissolution, high-strength amorphous, high-entropy composite brazing material for TC4 titanium alloy brazing, and the TC4 alloy, and finally put them into a vacuum brazing furnace for brazing, and then complete;

[0046] The brazing process is as follows: heating to 940-960°C at a speed of 10°C / min and keeping the temperature for 10 minutes, then cooling to 150-200°C at a speed of 10-15°C / min, and then cooling to room temperature with the furnace to complete the brazing of the TC4 alloy.

[0047] 1. The TiZrHfCuNiCo amorphous high entropy foil in the low-dissolution, high-strength amorphous high-entropy composite brazing material for TC4 titanium alloy brazing in this embodiment has good wettability with the base material, and has many types of components, high content, and relatively close content of each component. The atomic arrangement is relatively chaotic, so the mixing entropy of the atomic arrangement is very high, thereby inhibiting the formation of intermetallic compounds. At the same time, the atomic sizes of various elements in the high-entropy alloy vary greatly, especially when the mixing entropy of the alloy is high, the coordinated diffusion between the main elements of the alloy becomes difficult, and the differences in atomic size, bond type and lattice potential between the main elements cause the crystal structure of the high-entropy alloy to be distorted, which also hinders the movement of atoms and makes it difficult to diffuse in the high-entropy alloy, thereby inhibiting the diffusion rate of atoms, which can improve the performance of the brazed joint while effectively reducing the corrosion of the base material.

[0048] 3. The pure Ti foil in the composite solder of this embodiment can be transformed into β-Ti during brazing, which increases the diffusion coefficient and solubility of melting-reducing elements such as Cu, Ni, and Co in the pure Ti foil, causing the pure Ti foil to melt before the TC4 base material, allowing the Ti element to fully react with the solder and improve the joint strength.

[0049] 4. The main product form of the composite solder in this embodiment is foil, which has uniform composition, is easy to assemble, and can better control the width of the soldering seam. It is an ideal solder material, more suitable for actual production, and can greatly improve the joint strength under the condition of low dissolution of the base material.

[0050] Specific embodiment ten: This embodiment differs from specific embodiment nine in that the brazing process is as follows: initially heating to 940°C at a rate of 10°C / min and keeping warm for 10 minutes, then cooling to 200°C at a rate of 10°C / min, and then cooling to room temperature in the furnace to complete the brazing of TC4 alloy.

[0051] Embodiment 1:

[0052] The composite brazing filler metal for low-melting brazing of titanium alloy thin-walled structural parts in this embodiment is composed of two layers of TiZrHfCuNiCo amorphous high-entropy foils and a layer of Ti foil, wherein the layer of Ti foil is arranged between the two layers of TiZrHfCuNiCo amorphous high-entropy foils, and the TiZrHfCuNiCo amorphous high-entropy foils and the Ti foil are composited together by a binder or resistance spot welding method;

[0053] The TiZrHfCuNiCo amorphous high entropy foil is composed of 25 at.% Ti, 25 at.% Zr, 25 at.% Hf, 8 at.% Cu, 8 at.% Ni and 9 at.% Co in atomic percentage;

[0054] The purity of the Ti foil is 99.9wt.%;

[0055] The preparation method of the composite brazing material suitable for low-corrosion brazing of titanium alloy thin-walled structural parts is carried out according to the following steps:

[0056] Step 1: weigh the raw materials of TiZrHfCuNiCo amorphous high entropy foil according to atomic percentage;

[0057] Step 2: Melting the raw materials weighed in step 1 to obtain a brazing ingot;

[0058] The smelting is carried out in an arc melting furnace or an induction melting furnace;

[0059] The smelting atmosphere is a vacuum or inert gas protective atmosphere;

[0060] Step 3: preparing the solder ingot obtained in step 2 into a TiZrHfCuNiCo amorphous high entropy foil by a single-roll spinning method;

[0061] The thickness of the TiZrHfCuNiCo amorphous high entropy foil is 50 μm;

[0062] Step 4: placing the Ti foil between two layers of TiZrHfCuNiCo amorphous high entropy foils and compounding them together using an adhesive or resistance spot welding method to prepare a low-dissolution, high-strength amorphous high-entropy composite brazing material for TC4 titanium alloy brazing;

[0063] The thickness ratio of the TiZrHfCuNiCo amorphous high entropy foil to the Ti foil is 2:1;

[0064] The binder is an aqueous solution of carboxymethyl cellulose with a mass fraction of 35%;

[0065] The method for brazing TC4 titanium alloy using the composite brazing filler metal suitable for low-corrosion brazing of titanium alloy thin-walled structural parts is carried out in the following steps:

[0066] Step 1: Grind the surface of the TC4 alloy to be welded with fine sandpaper to remove surface oil and oxides, and then put the grinded TC4 alloy and the low-dissolution, high-strength amorphous, high-entropy composite brazing material for TC4 titanium alloy brazing into anhydrous ethanol for ultrasonic cleaning;

[0067] Step 2: Assemble from top to bottom the TC4 alloy, the low-dissolution, high-strength amorphous, high-entropy composite brazing material for TC4 titanium alloy brazing, and the TC4 alloy, and finally put them into a vacuum brazing furnace for brazing, and then complete;

[0068] The brazing process is as follows: heating to 940°C at a speed of 10°C / min and keeping the temperature for 10 minutes, then cooling to 200°C at a speed of 10°C / min, and then cooling to room temperature in the furnace to complete the brazing of the TC4 alloy.

[0069] Comparative Example 1:

[0070] The method of brazing TC4 titanium alloy using TiZrHfCuNiCo amorphous high entropy foil is carried out in the following steps:

[0071] Step 1: Grind the surface of the TC4 alloy to be welded with fine sandpaper to remove surface oil and oxides, and then put the polished TC4 alloy and TiZrHfCuNiCo amorphous high entropy foil into anhydrous ethanol for ultrasonic cleaning;

[0072] The preparation method of the TiZrHfCuNiCo amorphous high entropy foil is carried out according to the following steps: weighing the raw materials of the TiZrHfCuNiCo amorphous high entropy foil according to atomic percentage; the TiZrHfCuNiCo amorphous high entropy foil is composed of 25at.% Ti, 25at.% Zr, 25at.% Hf, 8at.% Cu, 8at.% Ni and 9at.% Co according to atomic percentage; smelting the weighed raw materials to obtain a solder ingot; the smelting is carried out in an arc melting furnace or an induction melting furnace; the smelting atmosphere is a vacuum or an inert gas protective atmosphere; the solder ingot is prepared into a TiZrHfCuNiCo amorphous high entropy foil by a single roller spinning method; the thickness of the TiZrHfCuNiCo amorphous high entropy foil is 50μm;

[0073] Step 2: Assemble from top to bottom the TC4 alloy, TiZrHfCuNiCo amorphous high entropy foil, and TC4 alloy, and finally put them into a vacuum brazing furnace for brazing.

[0074] The brazing process is as follows: heating to 940°C at a speed of 10°C / min and keeping the temperature for 10 minutes, then cooling to 200°C at a speed of 10°C / min, and then cooling to room temperature in the furnace to complete the brazing of the TC4 alloy.

[0075] Figure 1 The interface microstructure diagram of the TC4 / TiZrHfCuNiCo / pure Ti / TiZrHfCuNiCo / TC4 brazed joint obtained under the brazing condition of 940°C / 10min in Example 1; Figure 2 This is the interface structure diagram of the TC4 / TiZrHfCuNiCo / TC4 brazed joint obtained under the brazing conditions of 940℃ / 10min in the comparative example. Figure 1 and Figure 2It can be seen that, with the same process parameters, there is no residual brazing material layer in the brazed joint obtained by using the composite brazing material in Example 1, and the weld is not significantly widened after welding, while the comparative example uses a single TiZrHfCuNiCo high entropy brazing material, and a residual brazing material layer is generated in the brazed joint, and the weld increases by about 40μm after welding. The joint strength of Example 1 is 248MPa, while that of the comparative example is only 79MPa.

[0076] Embodiment 2:

[0077] The composite brazing filler metal for low-melting brazing of titanium alloy thin-walled structural parts in this embodiment is composed of two layers of TiZrHfCuNiCo amorphous high-entropy foils and a layer of Ti foil, wherein the layer of Ti foil is arranged between the two layers of TiZrHfCuNiCo amorphous high-entropy foils, and the TiZrHfCuNiCo amorphous high-entropy foils and the Ti foil are composited together by a binder or resistance spot welding method;

[0078] The TiZrHfCuNiCo amorphous high entropy foil is composed of 22 at.% Ti, 22 at.% Zr, 22 at.% Hf, 11 at.% Cu, 11 at.% Ni and 12 at.% Co in atomic percentage;

[0079] The purity of the Ti foil is 99.9wt.%;

[0080] The preparation method of the composite brazing material suitable for low-corrosion brazing of titanium alloy thin-walled structural parts is carried out according to the following steps:

[0081] Step 1: weigh the raw materials of TiZrHfCuNiCo amorphous high entropy foil according to atomic percentage;

[0082] Step 2: Melting the raw materials weighed in step 1 to obtain a brazing ingot;

[0083] The smelting is carried out in an arc melting furnace or an induction melting furnace;

[0084] The smelting atmosphere is a vacuum or inert gas protective atmosphere;

[0085] Step 3: preparing the solder ingot obtained in step 2 into a TiZrHfCuNiCo amorphous high entropy foil by a single-roll spinning method;

[0086] The thickness of the TiZrHfCuNiCo amorphous high entropy foil is 50 μm;

[0087] Step 4: placing the Ti foil between two layers of TiZrHfCuNiCo amorphous high entropy foils and compounding them together using an adhesive or resistance spot welding method to prepare a low-dissolution, high-strength amorphous high-entropy composite brazing material for TC4 titanium alloy brazing;

[0088] The thickness ratio of the TiZrHfCuNiCo amorphous high entropy foil to the Ti foil is 2:1;

[0089] The binder is an aqueous solution of carboxymethyl cellulose with a mass fraction of 35%;

[0090] The method for brazing TC4 titanium alloy using the composite brazing filler metal suitable for low-corrosion brazing of titanium alloy thin-walled structural parts is carried out in the following steps:

[0091] Step 1: Grind the surface of the TC4 alloy to be welded with fine sandpaper to remove surface oil and oxides, and then put the grinded TC4 alloy and the low-dissolution, high-strength amorphous, high-entropy composite brazing material for TC4 titanium alloy brazing into anhydrous ethanol for ultrasonic cleaning;

[0092] Step 2: Assemble from top to bottom the TC4 alloy, the low-dissolution, high-strength amorphous, high-entropy composite brazing material for TC4 titanium alloy brazing, and the TC4 alloy, and finally put them into a vacuum brazing furnace for brazing, and then complete;

[0093] The brazing process is as follows: heating to 950°C at a speed of 10°C / min and keeping the temperature for 10 minutes, then cooling to 200°C at a speed of 10°C / min, and then cooling to room temperature with the furnace to complete the brazing of the TC4 alloy.

[0094] Comparative Example 2:

[0095] The method of brazing TC4 titanium alloy using TiZrHfCuNiCo amorphous high entropy foil is carried out in the following steps:

[0096] Step 1: Grind the surface of the TC4 alloy to be welded with fine sandpaper to remove surface oil and oxides, and then put the polished TC4 alloy and TiZrHfCuNiCo amorphous high entropy foil into anhydrous ethanol for ultrasonic cleaning;

[0097] The preparation method of the TiZrHfCuNiCo amorphous high entropy foil is carried out according to the following steps: weighing the raw materials of the TiZrHfCuNiCo amorphous high entropy foil according to atomic percentage; the TiZrHfCuNiCo amorphous high entropy foil is composed of 22at.% Ti, 22at.% Zr, 22at.% Hf, 11at.% Cu, 11at.% Ni and 12at.% Co according to atomic percentage; smelting the weighed raw materials to obtain a solder ingot; the smelting is carried out in an arc melting furnace or an induction melting furnace; the smelting atmosphere is a vacuum or an inert gas protective atmosphere; the solder ingot is prepared into a TiZrHfCuNiCo amorphous high entropy foil by a single roller spinning method; the thickness of the TiZrHfCuNiCo amorphous high entropy foil is 50μm;

[0098] Step 2: Assemble from top to bottom the TC4 alloy, TiZrHfCuNiCo amorphous high entropy foil, and TC4 alloy, and finally put them into a vacuum brazing furnace for brazing.

[0099] The brazing process is as follows: heating to 950°C at a speed of 10°C / min and keeping the temperature for 10 minutes, then cooling to 200°C at a speed of 10°C / min, and then cooling to room temperature with the furnace to complete the brazing of the TC4 alloy.

[0100] The joint strength in Example 2 is 233 MPa, while the joint strength in Comparative Example 2 is only 68 MPa.

[0101] Embodiment 3:

[0102] The composite brazing filler metal for low-melting brazing of titanium alloy thin-walled structural parts in this embodiment is composed of two layers of TiZrHfCuNiCo amorphous high-entropy foils and a layer of Ti foil, wherein the layer of Ti foil is arranged between the two layers of TiZrHfCuNiCo amorphous high-entropy foils, and the TiZrHfCuNiCo amorphous high-entropy foils and the Ti foil are composited together by a binder or resistance spot welding method;

[0103] The TiZrHfCuNiCo amorphous high entropy foil is composed of 20 at.% Ti, 20 at.% Zr, 20 at.% Hf, 13 at.% Cu, 13 at.% Ni and 14 at.% Co in atomic percentage;

[0104] The purity of the Ti foil is 99.9wt.%;

[0105] The preparation method of the composite brazing material suitable for low-corrosion brazing of titanium alloy thin-walled structural parts is carried out according to the following steps:

[0106] Step 1: weigh the raw materials of TiZrHfCuNiCo amorphous high entropy foil according to atomic percentage;

[0107] Step 2: Melting the raw materials weighed in step 1 to obtain a brazing ingot;

[0108] The smelting is carried out in an arc melting furnace or an induction melting furnace;

[0109] The smelting atmosphere is a vacuum or inert gas protective atmosphere;

[0110] Step 3: preparing the solder ingot obtained in step 2 into a TiZrHfCuNiCo amorphous high entropy foil by a single-roll spinning method;

[0111] The thickness of the TiZrHfCuNiCo amorphous high entropy foil is 50 μm;

[0112] Step 4: placing the Ti foil between two layers of TiZrHfCuNiCo amorphous high entropy foils and compounding them together using an adhesive or resistance spot welding method to prepare a low-dissolution, high-strength amorphous high-entropy composite brazing material for TC4 titanium alloy brazing;

[0113] The thickness ratio of the TiZrHfCuNiCo amorphous high entropy foil to the Ti foil is 2:1;

[0114] The binder is an aqueous solution of carboxymethyl cellulose with a mass fraction of 35%;

[0115] The method for brazing TC4 titanium alloy using the composite brazing filler metal suitable for low-corrosion brazing of titanium alloy thin-walled structural parts is carried out in the following steps:

[0116] Step 1: Grind the surface of the TC4 alloy to be welded with fine sandpaper to remove surface oil and oxides, and then put the grinded TC4 alloy and the low-dissolution, high-strength amorphous, high-entropy composite brazing material for TC4 titanium alloy brazing into anhydrous ethanol for ultrasonic cleaning;

[0117] Step 2: Assemble from top to bottom the TC4 alloy, the low-dissolution, high-strength amorphous, high-entropy composite brazing material for TC4 titanium alloy brazing, and the TC4 alloy, and finally put them into a vacuum brazing furnace for brazing, and then complete;

[0118] The brazing process is as follows: heating to 960°C at a speed of 10°C / min and keeping the temperature for 10 minutes, then cooling to 200°C at a speed of 10°C / min, and then cooling to room temperature with the furnace to complete the brazing of the TC4 alloy.

[0119] Comparative Example 3:

[0120] The method of brazing TC4 titanium alloy using TiZrHfCuNiCo amorphous high entropy foil is carried out in the following steps:

[0121] Step 1: Grind the surface of the TC4 alloy to be welded with fine sandpaper to remove surface oil and oxides, and then put the polished TC4 alloy and TiZrHfCuNiCo amorphous high entropy foil into anhydrous ethanol for ultrasonic cleaning;

[0122] The preparation method of the TiZrHfCuNiCo amorphous high entropy foil is carried out according to the following steps: weighing the raw materials of the TiZrHfCuNiCo amorphous high entropy foil according to atomic percentage; the TiZrHfCuNiCo amorphous high entropy foil is composed of 22at.% Ti, 22at.% Zr, 22at.% Hf, 11at.% Cu, 11at.% Ni and 12at.% Co according to atomic percentage; smelting the weighed raw materials to obtain a solder ingot; the smelting is carried out in an arc melting furnace or an induction melting furnace; the smelting atmosphere is a vacuum or an inert gas protective atmosphere; the solder ingot is prepared into a TiZrHfCuNiCo amorphous high entropy foil by a single roller spinning method; the thickness of the TiZrHfCuNiCo amorphous high entropy foil is 50μm;

[0123] Step 2: Assemble from top to bottom the TC4 alloy, TiZrHfCuNiCo amorphous high entropy foil, and TC4 alloy, and finally put them into a vacuum brazing furnace for brazing.

[0124] The brazing process is: heating to 960°C at a rate of 10°C / min and keeping the temperature for 10 minutes, then cooling to 200°C at a rate of 10°C / min, and then cooling to room temperature with the furnace to complete the brazing of TC4 alloy. The joint strength in Example 3 is 198MPa. The joint strength in Comparative Example 3 is only 53MPa.

Claims

1. A composite brazing material suitable for low-corrosion brazing of titanium alloy thin-walled structural parts. Features: The composite brazing filler metal suitable for low-corrosion brazing of titanium alloy thin-walled structural parts is composed of two layers of TiZrHfCuNiCo amorphous high-entropy foils and a layer of Ti foil, wherein the layer of Ti foil is arranged between the two layers of TiZrHfCuNiCo amorphous high-entropy foils, and the TiZrHfCuNiCo amorphous high-entropy foils and the Ti foil are composited together by an adhesive or resistance spot welding.

2. The composite brazing material suitable for low-corrosion brazing of titanium alloy thin-walled structural parts according to claim 1, Features: The purity of the Ti foil was 99.9 wt. %.

3. The composite brazing material suitable for low-corrosion brazing of titanium alloy thin-walled structural parts according to claim 1, Features: The TiZrHfCuNiCo amorphous high entropy foil consists of 12-30% Ti, 12-30% Zr, 12-30% Hf, 12-30% Cu, 12-30% Ni and 12-30% Co in atomic percentage.

4. The method for preparing the composite brazing material suitable for low-corrosion brazing of titanium alloy thin-walled structural parts according to claim 1, Features: The method proceeds as follows: Step 1: weigh the raw materials of TiZrHfCuNiCo amorphous high entropy foil according to atomic percentage; The TiZrHfCuNiCo amorphous high entropy foil is composed of 12-30% Ti, 12-30% Zr, 12-30% Hf, 12-30% Cu, 12-30% Ni and 12-30% Co in atomic percentage; Step 2: Melting the raw materials weighed in step 1 to obtain a brazing ingot; Step 3: preparing the solder ingot obtained in step 2 into a TiZrHfCuNiCo amorphous high entropy foil by a single-roll spinning method; Step 4: placing the Ti foil between two layers of TiZrHfCuNiCo amorphous high entropy foils and compounding them together using an adhesive or resistance spot welding method to prepare a low-dissolution, high-strength amorphous high-entropy composite brazing material for TC4 titanium alloy brazing; The thickness ratio of the TiZrHfCuNiCo amorphous high entropy foil to the Ti foil is 0.8-3:

1.

5. The method for preparing the composite brazing material suitable for low-corrosion brazing of titanium alloy thin-walled structural parts according to claim 4, Features: The smelting in step 2 is carried out in an arc melting furnace or an induction melting furnace.

6. The method for preparing the composite brazing material suitable for low-corrosion brazing of titanium alloy thin-walled structural parts according to claim 4, Features: The smelting atmosphere in step 2 is a vacuum or inert gas protective atmosphere.

7. The method for preparing the composite brazing material suitable for low-corrosion brazing of titanium alloy thin-walled structural parts according to claim 4, Features: Step 3: The thickness of the TiZrHfCuNiCo amorphous high entropy foil is 30-100 μm.

8. The method for preparing the composite brazing material suitable for low-corrosion brazing of titanium alloy thin-walled structural parts according to claim 4, Features: In step 4, the binder is an aqueous solution of carboxymethyl cellulose with a mass fraction of 20 to 50%.

9. A method for brazing TC4 titanium alloy using the composite brazing filler metal suitable for low-corrosion brazing of titanium alloy thin-walled structural parts as claimed in claim 1, Features: The method proceeds as follows: Step 1: Grind the surface of the TC4 alloy to be welded with fine sandpaper to remove surface oil and oxides, and then put the grinded TC4 alloy and the low-dissolution, high-strength amorphous, high-entropy composite brazing material for TC4 titanium alloy brazing into anhydrous ethanol for ultrasonic cleaning; Step 2: Assemble from top to bottom the TC4 alloy, the low-dissolution, high-strength amorphous, high-entropy composite brazing material for TC4 titanium alloy brazing, and the TC4 alloy, and finally put them into a vacuum brazing furnace for brazing, and then complete; The brazing process is as follows: heating to 940-960°C at a speed of 10°C / min and keeping the temperature for 10 minutes, then cooling to 150-200°C at a speed of 10-15°C / min, and then cooling to room temperature with the furnace to complete the brazing of the TC4 alloy.

10. The method for brazing TC4 titanium alloy using a composite brazing filler metal suitable for low-corrosion brazing of titanium alloy thin-walled structural parts according to claim 1, Features: The brazing process is as follows: heating to 940°C at a speed of 10°C / min and keeping the temperature for 10 minutes, then cooling to 200°C at a speed of 10°C / min, and then cooling to room temperature in the furnace to complete the brazing of the TC4 alloy.

Citation Information

Patent Citations

  • Composite foil brazing material

    CA2007382A1

  • Method for preparing titanium based solder

    CN101352787A

  • Near eutectic composition nickel base sandwich braze foil

    CN105246643A

  • Method for brazing ceramic and metal by adopting composite high-entropy alloy solder

    CN107363359A

  • Titanium alloy brazing sandwich structural panel and manufacturing method thereof

    CN109465608A