Modified wood for inhibiting growth of indoor bacteria as well as preparation method and application of modified wood

By introducing MOF nanoparticles into the wood to form composite materials, the humidity regulation and bacterial inhibition of wood are achieved, and the existing problems of low humidity regulation efficiency and insufficient antibacterial effect are solved, and the indoor humidity control and bacterial inhibition are achieved.

CN118893689APending Publication Date: 2024-11-05CHINA UNIV OF MINING & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411207042.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing wood has low humidity regulation efficiency and cannot effectively inhibit indoor bacterial growth. Traditional modified wood can only inhibit its own mold and cannot inhibit bacterial growth in the surrounding environment through humidity regulation.

Method used

Using wood/MOF composite materials, the hygroscopic points and desorption points of MOF nanoparticles are between 40% and 65%, and the hygroscopic capacity is not less than 35%. The MOF nanoparticles are loaded into wood through a specific preparation method to form a modification. Wood to achieve passive humidity regulation and bacterial inhibition.

Benefits of technology

It realizes rapid humidity adjustment, keeps indoor humidity within the ideal range, effectively inhibits indoor bacterial growth, and does not require external energy, and is environmentally friendly and energy-saving.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118893689A_ABST
    Figure CN118893689A_ABST
Patent Text Reader

Abstract

The invention discloses modified wood for inhibiting growth of indoor bacteria as well as a preparation method and application of the modified wood, the modified wood is a wood / MOF composite material, and the loading capacity of MOF nanoparticles in the wood is not less than 5%; the moisture absorption point and the desorption point of the wood / MOF composite material are both 40%-65% in humidity, and the moisture absorption capacity is not less than 35%; if the indoor humidity is higher than the moisture absorption point of the wood / MOF composite material, the wood / MOF composite material can quickly absorb moisture in the surrounding environment so as to reduce the indoor humidity; if the indoor humidity is lower than the desorption point of the wood / MOF composite material, the wood / MOF composite material can quickly release water to the surrounding environment to increase the indoor humidity, and finally the indoor humidity is controlled to be 40%-65%, so that the effect of inhibiting the growth of indoor bacteria is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to modified wood for inhibiting indoor bacterial growth, a preparation method and application thereof, and belongs to the technical field of environmentally friendly building materials. Background Art

[0002] The suitable humidity for human habitation is 40% to 65%. Too low or too high humidity can easily cause human diseases and the growth of fungi (such as Figure 1 As shown). In order to maintain a comfortable temperature and humidity environment for humans, active adjustment is currently mainly carried out through power equipment such as air conditioners, humidifiers and dehumidifiers, which consumes a lot of electricity. Therefore, it is of great significance to develop new environmentally friendly and energy-saving building materials to adjust indoor humidity by passive moisture absorption or dehumidification to achieve the purpose of inhibiting indoor bacterial growth. Wood has a natural indoor humidity regulation function due to its multi-level pore structure and rich hydroxyl groups. However, due to its limited adsorption capacity and slow water diffusion rate, wood has low efficiency and poor effect in humidity regulation. Studies have shown that water vapor has reversible moisture absorption / desorption performance and optimal humidity regulation performance in the pore size range of 3-7.4 nm. Although the rich hierarchical porous structure is a unique natural advantage of wood, this pore structure is unevenly distributed and the pore type is relatively fixed. Currently, the industry improves the wood's ability to absorb / desorb moisture by carbonizing the wood or introducing hygroscopic salts. However, the humidity-controlled wood obtained by such methods has problems such as weak moisture absorption capacity, high regeneration temperature, or the adjusted humidity range is not within the ideal humidity range (40%~65%). It is also impossible to achieve the purpose of inhibiting indoor bacterial growth through passive humidity control.

[0003] In addition, through literature and patent searches, there are currently some modified woods that are formed by compounding wood with other substances or improving the wood itself, so that these modified woods have certain antibacterial effects. However, the antibacterial properties of the above-mentioned modified woods with antibacterial effects are only effective against molds produced by the wood itself, and cannot inhibit bacterial growth by adjusting the humidity of the surrounding environment, thereby failing to achieve an indoor antibacterial effect.

[0004] Therefore, how to provide a new modified wood and a preparation method thereof, so that it can quickly adjust the humidity of the surrounding environment, keep the indoor environment within the required humidity range and thus inhibit bacterial growth, is the research direction required by the present invention. Summary of the invention

[0005] In view of the problems existing in the above-mentioned prior art, the present invention provides a modified wood for inhibiting the growth of indoor bacteria, a preparation method and its application, and adopts a specific wood / MOF composite material so that it can quickly adjust the humidity of the surrounding environment according to the humidity conditions of the indoor environment, maintain the indoor environment in the required humidity range, and thus achieve the purpose of inhibiting bacterial growth.

[0006] In order to achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a modified wood for inhibiting the growth of indoor bacteria, wherein the modified wood is a wood / MOF composite material, wherein the loading amount of MOF (organic framework material) in the wood is not less than 5%; the moisture absorption point and desorption point of the wood / MOF composite material are both between 40% and 65% of humidity, and the moisture absorption capacity is not less than 35%.

[0007] The preparation method of the modified wood for inhibiting indoor bacterial growth comprises the following specific steps: A. Select MOF nanoparticles, the moisture absorption point and desorption point of the selected MOF nanoparticles are between 40% and 65% humidity, and the moisture absorption capacity is not less than 50%; B. dissolving the MOF nanoparticle powder in an ethanol solution and performing ultrasonic dispersion to obtain a MOF solution with a concentration of 1 to 30 g / L; C. Select wood and immerse the wood in the MOF solution prepared in step B for 0.5 to 24 h; D. Drying the composite material after impregnation in step C, the drying time is 0.5 to 24 hours; E. Repeat steps C and D alternately until the loading amount of MOF in the wood exceeds 5% and the loading amount does not increase with continued impregnation; the number of impregnations for different combinations of wood and MOF nanoparticles is different, and the number of impregnations for different types of wood and MOF nanoparticles is determined according to the above conditions; F. Finally, the wood / MOF composite material obtained in step E is dried for 6 to 24 hours to completely remove the solvent, thereby producing modified wood.

[0008] Furthermore, the wood is one of fir, poplar, balsa, spruce, fir, beech and eucalyptus; or one of fir, poplar, balsa, spruce, fir, beech and eucalyptus after delignification treatment; or one of fir, poplar, balsa, spruce, fir, beech and eucalyptus after sodium hydroxide treatment.

[0009] Furthermore, the drying in steps D and E is one of normal pressure drying, vacuum drying and vacuum freeze drying, wherein the drying temperatures of normal pressure drying and vacuum drying are both 65~103ºC; before vacuum freeze drying, the material to be dried is first frozen in a -18°C refrigerator.

[0010] Furthermore, the MOF nanoparticles are made of one of MIL-101(Cr), BIT-66, Y-shp-MOF-5, CAU-1-OH, Cr-soc-MOF-1, NU-1500-Cr, Basolite A300, and Molecular sieve MCM-41. The moisture absorption point and desorption point of these MOF nanoparticles are both between 40% and 65% humidity, and the moisture absorption capacity is not less than 50%.

[0011] Furthermore, the immersion in step C is carried out in a vacuum environment to shorten the immersion time.

[0012] The above-mentioned modified wood is used to inhibit the growth of indoor bacteria. The specific process is: if the indoor humidity is higher than the moisture absorption point of the wood / MOF composite material, the wood / MOF composite material will quickly absorb moisture from the surrounding environment to reduce the indoor humidity; if the indoor humidity is lower than the desorption point of the wood / MOF composite material, the wood / MOF composite material will quickly release moisture to the surrounding environment to increase the indoor humidity, and finally control the indoor humidity at 40%~65%, thereby achieving the effect of inhibiting the growth of indoor bacteria.

[0013] MOF is a type of crystalline material composed of metal ions or clusters and organic ligands, which has good adsorption and storage properties for water vapor. Due to the crystal structure characteristics of MOF, MOF usually exists in powder form. Using wood to load MOF can effectively solve the problem of MOF processing and molding difficulties. Wood / MOF composite materials have widely expanded the application of wood to water treatment, gas adsorption, friction power generation and other fields. Based on the above-mentioned prior art, the inventor of this application has concluded that introducing MOF with high moisture absorption capacity into wood can easily reduce indoor humidity, but the existing wood / MOF composite materials will continue to absorb moisture, making the humidity of the indoor environment lower than 40%, which will also cause bacterial growth; in order to achieve the purpose of inhibiting the growth of indoor bacteria, the inventor has conducted Through innovative research, they finally prepared a wood / MOF composite material with a moisture absorption point and desorption point between 40% and 65% humidity and a moisture absorption capacity of more than 35% by using specific preparation parameters to form a modified wood. This modified wood is used as a building material for interior decoration. When the indoor humidity is higher than the moisture absorption point, the wood / MOF composite material will quickly absorb moisture from the surrounding environment to reduce the indoor humidity; when the indoor humidity is lower than the desorption point, the wood / MOF composite material will quickly release moisture to the surrounding environment to increase the indoor humidity, and finally control the indoor humidity at 40%~65%, achieving the effect of inhibiting the growth of indoor bacteria. The entire process of regulating humidity and inhibiting bacterial growth does not require external energy consumption, but is only achieved through the material's own passive absorption and release of moisture, which not only saves energy and reduces emissions, but is also more environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a schematic diagram of the growth of bacteria in indoor environments at different humidity levels; Figure 2 It is the SEM image of MIL-101(Cr) nanoparticles in the experimental proof; Figure 3 It is the XRD pattern of untreated wood, MIL-101(Cr) and wood / MIL-101(Cr) composites in the test proof; Figure 4 The test demonstrates bacterial growth in test rooms constructed with a) no windows, b) untreated wood windows and c) wood / MIL-101(Cr) composite windows at 95% humidity and 37ºC. DETAILED DESCRIPTION

[0015] The present invention will be further described below. Example

[0016] Balsa wood / MIL-101 (Cr) composite material is selected as the modified wood. The moisture absorption point and desorption point of the modified material are both between 40% and 65% of humidity, and the moisture absorption capacity is not less than 35%.

[0017] First prepare MIL-101(Cr): 1. Prepare 150 mL of 0.05 mol L -1 Sodium acetate (C2H3NaO2, purity ≥99.0%) aqueous solution; 2. Add 4.95 g (0.03 mol) of terephthalic acid (C6H4(CO2H)2) ​​and 12 g of chromium nitrate (Cr(NO3)3) to the above aqueous solution; 3. Transfer the mixed solution into an autoclave and place it in an oven at 200°C for 20 hours; 4. After the reaction, slowly cool to room temperature, collect the synthesized MIL-101(Cr) by centrifugation, and wash twice with dimethylformamide (DMF), ethanol and water respectively; 5. Finally, the obtained product was dried in a vacuum oven at 120°C to obtain MIL-101(Cr) powder; thereby preparing the desired MOF nanoparticles; Annex Figure 2 The scanning electron microscope (SEM) image of MIL-101(Cr) is shown.

[0018] The method of the present invention is used to prepare a balsa wood / MIL-101 (Cr) composite material: Step 1: dissolving the above-mentioned MIL-101(Cr) powder in an ethanol solution and performing ultrasonic dispersion to obtain a MIL-101(Cr) solution with a concentration of 10 g / L; Step 2: Select balsa wood and obtain a cross section of the wood with a size of 40 mm × 40 mm × 1 mm (tangential × radial × longitudinal), and immerse the wood in the MIL-101 (Cr) solution prepared in step 1 for 4 h; Step 3, drying the impregnated composite material in an oven at normal pressure for 6 h; Step 4, alternately perform the dipping of step 2 and the drying of step 3 15 times each and then stop; Step 5: Finally, the wood / MOF composite material obtained in step 4 is dried in an oven at 103°C under normal pressure for 6 h to completely remove the solvent, thereby preparing a wood / MIL-101 (Cr) composite material as modified wood. Figure 2 X-ray diffraction (XRD) patterns of MIL-101(Cr), untreated wood and modified wood are shown. Example

[0019] Poplar wood / Y-shp-MOF-5 composite material was selected as the modified wood. The moisture absorption point and desorption point of the modified material were both between 40% and 65% humidity, and the moisture absorption capacity was not less than 35%.

[0020] Colorless Y-shp-MOF-5 powder was prepared as MOF nanoparticles according to the literature J. Am. Chem. Soc. 2017, 139, 31, 10715–10722; The method of the present invention is used to prepare a poplar wood / Y-shp-MOF-5 composite material: Step 1, dissolving the above Y-shp-MOF-5 powder in an ethanol solution and performing ultrasonic dispersion to obtain a Y-shp-MOF-5 solution with a concentration of 10 g / L; Step 2: Select balsa wood and obtain a cross section of the wood with a size of 40 mm × 40 mm × 1 mm (tangential × radial × longitudinal), and immerse the wood in the Y-shp-MOF-5 solution prepared in step 1 under vacuum for 4 hours; Step 3, drying the impregnated composite material in an oven at normal pressure for 6 h; Step 4, alternately perform the dipping of step 2 and the drying of step 3 15 times each and then stop; Step 5. Finally, the wood / MOF composite material obtained in step 4 is dried in an oven at 103°C under normal pressure for 6 h to completely remove the solvent, thereby preparing a poplar / Y-shp-MOF-5 composite material as a modified wood. Example

[0021] Delignified balsa wood / BIT-66 composite material was selected as the modified wood. The moisture absorption point and desorption point of the modified material were both between 40% and 65% of humidity, and the moisture absorption capacity was not less than 35%.

[0022] Green BIT-66 was prepared as MOF nanoparticles according to the literature Angew. Chem. Int. Ed. 2020, 59, 3905; The method of the present invention is used to prepare a delignified balsa wood / BIT-66 composite material: Step 1: dissolving the BIT-66 powder in an ethanol solution and performing ultrasonic dispersion to obtain a Y-shp-MOF-5 solution with a concentration of 10 g / L; Step 2: Select a tangential section of balsa wood with a size of 40 mm × 40 mm × 1 mm (tangential × longitudinal × radial). According to the literature ACS Appl. Mater. Interfaces 2024, 16, 14, 18173–18183, the wood is delignified and freeze-dried. Delignification can increase the micro-nano pore structure of the wood and increase the loading amount of MOF in the wood. The delignified balsa wood is immersed in the BIT-66 solution prepared in step 1 for 4 h. Step 3, drying the impregnated composite material in an oven at 65°C under normal pressure for 6 h; Step 4, alternately perform the dipping of step 2 and the drying of step 3 three times each and then stop; Step 5. Finally, the wood / MOF composite material obtained in step 4 is dried in an oven at 65°C under normal pressure for 6 h to completely remove the solvent, thereby preparing a delignified balsa wood / BIT-66 composite material as modified wood.

[0023] The balsa wood / MIL-101 (Cr) composite material prepared in Example 1 was subjected to an indoor bacteria inhibition test: Since E. coli is sensitive to humidity differences, E. coli ( E. coli Top10 strain, Invitrogen, cat# C404010) was used as a model organism to verify the effect of modified wood on inhibiting the proliferation of indoor bacterial cells.

[0024] E. coliThe Top10 strain was spread on an agar plate. The agar medium formula and preparation steps were as follows: 1 g casein peptone, 5 g yeast extract, 1 g NaCl, and 1.5 g agar were dissolved in distilled water and added to 100 mL. Sterilize at 121°C for 20 min and then cool to 55°C; pour the prepared medium into a petri dish, seal it with a film, and store it at 4°C.

[0025] will be dispersed E. coli The plates of Top10 strains were placed in the test room for cultivation. The test room was 7 cm × 7 cm × 5 cm (length × width × height). The test room was placed in an environment with a humidity of 95% and a temperature of 37ºC. The number of E. coli colonies in the culture dishes in the test room was recorded over 8 hours. In order to show the sample effect, the test room was set up in three conditions: no windows, four pieces of unmodified wood as windows, and four pieces of the above wood / MIL-101(Cr) composite materials as windows.

[0026] The bacteria grew normally in the case of no window and four pieces of unmodified wood as windows, indicating that the unmodified wood has no antibacterial effect. Figure 4 a and 4b; when there are four pieces of the above wood / MIL-101 (Cr) composite material as windows, the bacterial growth is inhibited, and the inhibition rate is greater than 90%. Figure 4 As shown in c, this indicates that introducing MOF with the ability to regulate specific humidity parameters into wood can increase the inhibitory effect of wood products on indoor bacteria.

[0027] In addition, the above test was repeated in Examples 2 and 3, and the antibacterial rates thereof were all greater than 90%, which also illustrates that the different modified woods prepared by the present invention all have good inhibitory effects on indoor bacteria.

[0028] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A modified wood for inhibiting indoor bacterial growth, characterized in that: The modified wood is a wood / MOF composite material, wherein the loading amount of MOF in the wood is not less than 5%; the moisture absorption point and desorption point of the wood / MOF composite material are both between 40% and 65% humidity, and the moisture absorption capacity is not less than 35%.

2. A method for preparing the modified wood for inhibiting indoor bacterial growth according to claim 1, characterized in that: The specific steps are: A. Select MOF nanoparticles, the moisture absorption point and desorption point of the selected MOF nanoparticles are between 40% and 65% humidity, and the moisture absorption capacity is not less than 50%; B. dissolving the MOF nanoparticle powder in an ethanol solution and performing ultrasonic dispersion to obtain a MOF solution with a concentration of 1 to 30 g / L; C. Select wood and immerse the wood in the MOF solution prepared in step B for 0.5 to 24 h; D. Drying the composite material after impregnation in step C, the drying time is 0.5 to 24 hours; E. Repeat steps C and D alternately until the loading of MOF in the wood exceeds 5% and the loading does not increase with continued impregnation; F. Finally, the wood / MOF composite material obtained in step E is dried for 6 to 24 hours to completely remove the solvent, thereby producing modified wood.

3. The preparation method according to claim 2, characterized in that: The wood is one of fir, poplar, balsa, spruce, fir, beech and eucalyptus; or one of fir, poplar, balsa, spruce, fir, beech and eucalyptus treated with delignification; or one of fir, poplar, balsa, spruce, fir, beech and eucalyptus treated with sodium hydroxide.

4. The preparation method according to claim 2, characterized in that: The drying in steps D and E is one of normal pressure drying, vacuum drying and vacuum freeze drying, wherein the drying temperatures of normal pressure drying and vacuum drying are both 65-103°C; before vacuum freeze drying, the material to be dried is first frozen in a -18°C refrigerator.

5. The preparation method according to claim 2, characterized in that the MOF nanoparticles are made of one of MIL-101(Cr), BIT-66, Y-shp-MOF-5, CAU-1-OH, Cr-soc-MOF-1, NU-1500-Cr, Basolite A300, and Molecular sieve MCM-41.

6. The preparation method according to claim 2, characterized in that: The dipping in step C is carried out in a vacuum environment to shorten the dipping time.

7. An application of the modified wood according to claim 1 for inhibiting indoor bacterial growth, the specific process is: if the indoor humidity is higher than the moisture absorption point of the wood / MOF composite material, the wood / MOF composite material will quickly absorb moisture from the surrounding environment to reduce the indoor humidity; if the indoor humidity is lower than the desorption point of the wood / MOF composite material, the wood / MOF composite material will quickly release moisture to the surrounding environment to increase the indoor humidity, and finally control the indoor humidity at 40%~65%, thereby achieving the effect of inhibiting indoor bacterial growth.