Coal-based graphene with few-layer structure and preparation method thereof
Through pickling, swelling, ultrasonication and high-temperature calcination treatment, coal-based graphene was prepared, which solved the problem of using catalysts and strong oxidants in the prior art, and achieved efficient preparation and excellent absorption performance of coal-based graphene .
Patent Information
- Application Number
- CN202410935902.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-12
AI Technical Summary
The introduction of catalysts and harsh graphitization conditions in the existing coal-based graphene preparation methods increase production costs. The use of strong oxidants causes damage to the chemical structure of coal, making it difficult to maintain the complete chemical structure of coal for high-value applications.
By pickling the coal raw material, heating and reflux with a swelling agent, sonication and high-temperature calcination, a free coal-based aromatic conjugated sheet structure was obtained, which was directly calcined under the conditions of catalyst without a catalyst, and the aromatic conjugated sheet structure was retained. , reduce the agglomeration of heteroatomic elements, improve specific surface area and absorbing properties.
The preparation of coal-based graphene in the absence of catalyst is achieved, and the aromatic conjugated sheet structure is retained, with a large specific surface area and excellent absorbing properties. The minimum reflection loss can reach -34.2dB, avoiding the increase in production costs. and chemical structural damage.
Smart Images

Figure CN118894525A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of high-value application of coal, and specifically relates to a coal-based graphene with a few-layer structure and a preparation method thereof. Background Art
[0002] Coal is the primary energy with the most abundant reserves and the most extensive uses in the world. It is an indispensable part of global energy consumption. High-value coal is one of the indispensable development directions for achieving clean and efficient use of coal. Therefore, actively carrying out non-energy utilization of coal and high-value-added deep processing and transformation have received close attention and high attention from all walks of life.
[0003] In the prior art, there are methods of oxidizing coal with a strong oxidant and then reducing it to obtain coal-based graphene; there are also methods of greatly increasing the graphitization degree of coal raw materials by introducing a catalyst and treating it at high temperature, and then obtaining coal-based graphene by adding a strong oxidant and treating it with thermal reduction. Although the above-mentioned coal-based graphene preparation methods are expected to provide a direction for the large-scale production of coal-based graphene, the introduction of catalysts and harsh graphitization conditions during the preparation process increase the production cost, and the use of strong oxidants also causes serious damage to the chemical structure of the coal itself.
[0004] Therefore, if the coal in an aggregated state can be dissociated into a free state while maintaining the integrity of its chemical structure, the structural advantages of the coal itself can be fully utilized and applied in a high-value manner. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies of the prior art, provide a few-layer structure coal-based graphene and a preparation method thereof, and solve the problems in the above-mentioned background technology.
[0006] The technical solution adopted by the present invention to solve the technical problem is: a method for preparing coal-based graphene with a few-layer structure is provided, comprising the following steps:
[0007] (1) grinding the coal raw material and performing an acid washing treatment to obtain a cleaned coal raw material;
[0008] (2) mixing the impurity-removed coal raw material with a swelling agent and heating and refluxing the mixture to make it swell, thereby obtaining a coal swelling product;
[0009] (3) subjecting the coal swelling product to ultrasonic treatment to remove the solvent to obtain a coal dissociation product;
[0010] (4) calcining the coal dissociation product to obtain coal-based graphene.
[0011] In a preferred embodiment of the present invention, in step (1), the coal raw material includes anthracite, lignite or bituminous coal. The particle size of the coal raw material is preferably ≤74 μm. When the particle size of the coal raw material does not meet the above requirements, the coal raw material is crushed, sieved and ground in sequence. The grinding time is preferably 2 to 4 hours, more preferably 2 to 3 hours; the grinding method is preferably ball milling.
[0012] The pickling treatment is carried out in sequence by using a hydrochloric acid aqueous solution or a hydrofluoric acid aqueous solution, wherein the volume ratio of concentrated hydrochloric acid to water in the hydrochloric acid aqueous solution is 20-100:180-100, more preferably 40-80:160-120; the volume ratio of hydrofluoric acid to water in the hydrofluoric acid aqueous solution is 20-100:180-100, more preferably 40-80:160-120. The volume ratio of the mass of the coal raw material to the hydrochloric acid aqueous solution or the hydrofluoric acid aqueous solution is 1-5 g:160-240 mL, more preferably 2-4 g:180-220 mL.
[0013] After the acid washing is completed, the present invention preferably dries the acid washed product in sequence to obtain the impurity-removed coal raw material. The drying temperature is preferably 50-80°C, more preferably 60-70°C; the drying time is preferably 10-14h, more preferably 12-13h.
[0014] After obtaining the impurity-free coal raw material, the present invention mixes the impurity-free coal raw material with a swelling agent and heats and refluxes to maximize the coal swelling degree. In this state, the intermolecular interactions such as π-π bonds and van der Waals forces in the coal structure can be greatly weakened.
[0015] In a preferred embodiment of the present invention, in step (2), the swelling agent is N-methylpyrrolidone / carbon disulfide, pyridine / xylene, N,N-dimethylformamide / toluene, and the volume ratio of the two components in the swelling agent is 40-60:60-40, preferably 50:50. The volume ratio of the mass of the impurity-removed coal raw material to the swelling agent is 0.1-0.5g:80-120mL, preferably 0.2-0.4g:90-110mL. The heating temperature of the heating reflux is 60-100°C, and the reflux reaction time is 12-36h, preferably 80-100°C, 18-30h.
[0016] After the swelling is completed, the present invention directly subjects the mixed solution of the impurity-removed coal and the swelling agent in the swollen state to ultrasonic treatment. Under the continuous action of the cavitation effect generated by the ultrasound, the coal in the solution will maintain a thermal swelling state and will fully dissociate, thereby obtaining a free coal-based aromatic conjugated sheet structure.
[0017] In a preferred embodiment of the present invention, in step (3), ultrasonic treatment is carried out in an ice bath with an ultrasonic power of 20 to 25 kW and a duration of 3 to 10 h, preferably 3 to 5 h.
[0018] The product treated with ultrasound is filtered, washed and freeze-dried, and then the solvent is removed to obtain a coal dissociation product. In the present invention, the coal dissociation product is dispersed in tert-butanol, and the tert-butanol solution is freeze-dried in the present invention. The freeze-drying process can reduce the agglomeration of the coal dissociation product. In the present invention, the ratio of the mass of the coal dissociation product to the volume of tert-butanol is preferably 0.1-0.5g:80-120mL, and more preferably 0.2-0.4g:90-110mL. In the present invention, the time required for the freeze drying is preferably 36-50h.
[0019] High temperature calcination can remove most of the sulfur, nitrogen and oxygen elements in the form of gaseous compounds, retaining the aromatic conjugated sheet structure. In the present invention, the calcination atmosphere is preferably argon; and the calcination device is preferably a tubular furnace.
[0020] In a preferred embodiment of the present invention, in step (4), the heating rate of the calcination treatment is 5-10°C / min, the calcination temperature is 1000-1500°C, and the duration is 1-3h, preferably 1200-1500°C, and the duration is 2-3h. In the present invention, the rate of heating to the high temperature calcination temperature is preferably 5-10°C / min.
[0021] The present invention also provides a few-layer structure coal-based graphene prepared by the above method, which has an aromatic conjugated sheet structure.
[0022] Compared with the background technology, this technical solution has the following advantages:
[0023] 1. The present invention can obtain a free coal-based aromatic conjugated sheet structure by dissociating coal in an aggregated state, and directly calcine the coal-based graphene under catalyst-free doping conditions;
[0024] 2. The present invention uses coal as raw material and utilizes the advantages of the molecular structure of coal itself. First, impurities such as ash and minerals in the coal are removed by acid washing, and then the coal is mixed with a swelling agent and heated and refluxed to put the coal in a swollen state, which can greatly weaken the molecular interaction forces such as π-π bonds and van der Waals forces in the coal structure. Then, under the continuous action of the cavitation effect generated by ultrasound, the coal in the swollen state is dissociated to obtain a free coal-based aromatic conjugated sheet structure. Finally, the structure is directly subjected to high-temperature calcination treatment, which can remove most of the heteroatoms (sulfur, nitrogen, and oxygen elements) in the form of gaseous compounds, retaining the aromatic conjugated sheet structure, and the high-temperature calcination will not cause agglomeration of the sheet structure material, thereby ensuring the specific surface area of the product coal-based graphene;
[0025] 3. The few-layered coal-based graphene obtained by the present invention retains the aromatic conjugated sheet structure, forming a two-dimensional sheet material composed of carbon atoms stacked periodically and closely in a benzene ring structure (i.e., a hexagonal honeycomb structure), with a large specific surface area (specific surface area of 615.2 m 2 / g) and has excellent wave absorbing performance, with the minimum reflection loss reaching -34.2dB. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is a diagram of the peeling mechanism in the preparation method;
[0027] Figure 2 Schematic diagram of the structure of coal-based graphene prepared in Example 1;
[0028] Figure 3 a and b are SEM images (different fields of view) of the coal-based graphene prepared in Example 1;
[0029] Figure 4 Ac are TEM images of the coal-based graphene prepared in Example 1 (different magnifications);
[0030] Figure 5 This is a diagram showing the microwave absorption performance of the coal-based graphene prepared in Example 1. DETAILED DESCRIPTION
[0031] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Example 1
[0033] The present embodiment provides a method for preparing coal-based graphene with a few-layer structure, comprising the following steps:
[0034] (1) crushing anthracite coal blocks and sieving them to obtain coal powder with a particle size of no more than 74 μm; using a hydrochloric acid aqueous solution prepared by 50 mL of concentrated hydrochloric acid and 150 mL of deionized water to soak the above coal powder (weighing 3 g) for pickling, after the hydrochloric acid pickling is completed, suction filtration is performed, and then the filter cake is dispersed in a hydrofluoric acid aqueous solution prepared by 50 mL of concentrated hydrofluoric acid and 150 mL of deionized water. After the hydrofluoric acid pickling is completed, suction filtration is performed, and the filter cake is dried at 60° C. for 12 hours to obtain a decontaminated coal raw material;
[0035] (2) 0.3 g of the above impurity-removed coal raw material was mixed with 100 mL of N-methylpyrrolidone / carbon disulfide swelling agent (the volume ratio of N-methylpyrrolidone to carbon disulfide was 50 mL:50 mL), and heated to 100 ° C in an oil bath under magnetic stirring at 400 r / min for reflux reaction for 24 h to obtain a coal swelling product;
[0036] (3) After heating, the mixed solution was ultrasonicated at a frequency of 20 kHz for 5 h, and the entire ultrasonic process was carried out under ice bath conditions; the solution was filtered, and the filter cake was washed with tert-butanol for 3 times, with tert-butanol used in an amount of 50 mL each time. After washing, the filter cake was dispersed in 100 mL of tert-butanol, and the tert-butanol dispersion of the coal dissociation product was cold-dried for 48 h to obtain the coal dissociation product.
[0037] (4) placing the coal dissociation product in a tubular furnace, and then heating it to 1200° C. at a rate of 5° C. / min under argon protection, and keeping the temperature for 3 hours to obtain the product coal-based graphene.
[0038] The peeling mechanism of this embodiment is as follows Figure 1 The coal dissociation product is directly calcined to obtain coal-based graphene, which retains the aromatic conjugated sheet structure. Figure 2 The coal-based graphene prepared in Example 1 was observed under a scanning electron microscope and a transmission electron microscope, respectively, and the microscopic morphology was obtained as shown in FIG. Figure 3 a, b and Figure 4 It can be seen that the coal-based graphene prepared in this embodiment has an obvious two-dimensional layer structure.
[0039] Wave absorption performance test: The prepared coal-based graphene and paraffin were mixed in a ratio of 0.015g:0.085g to prepare a test sample, and the wave absorption performance test was carried out. The test results are shown in Figure 5 As can be seen from the figure, the coal-based graphene prepared by the present invention has excellent wave absorbing performance, and the minimum reflection loss can reach -34.2dB.
[0040] Example 2
[0041] (1) crushing anthracite coal blocks and sieving them to obtain coal powder with a particle size of no more than 74 μm; using a hydrochloric acid aqueous solution prepared by 50 mL of concentrated hydrochloric acid and 150 mL of deionized water to soak the above coal powder (weighing 3 g) for pickling, after the hydrochloric acid pickling is completed, suction filtration is performed, and then the filter cake is dispersed in a hydrofluoric acid aqueous solution prepared by 50 mL of concentrated hydrofluoric acid and 150 mL of deionized water. After the hydrofluoric acid pickling is completed, suction filtration is performed, and the filter cake is dried at 60° C. for 12 hours to obtain a decontaminated coal raw material;
[0042] (2) 0.3 g of the above impurity-removed coal raw material was mixed with 100 mL of N-methylpyrrolidone / carbon disulfide swelling agent (the volume ratio of N-methylpyrrolidone to carbon disulfide was 50 mL:50 mL), and heated to 100 ° C in an oil bath under magnetic stirring at 400 r / min for reflux reaction for 24 h to obtain a coal swelling product;
[0043] (3) After heating, the mixed solution was ultrasonicated at a frequency of 25 kHz for 5 h, and the entire ultrasonic process was carried out under ice bath conditions. The solution was filtered, and the filter cake was washed with tert-butanol for 3 times, with tert-butanol used in an amount of 50 mL each time. After washing, the filter cake was dispersed in 100 mL of tert-butanol, and the tert-butanol dispersion of the coal dissociation product was cold-dried for 48 h to obtain the coal dissociation product.
[0044] (4) placing the coal dissociation product in a tubular furnace, and then heating it to 1200° C. at a rate of 5° C. / min under argon protection, and keeping the temperature for 3 hours to obtain the product coal-based graphene.
[0045] Example 3
[0046] (1) crushing anthracite coal blocks and sieving them to obtain coal powder with a particle size of no more than 74 μm; using a hydrochloric acid aqueous solution prepared by 50 mL of concentrated hydrochloric acid and 150 mL of deionized water to soak the above coal powder (weighing 3 g) for pickling, after the hydrochloric acid pickling is completed, suction filtration is performed, and then the filter cake is dispersed in a hydrofluoric acid aqueous solution prepared by 50 mL of concentrated hydrofluoric acid and 150 mL of deionized water. After the hydrofluoric acid pickling is completed, suction filtration is performed, and the filter cake is dried at 60° C. for 12 hours to obtain a decontaminated coal raw material;
[0047] (2) 0.3 g of the above impurity-removed coal raw material was mixed with 100 mL of N-methylpyrrolidone / carbon disulfide swelling agent (the volume ratio of N-methylpyrrolidone to carbon disulfide was 50 mL:50 mL), and heated to 100 ° C in an oil bath under magnetic stirring at 400 r / min for reflux reaction for 24 h to obtain a coal swelling product;
[0048] (3) After heating, the mixed solution was ultrasonicated at a frequency of 20 kHz for 10 h, and the entire ultrasonic process was carried out in an ice bath. The solution was filtered, and the filter cake was washed with tert-butanol for 3 times, with tert-butanol used in an amount of 50 mL each time. After washing, the filter cake was dispersed in 100 mL of tert-butanol, and the tert-butanol dispersion of the coal dissociation product was cold-dried for 48 h to obtain the coal dissociation product.
[0049] (4) placing the coal dissociation product in a tubular furnace, and then heating it to 1200° C. at a rate of 5° C. / min under argon protection, and keeping the temperature for 3 hours to obtain the product coal-based graphene.
[0050] Example 4
[0051] (1) crushing anthracite coal blocks and sieving them to obtain coal powder with a particle size of no more than 74 μm; using a hydrochloric acid aqueous solution prepared by 50 mL of concentrated hydrochloric acid and 150 mL of deionized water to soak the above coal powder (weighing 3 g) for pickling, after the hydrochloric acid pickling is completed, suction filtration is performed, and then the filter cake is dispersed in a hydrofluoric acid aqueous solution prepared by 50 mL of concentrated hydrofluoric acid and 150 mL of deionized water. After the hydrofluoric acid pickling is completed, suction filtration is performed, and the filter cake is dried at 60° C. for 12 hours to obtain a decontaminated coal raw material;
[0052] (2) 0.3 g of the above impurity-removed coal raw material was mixed with 100 mL of N-methylpyrrolidone / carbon disulfide swelling agent (the volume ratio of N-methylpyrrolidone to carbon disulfide was 50 mL:50 mL), and the mixture was heated to 90° C. in an oil bath under magnetic stirring at 400 r / min for reflux reaction for 24 h to obtain a coal swelling product;
[0053] (4) After heating, the mixed solution was ultrasonicated at a frequency of 20 kHz for 5 h, and the entire ultrasonic process was carried out under ice bath conditions. The solution was filtered, and the filter cake was washed with tert-butanol for 3 times, with tert-butanol used in each wash in an amount of 50 mL. After washing, the filter cake was dispersed in 100 mL of tert-butanol, and the tert-butanol dispersion of the coal dissociation product was cold-dried for 48 h to obtain the coal dissociation product.
[0054] (4) placing the coal dissociation product in a tubular furnace, and then heating it to 1200° C. at a rate of 5° C. / min under argon protection, and keeping the temperature for 3 hours to obtain the product coal-based graphene.
[0055] Example 5
[0056] (1) crushing anthracite coal blocks and sieving them to obtain coal powder with a particle size of no more than 74 μm; using a hydrochloric acid aqueous solution prepared by 50 mL of concentrated hydrochloric acid and 150 mL of deionized water to soak the above coal powder (weighing 3 g) for pickling, after the hydrochloric acid pickling is completed, suction filtration is performed, and then the filter cake is dispersed in a hydrofluoric acid aqueous solution prepared by 50 mL of concentrated hydrofluoric acid and 150 mL of deionized water. After the hydrofluoric acid pickling is completed, suction filtration is performed, and the filter cake is dried at 60° C. for 12 hours to obtain a decontaminated coal raw material;
[0057] (2) 0.3 g of the above impurity-removed coal raw material was mixed with 100 mL of N-methylpyrrolidone / carbon disulfide swelling agent (the volume ratio of N-methylpyrrolidone to carbon disulfide was 50 mL:50 mL), and heated to 100 ° C in an oil bath under magnetic stirring at 400 r / min for reflux reaction for 24 h to obtain a coal swelling product;
[0058] (3) After heating, the mixed solution was ultrasonicated at a frequency of 20 kHz for 5 h, and the entire ultrasonic process was carried out under ice bath conditions. The solution was filtered, and the filter cake was washed with tert-butanol for 3 times, with tert-butanol used in an amount of 50 mL each time. After washing, the filter cake was dispersed in 100 mL of tert-butanol, and the tert-butanol dispersion of the coal dissociation product was cold-dried for 48 h to obtain the coal dissociation product.
[0059] (4) placing the coal dissociation product in a tubular furnace, and then heating it to 1200° C. at a rate of 10° C. / min under argon protection, and keeping the temperature for 3 hours to obtain the product coal-based graphene.
[0060] Example 6
[0061] (1) crushing anthracite coal blocks and sieving them to obtain coal powder with a particle size of no more than 74 μm; using a hydrochloric acid aqueous solution prepared by 50 mL of concentrated hydrochloric acid and 150 mL of deionized water to soak the above coal powder (weighing 3 g) for pickling, after the hydrochloric acid pickling is completed, suction filtration is performed, and then the filter cake is dispersed in a hydrofluoric acid aqueous solution prepared by 50 mL of concentrated hydrofluoric acid and 150 mL of deionized water. After the hydrofluoric acid pickling is completed, suction filtration is performed, and the filter cake is dried at 60° C. for 12 hours to obtain a decontaminated coal raw material;
[0062] (2) 0.3 g of the above impurity-removed coal raw material was mixed with 100 mL of N-methylpyrrolidone / carbon disulfide swelling agent (the volume ratio of N-methylpyrrolidone to carbon disulfide was 50 mL:50 mL), and heated to 100 ° C in an oil bath under magnetic stirring at 400 r / min for reflux reaction for 24 h to obtain a coal swelling product;
[0063] (3) After heating, the mixed solution was ultrasonicated at a frequency of 20 kHz for 5 h, and the entire ultrasonic process was carried out under ice bath conditions. The solution was filtered, and the filter cake was washed with tert-butanol for 3 times, with tert-butanol used in an amount of 50 mL each time. After washing, the filter cake was dispersed in 100 mL of tert-butanol, and the tert-butanol dispersion of the coal dissociation product was cold-dried for 48 h to obtain the coal dissociation product.
[0064] (4) placing the coal dissociation product in a tubular furnace, and then heating it to 1400° C. at a rate of 5° C. / min under argon protection, and keeping the temperature for 3 hours to obtain the product coal-based graphene.
[0065] Example 7
[0066] (1) crushing anthracite coal blocks and sieving them to obtain coal powder with a particle size of no more than 74 μm; using a hydrochloric acid aqueous solution prepared by 50 mL of concentrated hydrochloric acid and 150 mL of deionized water to soak the above coal powder (weighing 3 g) for pickling, after the hydrochloric acid pickling is completed, suction filtration is performed, and then the filter cake is dispersed in a hydrofluoric acid aqueous solution prepared by 50 mL of concentrated hydrofluoric acid and 150 mL of deionized water. After the hydrofluoric acid pickling is completed, suction filtration is performed, and the filter cake is dried at 60° C. for 12 hours to obtain a decontaminated coal raw material;
[0067] (2) 0.3 g of the above impurity-removed coal raw material was mixed with 100 mL of N-methylpyrrolidone / carbon disulfide swelling agent (the volume ratio of N-methylpyrrolidone to carbon disulfide was 50 mL:50 mL), and heated to 100 ° C in an oil bath under magnetic stirring at 400 r / min for reflux reaction for 24 h to obtain a coal swelling product;
[0068] (3) After heating, the mixed solution was ultrasonicated at a frequency of 25 kHz for 3 h, and the entire ultrasonic process was carried out under ice bath conditions. The solution was filtered, and the filter cake was washed with tert-butanol for 3 times, with tert-butanol used in an amount of 50 mL each time. After washing, the filter cake was dispersed in 100 mL of tert-butanol, and the tert-butanol dispersion of the coal dissociation product was cold-dried for 48 h to obtain the coal dissociation product.
[0069] (4) placing the coal dissociation product in a tubular furnace, and then heating it to 1200° C. at a rate of 5° C. / min under argon protection, and keeping the temperature for 3 hours to obtain the product coal-based graphene.
[0070] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing coal-based graphene with a few-layer structure, characterized in that: The steps include: (1) grinding the coal raw material and performing an acid washing treatment to obtain a cleaned coal raw material; (2) mixing the impurity-removed coal raw material with a swelling agent and heating and refluxing the mixture to make it swell, thereby obtaining a coal swelling product; (3) subjecting the coal swelling product to ultrasonic treatment to remove the solvent to obtain a coal dissociation product; (4) calcining the coal dissociation product to obtain coal-based graphene.
2. The method for preparing a few-layer structure coal-based graphene according to claim 1, characterized in that: In step (1), the coal raw material includes anthracite, lignite or bituminous coal, and is ground to a particle size of ≤74 μm.
3. The method for preparing a few-layer structure coal-based graphene according to claim 1, characterized in that: In step (1), the pickling treatment is carried out by using a hydrochloric acid aqueous solution and a hydrofluoric acid aqueous solution in sequence, the volume ratio of concentrated hydrochloric acid to water in the hydrochloric acid aqueous solution is 20-100:180-100, the volume ratio of hydrofluoric acid to water in the hydrofluoric acid aqueous solution is 20-100:180-100, and the volume ratio of the mass of the coal raw material to the hydrochloric acid aqueous solution or the hydrofluoric acid aqueous solution is 1-5 g:160-240 mL.
4. The method for preparing a few-layer structure coal-based graphene according to claim 1, characterized in that: In step (2), the swelling agent is N-methylpyrrolidone / carbon disulfide, pyridine / xylene, N,N-dimethylformamide / toluene, and the volume ratio of the front and rear components in the swelling agent is 40-60:60-40; the volume ratio of the mass of the impurity-removed coal raw material to the swelling agent is 0.1-0.5g:80-120mL.
5. The method for preparing a few-layer structure coal-based graphene according to claim 1, characterized in that: In step (2), the heating temperature of the reflux is 60 to 100° C., and the reflux reaction time is 12 to 36 hours.
6. The method for preparing a few-layer structure coal-based graphene according to claim 1, characterized in that: In step (3), ultrasonic treatment is carried out in an ice bath with an ultrasonic power of 20 to 25 kW and a duration of 3 to 10 h.
7. The method for preparing a few-layer structure coal-based graphene according to claim 1, characterized in that: In step (3), the product treated with ultrasound is filtered, washed and freeze-dried, and then the solvent is removed to obtain a coal dissociation product.
8. The method for preparing a few-layer structure coal-based graphene according to claim 1, characterized in that: In step (4), the heating rate of the calcination treatment is 5-10°C / min, the calcination temperature is 1000-1500°C, and the duration is 1-3h.
9. A few-layer structure coal-based graphene, characterized in that: The method is prepared according to any one of claims 1 to 8.
10. The coal-based graphene with few layers structure according to claim 9, characterized in that: It has an aromatic conjugated lamellar structure.
Citation Information
Patent Citations
Direct ultrasonication production of graphene sheets from coke or coal
CN109476490A
Coal-based nano porous carbon and preparation method thereof
CN112062127A
Method for preparing coal-based graphene and coal-based graphene quantum dot co-organism
CN114538428A
A preparation method of graphene as well as graphene oxide based on anthracite
US20160347617A1