Sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material with antiferroelectric-like characteristic and preparation method of sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material

By doping bismuth-containing complex ions Bi(Mg0.5Zr0.5)6+ in sodium bismuth titanate-based relaxation ferroelectric, the low energy storage density and efficiency loss of dielectric energy storage ceramic capacitors are solved. The problem of matching has achieved high release energy storage density and efficiency ceramic materials, suitable for environmentally friendly dielectric energy storage ceramic capacitors.

CN118894722AActive Publication Date: 2024-11-05UNIV OF ELECTRONICS SCI & TECH OF CHINA

Patent Information

Application Number
CN202410927305.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-05
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

The low energy storage density and mismatch of existing dielectric energy storage ceramic capacitors limit their application and development.

Method used

By doping bismuth-containing complex ion Bi(Mg0.5Zr0.5)6+ into the sodium bismuth titanate-based relaxation ferroelectric, the ceramic material structure is coordinated to achieve high releasable energy storage density and efficiency, specifically including in Na0. Bi(Mg0.5Zr0.5)6+ is introduced into 3Bi0.38Sr0.28TiO3 relaxation ferroelectric, to regulate grain size and structural disorder, enhance local random field, weaken the anisotropic field, and induce defect dipoles. Pinning domain wall effect improves insulation characteristics and breakdown electric field.

Benefits of technology

It realizes high releasable energy storage density and efficiency of ceramic materials, with energy storage density up to 2~5J/cm3 and energy storage efficiency up to 80~95%, and provides an environment with high energy storage density and efficiency Material selection for friendly dielectric energy storage ceramic capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894722A_ABST
    Figure CN118894722A_ABST
Patent Text Reader

Abstract

The invention discloses a sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material with antiferroelectric-like characteristics and a preparation method thereof, the ceramic material comprises the sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material with antiferroelectric-like characteristics represented by a general formula (1-x) (Na < 0.3 > Bi < 0.38 > Sr < 0.28 > TiO3)-xBi (Mg < 0.5 > Zr < 0.5 >) O3, and x is more than or equal to 0 and less than or equal to 0.2. The structure is regulated and controlled from multiple dimensions through a collaborative optimization strategy, the lead-free relaxor ferroelectric energy storage ceramic material with extremely low ferroelectric hysteresis loss and similar antiferroelectric characteristics is obtained, a ferroelectric hysteresis loop of the lead-free relaxor ferroelectric energy storage ceramic material is in a slender girdling shape, and the girdling degree is obviously increased along with increase of the content of Bi (Mg0. 5Zr0. 5) O3. Meanwhile, due to the increase of the content of Bi (Mg0. 5Zr0. 5) O3, the breakdown electric field of the ceramic material is greatly improved, polarization saturation is delayed, the energy storage performance of the ceramic material is greatly improved, and high energy storage density and efficiency can be achieved at the same time. According to the invention, the problems of low energy storage density and mismatch between the energy storage density and the efficiency of a dielectric material are solved to a certain extent, and a preparation method and material selection are provided for developing an environment-friendly dielectric energy storage ceramic capacitor with high energy storage density and efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electronic information functional materials and devices, and specifically relates to a sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material with antiferroelectric-like properties and a preparation method thereof. Background Art

[0002] Due to its ultra-high power density, ultra-fast charge and discharge speed, and excellent energy storage stability, dielectric energy storage ceramic capacitors have broad application prospects in military, civilian, and commercial fields, such as electromagnetic railguns, electromagnetic catapults, green intermittent energy storage, pulse power systems, power grid systems, hybrid electric vehicles, medical equipment, etc. However, the low energy storage density and the mismatch between energy storage density and efficiency severely restrict its application and development. For dielectric energy storage ceramic capacitors, the key to its energy storage performance lies in its underlying core material, namely the dielectric material (ceramic dielectric). In addition, in recent years, electronic components have been continuously developing towards lead-free, miniaturized, lightweight, and integrated directions. Therefore, the development of lead-free ceramic dielectrics with excellent performance and the fundamental solution to the above problems has become a research hotspot in the field of materials in recent years, which is of great practical and strategic significance.

[0003] Due to its large spontaneous polarization, strong dielectric relaxation characteristics, wide dielectric adjustability and stability, research on sodium bismuth titanate-based lead-free relaxor ferroelectrics has been booming in recent years. Research on sodium bismuth titanate-based lead-free relaxor ferroelectrics can be divided into two categories. One is conventional relaxor ferroelectrics, as reported in Ceramics International (DOI: 10.1016 / j.ceramint.2021.12.171) and Chinese patent "A sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material and its preparation method" (application number: CN202311067754.4); the other is relaxor ferroelectrics with antiferroelectric-like properties, as reported in Applied Physics Letters (DOI: 10.1063 / 1.4950974) and Journal of Materiomics (DOI: 10.1016 / j.jmat.2022.01.007). Compared with the former, the latter has more energy storage advantages due to its waisted hysteresis loop with antiferroelectric-like properties, and has the potential to become a key material for the development of ceramic capacitors with high energy storage density and efficiency. Although there have been reports on this type of sodium bismuth titanate-based lead-free relaxor ferroelectrics with antiferroelectric-like properties in recent years, such as "Rare Metals" (DOI: 10.1007 / s12598-022-02176-x) and "Small" (DOI: 10.1002 / smll.202302346), there are still few reports and technical achievements on this type of sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic materials with antiferroelectric-like properties and their preparation methods, which is far less than the research on conventional relaxor ferroelectrics, which means that there is much room for improvement in this type of research. Summary of the invention

[0004] The purpose of the present invention is to propose a sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material with antiferroelectric properties and a preparation method thereof in response to the problems existing in the background technology, and to achieve high releasable energy storage density and efficiency simultaneously through a collaborative optimization strategy to regulate the structure from multiple dimensions.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material with antiferroelectric properties, comprising a general formula (1-x) (Na 0.3 Bi 0.38 Sr 0.28 TiO3)-xBi(Mg 0.5 Zr 0.5)O3 (hereinafter abbreviated as: NBST-BMZ) represents a sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material with antiferroelectric-like properties, wherein the range of x is 0≤x≤0.2.

[0007] Preferably, in the ceramic material x=0.15.

[0008] The present invention uses Na 0.3 Bi 0.38 Sr 0.28 TiO3 relaxor ferroelectric is used as the matrix and doped with bismuth-containing complex ions Bi(Mg 0.5 Zr 0.5 ) 6+ Entering the matrix to achieve multi-dimensional coordinated optimization and regulation of the ceramic material structure, in order to achieve high releasable energy storage density and efficiency at the same time. The specific principles are as follows:

[0009] Bismuth-containing complex ions Bi(Mg 0.5 Zr 0.5 ) 6+ Doping and slightly excessive Bi2O3 and Na2CO3 during weighing can reduce the production of oxygen vacancies, reduce the oxygen vacancy concentration, inhibit high-temperature mass transfer, reduce grain size, increase the number of grain boundaries, and improve the breakdown electric field; due to the large band gap Mg 2+ and Zr 4+ The introduction also improves the insulation properties of NBST-BMZ ceramic materials and further increases the breakdown electric field.

[0010] Furthermore, due to the introduction of ions with different valence states and radii, the phase structure evolution is regulated and the multi-phase coexistence state is stabilized; lattice distortion and charge imbalance are caused, which enhances the structural disorder of NBST-BMZ ceramic materials, making the local random field stronger and the anisotropic field weaker. The enhancement of the local random field will destroy the long-range ordered structure of the ferroelectric, and promote the evolution of the ferroelectric macrodomain to the short-range ordered microdomain and / or polar nano-microregion; the weakening of the anisotropic field can flatten the free energy and reduce the free energy barrier between the phases.

[0011] Furthermore, due to the introduction of ions of various valence states and radii, the defect dipole pinning domain wall effect is induced, which increases the domain reversal field and provides a restoring force for the domain rotation, which is manifested as the hysteresis loop transforming to a waist type or antiferroelectric-like type accompanied by the occurrence of saturation polarization delay.

[0012] Furthermore, thanks to the synergistic effects of grains, band gaps, local random fields, anisotropic fields and defect dipoles, the insulation properties of NBST-BMZ ceramic materials are improved and the breakdown electric field is increased, the domain structure is refined and the inter-domain coupling is weakened, the phase structure evolution is regulated and the multi-phase coexistence state is stabilized, the domain reversal barrier is reduced and the domain response rate is accelerated, and the domain reversal and rotation (polarization expansion and recovery) are promoted; the relaxation characteristics are enhanced and the polarization saturation is delayed, and finally a sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material with antiferroelectric-like properties and high releasable energy storage density and efficiency is obtained.

[0013] Furthermore, in the present invention, the range of x is 0≤x≤0.2, within which the energy storage density of the NBST-BMZ ceramic material can reach 2 to 5 J / cm 3 , the energy storage efficiency can reach 80-95%; thanks to the above synergistic effect, x=0.15 is preferred, and the maximum releasable energy storage density of this component is 5J / cm 3 , the energy storage efficiency is 90%.

[0014] A method for preparing a sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material having antiferroelectric properties, comprising: 0.3 Bi 0.38 Sr 0.28 TiO3)-xBi(Mg 0.5 Zr 0.5 )O3 (hereinafter abbreviated as: NBST-BMZ) represented by a lead-free relaxor ferroelectric energy storage ceramic material based on bismuth titanate having antiferroelectric properties, wherein the range of x is 0≤x≤0.2, and the preparation method of the ceramic material comprises the following steps:

[0015] S1: Select Na2CO3, Bi2O3, Sr2CO3, TiO2, MgO, ZrO2 with a purity of not less than 98% as raw materials, and follow the general composition formula (1-x) (Na 0.3 Bi 0.38 Sr 0.28 TiO3)-xBi(Mg 0.5 Zr 0.5 )O3 in a stoichiometric ratio, and NBST-BMZ ceramic powder is obtained through ball milling, pre-sintering and crushing.

[0016] S2: uniformly mixing the NBST-BMZ ceramic powder obtained in step S1 with a solvent, a dispersant, a binder, and a defoaming agent to obtain a NBST-BMZ ceramic slurry, preparing a NBST-BMZ thick film by a tape casting process, and preparing a NBST-BMZ ceramic green body by a laminated hot pressing process;

[0017] S3: Debinding and sintering the NBST-BMZ ceramic green body obtained in step S2 to obtain NBST-BMZ ceramics with antiferroelectric-like properties.

[0018] Furthermore, the Na2CO3 and Bi2O3 weighed in step S1 are slightly excessive by 1 to 5%.

[0019] Further, step S1 is specifically as follows:

[0020] S101: placing the raw material powder in step S1 in an oven and drying at 80-100° C. for 1-2 hours;

[0021] S102: Weigh the dried raw material powder according to the stoichiometric ratio in the general formula and place it in a grinding jar, add grinding media according to the mass ratio of powder: zirconium ball: anhydrous ethanol = 1: (1-5): (1-3), mix in a ball mill at a speed of 200-300 rpm for 6-18 hours to obtain a uniform slurry;

[0022] S103: Separate the slurry and zirconium balls in step S102 and place them in an oven to dry at 80-120°C for 3-6 hours until dry, then place them in a muffle furnace at 800-950°C for 2-6 hours after being screened with a 60-120 mesh screen to complete pre-sintering treatment, with a heating rate of 2-5°C / min and a cooling rate of natural cooling with the furnace;

[0023] S104: Grind and crush the pre-calcined powder obtained in step S103, and then perform secondary ball milling, drying and sieving according to the processes in steps S102 to S103 to obtain NBST-BMZ ceramic powder.

[0024] Preferably, the solvent in step S2 is one or more of toluene, xylene, ethyl acetate, ethanol, and butanone, and its content is 70-150% of the mass of the ceramic powder; the dispersant is one or more of tributyl phosphate, triolein, and castor oil, and its content is 1-5% of the mass of the ceramic powder; the binder is polyvinyl butyral, and its content is 6-14% of the mass of the ceramic powder; the plasticizer is one or more of butyl benzyl phthalate, dibutyl phthalate, and polyethylene glycol, and its content is 3-8% of the mass of the ceramic powder; the defoamer is one or more of dimethyl silicone oil and defoamer 716, and its content is 0-1% of the mass of the ceramic powder.

[0025] Further, step S2 is specifically as follows:

[0026] S201: Preliminarily mix the NBST-BMZ ceramic powder obtained in step S1 with a solvent and a dispersant by ball milling dispersion process, wherein the dispersion medium is zirconium balls, the slurry: zirconium balls = 1: (1-3), the dispersion time is 4-12 hours, and the dispersion speed is 100-250 rpm;

[0027] S202: Add a binder, a plasticizer and a defoamer to the primary slurry obtained in step S201 and

[0028] Continue ball milling at the parameters described above to mix well.

[0029] S203: placing the uniform slurry obtained in step S202 in a degassing device for vacuum stirring and degassing for 5 to 30 minutes;

[0030] S204: the degassed slurry is sealed and placed in a room temperature environment for 20 to 60 minutes for homogenization and temperature recovery treatment, and then the slurry is evenly coated on a PET base tape by a casting machine or a coating machine and dried to obtain a NBST-BMZ thick film;

[0031] S205: The NBST-BMZ thick film is cut into required sizes and stacked, and then a ceramic green body is obtained by a multi-stage hot pressing process.

[0032] Preferably, the multi-stage hot pressing process in steps S2 and S205 is as follows: the hot pressing temperature is 50-80°C, the hot pressing pressure in the first stage is 10Mpa, the hot pressing pressure in the second stage is 20Mpa, the hot pressing pressure in the third stage is 30Mpa, the single-stage heat preservation and pressure holding time is 5-20min, and the hot pressing is naturally cooled to room temperature after the hot pressing is completed.

[0033] Further, step S3 is specifically as follows:

[0034] S301: placing the NBST-BMZ ceramic green body obtained in step S2 directly on the zirconium plate and performing debinding in a low-temperature muffle furnace by adopting a multi-stage temperature rise and fall process;

[0035] S302: placing the NBST-BMZ ceramic body after debinding in step S301 in a sealed alumina or zirconia crucible and sintering it in a high-temperature muffle furnace using a multi-stage temperature rise and fall process.

[0036] Preferably, the multi-stage debinding process of heating and cooling described in steps S3 and S301 is as follows: in the first stage of the debinding process, the temperature is raised from room temperature to 180-200°C at a heating rate of 0.5-3°C / min and kept warm for 60-120min; in the second stage of the debinding process, the temperature is further raised from 180-200°C to 500-600°C at a heating rate of 0.5-1.5°C / min and kept warm for 300-480min; in the third stage of the debinding process, the temperature is reduced from 500-600°C to 200-300°C at a cooling rate of 1-2°C / min, and then cooled to room temperature with the furnace.

[0037] Preferably, the multi-stage temperature rise and fall sintering process described in steps S3 and S302 is: the first stage sintering process is to heat the temperature from room temperature to 800-950°C at a heating rate of 5-8°C / min and keep it for 0 min; the second stage is to heat the temperature from 800-950°C to 1100-1180°C at a heating rate of 2-5°C / min and keep it for 1-5h; the third stage is to cool the temperature from 1100-1180°C to 800-950°C at a cooling rate of 3-6°C / min, and then naturally cool to room temperature with the furnace.

[0038] Through the above technical solution, the present invention achieves the following beneficial effects:

[0039] 1. The chemical formula proposed by the present invention is (1-x)(Na 0.3 Bi 0.38 Sr 0.28 TiO3)-xBi(Mg 0.5 Zr 0.5 )O3, wherein 0≤x≤0.2, has obvious antiferroelectric properties and exhibits a thin waisted hysteresis loop with both high saturation polarization and extremely low remnant polarization; with the addition of bismuth complex ions Bi(Mg 0.5 Zr 0.5 ) 6+ With the increase of doping content, the waist of the hysteresis loop increases and presents a double hysteresis loop similar to that of antiferroelectrics.

[0040] 2. The present invention comprises bismuth-containing complex ions Bi(Mg 0.5 Zr 0.5 ) 6+ Doping refines the ceramic grains and increases the band gap, effectively improving the breakdown electric field.

[0041] 3. The present invention provides 0.3 Bi 0.38 Sr 0.28 TiO3 relaxor ferroelectric matrix doped with Bi(Mg 0.5 Zr 0.5 ) 6+, introducing a variety of ions with different valence states and radii, enhanced the local random field, weakened the anisotropic field and induced the defect dipole pinning domain wall effect, enhanced the relaxation characteristics and delayed the polarization saturation, and promoted the transformation of the waist-type hysteresis loop to the antiferroelectric-like double hysteresis loop.

[0042] 4. The present invention uses a collaborative optimization strategy to perform multi-dimensional regulation on the structure of the ceramic material, ultimately achieving high releasable energy storage density and efficiency at the same time, solving the problem of low energy storage density of dielectric materials and mismatch between energy storage density and efficiency to a certain extent, and providing a preparation method and material selection for the development of environmentally friendly dielectric energy storage ceramic capacitors with high energy storage density and efficiency. The energy storage density of the ceramic material can reach 2 to 5 J / cm 3 , the energy storage efficiency can reach 80-95%; preferably x = 0.15, the maximum releasable energy storage density of this component is 5J / cm 3 , the energy storage efficiency is 90%.

[0043] 5. The preparation process of the sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material described in the present invention adopts a multi-stage hot pressing process, which can reduce interlayer gas residue, reduce film material delamination, cracking and flow during hot pressing, and improve material uniformity and density to a certain extent.

[0044] 6. The preparation process of the sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material described in the present invention adopts a multi-stage debinding and sintering process, which can effectively remove organic substances such as binders to improve the density of ceramics and avoid deformation and / or cracking of the ceramic green body during high-temperature treatment.

[0045] 7. The sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material with antiferroelectric-like properties provided by the present invention does not contain toxic metals such as lead, is friendly to the environment and humans, and can be widely used in various energy storage components. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 The hysteresis loop diagram of the ceramic material prepared in Examples 1 to 4 of the present invention under the breakdown electric field;

[0047] Figure 2 This is a diagram showing the energy storage performance of the ceramic materials prepared in Examples 1 to 4 of the present invention under a breakdown electric field. DETAILED DESCRIPTION

[0048] The specific implementation of the present invention is described in detail below in conjunction with the examples. It should be understood that the specific implementation described herein is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0049] Example 1

[0050] (1) According to the chemical formula Na0.3 Bi 0.38 Sr 0.28 The dried raw material powder is weighed and placed in a ball mill according to the stoichiometric ratio of TiO3 and a slightly excessive ratio of 3% of Na2CO3 and Bi2O3, and the grinding medium is added in a mass ratio of powder: zirconium ball: anhydrous ethanol = 1:4:2, and the mixture is mixed in a ball mill at a speed of 240 rpm for 12 hours to obtain a uniform slurry; the slurry is then placed in an oven at 90°C for 5 hours, and then ground and sieved through a 60-mesh screen to obtain a primary mixed powder; the primary mixed powder is placed in The pre-sintering treatment is carried out in a muffle furnace, the heating rate is 3℃ / min, the holding temperature is 950℃, the holding time is 2h, and the cooling process is cooling with the furnace; the pre-sintered powder is then obtained by crushing, grinding and passing through a 100-mesh sieve; the pre-sintered powder and the grinding medium are subjected to secondary ball milling according to the mass ratio of powder: zirconium ball: anhydrous ethanol = 1:4:2, the speed is 240rpm, and the time is 18h; the slurry after the secondary ball milling is dried, ground and sieved according to the above-mentioned process to obtain Na 0.3 Bi 0.38 Sr 0.28 TiO3 ceramic powder.

[0051] (2) 30 g of Na 0.3 Bi 0.38 Sr 0.28 TiO3 ceramic powder is ball-milled with 20g xylene, 20g anhydrous ethanol and 1.5g triolein, wherein the slurry: zirconium ball = 1:3, the dispersion time is 12h, and the dispersion speed is 200rpm; then 3g polyvinyl butyral, 3g dibutyl phthalate and 0.5g defoamer 716 are added and mixed for 12h to obtain a casting slurry; then the slurry is subjected to vacuum stirring degassing and homogenization and temperature return treatment for a total of 40 to 60min; the slurry is evenly coated on the PET base tape by a casting machine or a coating machine and dried to obtain a thick film; then the Na 0.3 Bi 0.38 Sr 0.28 The TiO3 ceramic green body has a hot pressing temperature of 50-80°C, a first-stage hot pressing pressure of 10 MPa, a second-stage hot pressing pressure of 20 MPa, and a third-stage hot pressing pressure of 30 MPa. The single-stage heat preservation and pressure holding time is 5-20 minutes, and the product is naturally cooled to room temperature after the hot pressing is completed.

[0052] (3) Put Na 0.3 Bi 0.38 Sr 0.28The TiO3 ceramic green body is placed on a zirconium plate and debinded by a multi-stage heating and cooling process in a low-temperature muffle furnace. In the first stage of the debinding process, the temperature is raised from room temperature to 180°C at a heating rate of 2°C / min and kept at this temperature for 120 minutes. In the second stage of the debinding process, the temperature is further raised from 180°C to 500°C at a heating rate of 1°C / min and kept at this temperature for 480 minutes. In the third stage of the debinding process, the temperature is lowered from 500°C to 200°C at a cooling rate of 2°C / min, and then cooled to room temperature with the furnace. The debinding ceramic body is placed in a sealed alumina crucible and sintered in a high-temperature muffle furnace using a multi-stage heating and cooling process, wherein the first stage of the sintering process is to heat the temperature from room temperature to 800°C at a heating rate of 8°C / min and keep it for 0 min; the second stage is to heat the temperature from 900°C to 1160°C at a heating rate of 4°C / min and keep it for 3h; the third stage is to cool the temperature from 1160°C to 900°C at a cooling rate of 6°C / min, and then naturally cool it to room temperature in the furnace to obtain the Na2O3 with antiferroelectric properties. 0.3 Bi 0.38 Sr 0.28 TiO3 lead-free relaxor ferroelectric energy storage ceramic material.

[0053] Example 2

[0054] (1) According to the chemical formula 0.95(Na 0.3 Bi 0.38 Sr 0.28 TiO3)-0.05Bi(Mg 0.5 Zr 0.5 )O3 and a slightly excessive 2% ratio of Na2CO3 and Bi2O3. The dried raw material powder is weighed and placed in a ball mill, and grinding media is added according to the mass ratio of powder: zirconium ball: anhydrous ethanol = 1:4:3. The mixture is mixed in a ball mill at a speed of 280 rpm for 8 hours to obtain a uniform slurry; the slurry is then placed in an oven and dried at 110°C for 3 hours; the mixed powder obtained by drying, grinding and passing through a 60-mesh screen is placed in a muffle furnace for pre-sintering treatment, with a heating rate of 3°C / min, a holding temperature of 900°C, and a holding time of 3 hours. After cooling with the furnace, the pre-sintered powder is taken out after crushing, grinding and passing through a 120-mesh screen. The pre-sintered powder and the grinding media are subjected to secondary ball milling according to the mass ratio of powder: zirconium ball: anhydrous ethanol = 1:4:3, at a speed of 280 rpm and a time of 12 hours; the slurry after the secondary ball milling is treated according to the aforementioned drying, grinding and screening process to obtain 0.95 (Na 0.3 Bi 0.38 Sr 0.28 TiO3)-0.05Bi(Mg 0.5 Zr 0.5 )O3 ceramic powder.

[0055] (2) Add 30 g of 0.95 (Na 0.3 Bi 0.38 Sr 0.28 TiO3)-0.05Bi(Mg 0.5 Zr 0.5 )O3 ceramic powder is ball-milled with 15g toluene, 15g anhydrous ethanol and 1.2g tributyl phosphate, wherein the slurry: zirconium ball = 1:5, the dispersion time is 6h, and the dispersion speed is 280rpm; then 2.7g polyvinyl butyral, 1.5g dibutyl phthalate, 1.5g polyethylene glycol and 0.5g methyl silicone oil are added and mixed for 10h to obtain a casting slurry; then the slurry is vacuum stirred for degassing and homogenized and warmed for a total of 30 to 40min; the slurry is evenly coated on the PET base tape by a casting machine or a coating machine and dried to obtain a thick film; and then 0.95 (Na 0.3 Bi 0.38 Sr 0.28 TiO3)-0.05Bi(Mg 0.5 Zr 0.5 )O3 ceramic green body, wherein the hot pressing temperature is 50-80°C, the first stage hot pressing pressure is 10Mpa, the second stage hot pressing pressure is 20Mpa, the third stage hot pressing pressure is 30Mpa, the single stage heat preservation and pressure holding time is 5-20min, and it is naturally cooled to room temperature after the hot pressing is completed.

[0056] (3) Change 0.95(Na 0.3 Bi 0.38 Sr 0.28 TiO3)-0.05Bi(Mg 0.5 Zr 0.5 )O3 ceramic green body is placed on the zirconium plate and debinded by multi-stage heating and cooling process in a low-temperature muffle furnace. In the first debinding process, the temperature is raised from room temperature to 200℃ at a heating rate of 1℃ / min and kept at this temperature for 90min. In the second debinding process, the temperature is further raised from 200℃ to 600℃ at a heating rate of 1℃ / min and kept at this temperature for 300min. In the third debinding process, the temperature is lowered from 600℃ to 300℃ at a cooling rate of 2℃ / min, and then cooled to room temperature with the furnace. After that, the ceramic green body after debinding is placed on the zirconium plate and debinded by multi-stage heating and cooling process in a low-temperature muffle furnace. The ceramic body is placed in a sealed alumina crucible and sintered in a high-temperature muffle furnace using a multi-stage heating and cooling process, wherein the first stage of the sintering process is to heat the temperature from room temperature to 800°C at a heating rate of 6°C / min and keep it for 0 min; the second stage is to heat the temperature from 900°C to 1150°C at a heating rate of 3°C / min and keep it for 2.5 h; the third stage is to cool the temperature from 1160°C to 900°C at a cooling rate of 5°C / min, and then naturally cool it to room temperature in the furnace to obtain the 0.95 (Na2O3) with antiferroelectric properties. 0.3 Bi 0.38 Sr0.28 TiO3)-0.05Bi(Mg 0.5 Zr 0.5 )O3 lead-free relaxor ferroelectric energy storage ceramic material.

[0057] Example 3

[0058] (1) According to the chemical formula 0.85(Na 0.3 Bi 0.38 Sr 0.28 TiO3)-0.15Bi(Mg 0.5 Zr 0.5 )O3 in a stoichiometric ratio and a slightly excessive 1.5% of Na2CO3 and a slightly excessive 3% of Bi2O3, the raw material powder after drying is weighed and placed in a ball mill, and grinding media is added in a mass ratio of powder: zirconium ball: anhydrous ethanol = 1:3:2, and the mixture is mixed in a ball mill at a speed of 260 rpm for 10 hours to obtain a uniform slurry; then the slurry is placed in an oven at 100°C for 4 hours; the mixed powder obtained by drying, grinding and passing through a 60-mesh screen is placed The pre-sintering treatment was carried out in a muffle furnace, with a heating rate of 5°C / min, a holding temperature of 880°C, and a holding time of 4h. After cooling with the furnace, the pre-sintered powder was taken out and crushed, ground, and passed through a 100-mesh sieve to obtain the pre-sintered powder; the pre-sintered powder and the grinding medium were subjected to secondary ball milling according to the mass ratio of powder: zirconium ball: anhydrous ethanol = 1:3:2, with a rotation speed of 300rpm and a time of 12h; the slurry after the secondary ball milling was treated according to the aforementioned drying, grinding, and screening process to obtain 0.85 (Na 0.3 Bi 0.38 Sr 0.28 TiO3)-0.15Bi(Mg 0.5 Zr 0.5 )O3 ceramic powder.

[0059] (2) Add 30 g of 0.85 (Na 0.3 Bi 0.38 Sr 0.28 TiO3)-0.15Bi(Mg 0.5 Zr 0.5 )O3 ceramic powder is ball-milled with 10g toluene, 20g anhydrous ethanol and 1.5g tributyl phosphate, wherein the slurry: zirconium ball = 1:4, the dispersion time is 8h, and the dispersion speed is 240rpm; then 2.85g polyvinyl butyral, 1.8g dibutyl phthalate, 1.8g polyethylene glycol and 0.3g defoamer 716 are added and mixed evenly to obtain a casting slurry; then the slurry is subjected to vacuum stirring degassing and homogenization and temperature return treatment for a total of 15 to 30min; the slurry is evenly coated on the PET base tape by a casting machine or a coating machine and dried to obtain a thick film; and then 0.95 (Na0.3 Bi 0.38 Sr 0.28 TiO3)-0.05Bi(Mg 0.5 Zr 0.5 )O3 ceramic green body, wherein the hot pressing temperature is 50-80°C, the first stage hot pressing pressure is 10Mpa, the second stage hot pressing pressure is 20Mpa, the third stage hot pressing pressure is 30Mpa, the single stage heat preservation and pressure holding time is 5-20min, and it is naturally cooled to room temperature after the hot pressing is completed.

[0060] (3) Change 0.85(Na 0.3 Bi 0.38 Sr 0.28 TiO3)-0.15Bi(Mg 0.5 Zr 0.5 )O3 ceramic green body is placed on the zirconium plate and debinded by multi-stage heating and cooling process in a low-temperature muffle furnace. In the first stage of debinding process, the temperature is raised from room temperature to 200℃ at a heating rate of 1℃ / min and kept at this temperature for 90min. In the second stage of debinding process, the temperature is further raised from 200℃ to 550℃ at a heating rate of 0.5℃ / min and kept at this temperature for 420min. In the third stage of debinding process, the temperature is lowered from 550℃ to 300℃ at a cooling rate of 2℃ / min, and then cooled to room temperature with the furnace. The ceramic body is placed in a sealed alumina crucible and sintered in a high-temperature muffle furnace using a multi-stage heating and cooling process, wherein the first stage of the sintering process is to heat the temperature from room temperature to 800°C at a heating rate of 6°C / min and keep it for 0 min; the second stage is to heat the temperature from 900°C to 1135°C at a heating rate of 3°C / min and keep it for 3h; the third stage is to cool the temperature from 1135°C to 900°C at a cooling rate of 5°C / min, and then naturally cool it to room temperature in the furnace to obtain the 0.85 (Na2O3) having antiferroelectric properties. 0.3 Bi 0.38 Sr 0.28 TiO3)-0.15Bi(Mg 0.5 Zr 0.5 )O3 lead-free relaxor ferroelectric energy storage ceramic material.

[0061] Example 4

[0062] (1) According to the chemical formula 0.80(Na 0.3 Bi 0.38 Sr 0.28 TiO3)-0.20Bi(Mg 0.5 Zr 0.5)O3 and a slightly excessive 2% of Na2CO3 and a slightly excessive 3% of Bi2O3, the raw material powder after drying is weighed and placed in a ball mill, and grinding media is added in a mass ratio of powder: zirconium ball: anhydrous ethanol = 1:3:2, and the mixture is mixed in a ball mill at a speed of 280 rpm for 10 hours to obtain a uniform slurry; then the slurry is placed in an oven at 115°C for 3 hours; the mixed powder obtained by drying, grinding and passing through a 60-mesh screen is placed The pre-sintering treatment was carried out in a muffle furnace, with a heating rate of 5°C / min, a holding temperature of 850°C, and a holding time of 5h. After cooling with the furnace, the pre-sintered powder was taken out and crushed, ground, and passed through a 100-mesh sieve to obtain the pre-sintered powder; the pre-sintered powder and the grinding medium were subjected to secondary ball milling according to the mass ratio of powder: zirconium ball: anhydrous ethanol = 1:3:2, with a rotation speed of 300rpm and a time of 10h; the slurry after the secondary ball milling was treated according to the aforementioned drying, grinding, and screening process to obtain 0.80 (Na 0.3 Bi 0.38 Sr 0.28 TiO3)-0.20Bi(Mg 0.5 Zr 0.5 )O3 ceramic powder.

[0063] (2) Add 30 g of 0.80 (Na 0.3 Bi 0.38 Sr 0.28 TiO3)-0.20Bi(Mg 0.5 Zr 0.5 )O3 ceramic powder is ball-milled with 18xylene, 12g anhydrous ethanol, and 1.2g triolein, wherein the slurry: zirconium ball = 1:4, the dispersion time is 8h, and the dispersion speed is 240rpm; then 2.85g polyvinyl butyral, 1.5g dibutyl phthalate, 1.5g polyethylene glycol, and 0.3g defoamer 716 are added and continued to be mixed evenly to obtain a casting slurry; then the slurry is subjected to vacuum stirring degassing and homogenization and temperature return treatment for a total of 15 to 30min; the slurry is evenly coated on the PET base tape by a casting machine or a coating machine and dried to obtain a thick film; and then 0.80 (Na 0.3 Bi 0.38 Sr 0.28 TiO3)-0.20Bi(Mg 0.5 Zr 0.5 )O3 ceramic green body, wherein the hot pressing temperature is 50-80°C, the first stage hot pressing pressure is 10Mpa, the second stage hot pressing pressure is 20Mpa, the third stage hot pressing pressure is 30Mpa, the single stage heat preservation and pressure holding time is 5-20min, and it is naturally cooled to room temperature after the hot pressing is completed.

[0064] (3) Change 0.80(Na 0.3 Bi0.38 Sr 0.28 TiO3)-0.20Bi(Mg 0.5 Zr 0.5 )O3 ceramic green body is placed on the zirconium plate and debinded by multi-stage heating and cooling process in a low-temperature muffle furnace, wherein the first debinding process increases the temperature from room temperature to 200°C at a heating rate of 0.5°C / min and keeps it warm for 90min, the second debinding process increases the temperature from 200°C to 550°C at a heating rate of 0.5°C / min and keeps it warm for 420min, the third debinding process decreases the temperature from 550°C to 300°C at a cooling rate of 2°C / min, and then cools to room temperature with the furnace; then the debinding The ceramic body is placed in a sealed alumina crucible and sintered in a high-temperature muffle furnace using a multi-stage heating and cooling process, wherein the first stage of the sintering process is to heat the temperature from room temperature to 800°C at a heating rate of 8°C / min and keep it for 0 min; the second stage is to heat the temperature from 900°C to 1120°C at a heating rate of 3°C / min and keep it for 2 h; the third stage is to cool the temperature from 1120°C to 900°C at a cooling rate of 5°C / min, and then naturally cool to room temperature in the furnace to obtain the 0.80 (Na2O3) with antiferroelectric properties. 0.3 Bi 0.38 Sr 0.28 TiO3)-0.20Bi(Mg 0.5 Zr 0.5 )O3 lead-free relaxor ferroelectric energy storage ceramic material.

[0065] The energy storage performance of the lead-free relaxor ferroelectric ceramics prepared in the above examples was analyzed, and the results are as follows: Figures 1-2 shown.

[0066] Ginseng Figure 1 , that is, the hysteresis loop diagram of the NBST-BMZ ceramic materials prepared in Examples 1 to 4 under the breakdown electric field, it can be found that: the ceramic materials prepared in each embodiment show extremely low hysteresis loss and antiferroelectric-like properties, and their hysteresis loops are slender waisted and increase with the Bi(Mg 0.5 Zr 0.5 )O3 content increases significantly. 0.5 Zr 0.5 The increase in O3 content greatly increases the breakdown electric field and delays polarization saturation, which is beneficial to the improvement of energy storage performance. When x = 0.15, corresponding to the ceramic material described in Example 3, its breakdown electric field can reach 340 kV / cm, and the maximum polarization obtained after delay can reach 42 μC / cm 2 , the difference between the maximum polarization and the residual polarization can reach ~41μC / cm 2 , laying the foundation for achieving high releasable energy storage density and efficiency at the same time.

[0067] Ginseng Figure 2 , that is, the energy storage performance diagram of the NBST-BMZ ceramic materials prepared in Examples 1 to 4 under the breakdown electric field. By comparison, it can be found that: Bi(Mg 0.5 Zr 0.5 The increase in O3 content greatly improves the energy storage performance of the ceramic material in the embodiment. The best energy storage performance is obtained when x=0.15, corresponding to the ceramic material in Example 3, whose releasable energy storage density is as high as 5J / cm 3 The invention solves the problem of low energy storage density of dielectric materials and mismatch between energy storage density and efficiency to a certain extent, and provides a preparation method and material selection for developing environmentally friendly dielectric energy storage ceramic capacitors with high energy storage density and efficiency.

[0068] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material with antiferroelectric-like properties, characterized in that: The general composition formula of the ceramic material is: (1-x)(Na 0.3 Bi 0.38 Sr 0.28 TiO3)-xBi(Mg 0.5 Zr 0.5 )O3 (hereinafter abbreviated as: NBST-BMZ), where 0≤x≤0.

2.

2. A sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material with antiferroelectric-like properties as claimed in claim 1, characterized in that: The range of x in the above material composition formula is 0≤x≤0.2, wherein x=0.15 is preferred.

3. A method for preparing the sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material with antiferroelectric-like properties as claimed in claim 1, characterized in that: The steps include: S1: Selecting Na2CO3, Bi2O3, Sr2CO3, TiO2, MgO, and ZrO2 with a purity of not less than 98% as raw materials, and weighing them according to the stoichiometric ratio in the general composition formula described in claim 1, and preparing NBST-BMZ ceramic powder through ball milling, pre-sintering, and crushing; S2: uniformly mixing the NBST-BMZ ceramic powder obtained in step S1 with a solvent, a dispersant, a binder, and a defoaming agent to obtain a NBST-BMZ ceramic slurry, preparing a NBST-BMZ thick film by a tape casting process, and preparing a NBST-BMZ ceramic green body by a laminated hot pressing process; S3: Debinding and sintering the NBST-BMZ ceramic green body obtained in step S2 to obtain NBST-BMZ ceramics with antiferroelectric-like properties.

4. The preparation method according to claim 3, characterized in that: The Na2CO3 and Bi2O3 weighed in step S1 are slightly excessive by 1 to 5%.

5. The preparation method according to claim 3, characterized in that: Step S1 is specifically as follows: S101: placing the raw material powder in step S1 in an oven and drying at 80-100° C. for 1-2 hours; S102: according to the stoichiometric ratios described in claims 1 and 4, the dried raw material powders are weighed and placed in a grinding jar, grinding media are added in a mass ratio of powder: zirconium ball: anhydrous ethanol = 1: (1-5): (1-3), and the mixture is mixed in a ball mill at a speed of 200-300 rpm for 6-18 hours to obtain a uniform slurry; S103: Separate the slurry and zirconium balls in step S102 and place them in an oven to dry at 80-120°C for 3-6 hours until dry, then place them in a muffle furnace at 800-950°C for 2-6 hours after being screened with a 60-120 mesh screen to complete pre-sintering treatment, with a heating rate of 2-5°C / min and a cooling rate of natural cooling with the furnace; S104: Grind and crush the pre-calcined powder obtained in step S103, and then perform secondary ball milling, drying and sieving according to the processes in steps S102 to S103 to obtain NBST-BMZ ceramic powder.

6. The preparation method according to claim 3, characterized in that: The solvent in step S2 is one or more of toluene, xylene, ethyl acetate, ethanol, and butanone, and its content is 70-150% of the mass of the ceramic powder; the dispersant is one or more of tributyl phosphate, triolein, and castor oil, and its content is 1-5% of the mass of the ceramic powder; the binder is polyvinyl butyral, and its content is 5-15% of the mass of the ceramic powder; the plasticizer is one or more of butyl benzyl phthalate, dibutyl phthalate, and polyethylene glycol, and its content is 2-8% of the mass of the ceramic powder; the defoamer is one or more of dimethyl silicone oil and defoamer 716, and its content is 0-1% of the mass of the ceramic powder.

7. The preparation method according to claim 3, characterized in that: Step S2 is specifically as follows: S201: Preliminarily mix the NBST-BMZ ceramic powder obtained in step S1 with a solvent and a dispersant by ball milling dispersion process, wherein the dispersion medium is zirconium balls, the slurry: zirconium balls = 1: (1-3), the dispersion time is 4-12 hours, and the dispersion speed is 100-250 rpm; S202: Add a binder, a plasticizer and a defoamer to the primary slurry obtained in step S201 and Continue ball milling at the parameters described above to mix well. S203: placing the uniform slurry obtained in step S202 in a degassing device for vacuum stirring and degassing for 5 to 30 minutes; S204: the degassed slurry is sealed and placed in a room temperature environment for 20 to 60 minutes for homogenization and temperature recovery treatment, and then the slurry is evenly coated on a PET base tape by a casting machine or a coating machine and dried to obtain a NBST-BMZ thick film; S205: The NBST-BMZ thick film is cut into required sizes and stacked, and then a ceramic green body is obtained by a multi-stage hot pressing process.

8. The preparation method according to claims 3 and 7, characterized in that: The multi-stage hot pressing process described in steps S2 and S205 is as follows: the hot pressing temperature is 50-80°C, the hot pressing pressure in the first stage is 10Mpa, the hot pressing pressure in the second stage is 20Mpa, the hot pressing pressure in the third stage is 30Mpa, the single-stage heat preservation and pressure holding time is 5-20min, and the hot pressing is naturally cooled to room temperature after the hot pressing is completed.

9. The preparation method according to claim 3, characterized in that: Step S3 is as follows: S301: placing the NBST-BMZ ceramic green body obtained in step S2 directly on the zirconium plate and performing debinding in a low-temperature muffle furnace by adopting a multi-stage temperature rise and fall process; S302: placing the NBST-BMZ ceramic body after debinding in step S301 in a sealed alumina or zirconia crucible and sintering it in a high-temperature muffle furnace using a multi-stage temperature rise and fall process.

10. The preparation method according to claims 3 and 9, characterized in that: The multi-stage debinding process of heating and cooling described in steps S3 and S301 is as follows: in the first stage of the debinding process, the temperature is raised from room temperature to 180-200°C at a heating rate of 0.5-3°C / min and kept at this temperature for 60-120min; in the second stage of the debinding process, the temperature is further raised from 180-200°C to 500-600°C at a heating rate of 0.5-1.5°C / min and kept at this temperature for 300-480min; in the third stage of the debinding process, the temperature is lowered from 500-600°C to 200-300°C at a cooling rate of 1-2°C / min, and then cooled to room temperature with the furnace.

11. The preparation method according to claims 3 and 9, characterized in that: The multi-stage temperature rise and fall sintering process described in steps S3 and S302 is: the first stage sintering process is to heat up from room temperature to 800-950°C at a heating rate of 5-8°C / min and keep warm for 0 min; the second stage is to heat up from 800-950°C to 1100-1180°C at a heating rate of 2-5°C / min and keep warm for 1-5h; the third stage is to cool from 1100-1180°C to 800-950°C at a cooling rate of 3-6°C / min, and then naturally cool to room temperature with the furnace.

Citation Information

Patent Citations

  • Sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material and preparation method thereof

    CN116986900A

  • Sodium bismuth titanate and strontium titanate-based energy storage ceramic material and preparation method thereof

    CN111393161A

  • High-energy-storage-density barium strontium titanate-sodium bismuth titanate-based glass ceramic composite ceramic material and preparation method thereof

    CN114180958A

  • High-temperature-stability sodium bismuth titanate-based dielectric energy storage ceramic material and preparation method thereof

    CN114520114A

  • Sodium bismuth titanate-based relaxor ferroelectric ceramic material with wide temperature range and high electrocaloric effect as well as preparation method and application of sodium bismuth titanate-based relaxor ferroelectric ceramic material

    CN116813335A

Cited By

  • A sodium bismuth titanate-based lead-free relaxor ferroelectric energy storage ceramic material with antiferroelectric-like properties and a preparation method thereof

    CN118894722B

  • Nd and Mn co-doped sodium bismuth titanate based ferroelectric film and preparation method and application thereof

    CN119430916A