Antiskid ceramic tile and preparation process thereof

Through the interfacial polymerization of polyethyleneimine or polyvinyl alcohol and aromatic dianhydride, a micron-scale raised structure and a cilia structure are formed, which solves the problem of poor anti-slip effect and ageability of existing anti-slip tiles in humid environments, and achieves better results Anti-slip performance and longer timeliness.

CN118894735AActive Publication Date: 2024-11-05QINGYUAN GANI CERAMICS CO LTD +2
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410948364.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-05
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

The existing anti-slip tiles have poor anti-slip effect and age-effectiveness in humid environments, and commonly used anti-slip coating materials such as epoxy resin and silicone resin have durability and cost problems.

Method used

Polyethyleneimine or polyvinyl alcohol and aromatic dianhydride are used to polymerize interfacially to form a micron-scale convex structure, and combine with modifiers such as maleic anhydride, phthalic anhydride, and biphenyl dianhydride to lift the surface in a humid environment through hydrolysis reaction. Roughness forms a cilia-like structure, improves anti-slip performance, and has self-restoration ability.

Benefits of technology

It has achieved a significant improvement in anti-slip effect in humid environments and extended aging. The anti-slip tiles have better anti-slip performance in humid environments and have longer aging compared to conventional coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894735A_ABST
    Figure CN118894735A_ABST
Patent Text Reader

Abstract

The invention provides a preparation process of an anti-skid ceramic tile, which comprises the following steps: S1, applying a liquid A on the surface of a finished ceramic tile to form a water film on the surface of the ceramic tile; s2, spraying a liquid B on the surface of the ceramic tile treated in the step S1; and S3, baking the finished ceramic tile obtained in the step S2, taking out the finished ceramic tile, cleaning the surface with water, and draining water to obtain the anti-skid ceramic tile. The liquid A comprises a primer and water, and the primer is one of polyethyleneimine or polyvinyl alcohol; the liquid B comprises a modifier and diethyl ether, and the modifier is one or more of maleic anhydride, phthalic anhydride, biphenyl dianhydride and 4, 4 '-diphenyl ether dianhydride. According to the anti-skid ceramic tile prepared by adopting the scheme, an anti-skid coating with micron-sized bulges is formed on the tile surface, the roughness is high, the anti-skid effect is good, the anti-skid performance is greatly improved in a humid environment, and the anti-skid ceramic tile has self-repairing capability and long timeliness after being dried.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic tiles, and in particular to an anti-slip ceramic tile and a preparation process thereof. Background Art

[0002] In the building materials market, anti-slip tiles have always been in demand by customers, especially in humid environments such as bathrooms and toilets, where there is a greater demand for anti-slip effects and timeliness.

[0003] There are many types of anti-slip tiles popular on the market. One is antique tiles, which have an uneven surface, large roughness and good anti-slip effect, but the category is single, the ornamental value is poor, the application range is limited, and as bathroom floor tiles, they are in direct contact with the skin and have obvious wear and tear, and the comfort level is poor. In order to improve comfort, some manufacturers have developed micro-etched skin glazed tiles, which use some acidic substances such as hydrofluoric acid and magnesium fluorosilicate to slightly etch the surface of the tile to increase the surface roughness and enhance the anti-slip effect, but the depth and uniformity of the etching are difficult to control, and the yield rate is low in mass production, the loss increases, and the cost is uncontrollable. If an anti-slip glaze is developed specifically for the anti-slip effect, the thickness of the glaze is large and the cost is increased. Therefore, the most economical and practical way is to use an anti-slip coating to improve the anti-slip effect. The process is simple and the anti-slip effect is good. However, among the commonly used anti-slip coatings, epoxy resins are easy to turn yellow and have poor durability; silicone resins have poor timeliness; polyurethane resins are soft and the anti-slip effect is not obvious.

[0004] Therefore, there is an urgent need for an anti-slip tile to solve the above-mentioned technical problems. Summary of the invention

[0005] The main purpose of the present invention is to provide a preparation process of anti-skid ceramic tiles which have good anti-skid effect, longer aging period and better anti-skid effect in humid environments.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] A preparation process of anti-slip tiles comprises the following steps:

[0008] S1. Apply liquid A on the surface of the finished ceramic tile to form a water film on the surface of the ceramic tile;

[0009] S2, spraying liquid B on the surface of the tile treated in step S1;

[0010] S3, baking the finished ceramic tile obtained in step S2, taking it out, washing the surface with water, and draining the water to obtain the anti-slip ceramic tile;

[0011] The A liquid includes a primer and water, and the primer is one of polyethyleneimine or polyvinyl alcohol;

[0012] The B liquid includes a modifier and ether, and the modifier is one or more of maleic anhydride, phthalic anhydride, biphenyl dianhydride and 4,4'-biphenyl ether dianhydride.

[0013] In the preparation process adopted in this scheme, polyethyleneimine or polyvinyl alcohol is used to undergo interfacial polymerization reaction with aromatic dianhydride. The anhydride is hydrolyzed and ring-opened to form -COOH, which reacts and polymerizes with amino -NH. With the rigid structure of the benzene ring, the brick surface forms a micron-scale raised structure, the surface is rough, and the anti-slip performance is improved. In a humid environment, some of the -CO-NH- groups formed after the polymerization reaction undergo hydrolysis reaction, the chemical bonds are broken, and -COOH and -NH groups are generated, forming a cilia-like structure, thereby increasing the surface roughness and improving the anti-slip performance. After drying and standing for a period of time, the -COOH and -NH groups recombine to form -CO-NH- groups, which have the ability to self-recover, thereby returning to the initial stable state, and the timeliness is longer.

[0014] Preferably, in step S1, after the primer and water are mixed, they are stirred for 30 to 60 minutes, and the mass ratio of the primer and water is (10 to 50):50.

[0015] Preferably, in step S2, the modifier and diethyl ether are mixed and stirred for 30 to 60 minutes, and the mass ratio of the modifier to diethyl ether is (5 to 20):100.

[0016] Preferably, the baking temperature is 60° C. to 80° C., and the baking time is 40s to 90s.

[0017] Preferably, the primer is polyethyleneimine, and the modifier is 4,4'-biphenyl ether dianhydride. When polyethyleneimine and 4,4'-biphenyl ether dianhydride are used, the anti-slip effect and timeliness are the best.

[0018] In addition, the present invention also provides an anti-slip tile, which is prepared by any of the above-mentioned processes for preparing anti-slip tiles. The anti-slip tile has a good anti-slip effect, especially in a humid environment, the anti-slip performance is further improved, and the timeliness is longer than that of conventional polyurethane and silicone resin anti-slip coatings.

[0019] Compared with the prior art, the technical solution of the present invention has at least the following beneficial effects: using polyethyleneimine or polyvinyl alcohol and aromatic dianhydride to undergo interfacial polymerization reaction, a micron-scale convex structure is formed on the surface of the tile, the friction is improved, and the anti-slip effect is good. In a humid environment, the anti-slip coating on the surface of the tile undergoes a hydrolysis reaction, and some chemical bonds are broken, so that the surface coating becomes looser and the roughness increases, thereby greatly improving the anti-slip effect. After drying and standing, the anti-slip coating undergoes a condensation reaction and returns to the initial stable state, with a longer time effectiveness. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying any creative work.

[0021] Figure 1 This is a reaction principle diagram of the technical solution adopted by the present invention.

[0022] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0023] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the fact that ordinary technicians in the field can implement it. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0025] A preparation process of anti-slip tiles comprises the following steps:

[0026] S1. Apply liquid A on the surface of the finished ceramic tile to form a water film on the surface of the ceramic tile;

[0027] S2, spraying liquid B on the surface of the tile treated in step S1;

[0028] S3, baking the finished ceramic tile obtained in step S2, wherein the baking temperature is 60°C to 80°C and the baking time is 40s to 90s. After taking out, wash the surface with water and drain the water to obtain the anti-slip ceramic tile;

[0029] The A liquid includes a primer and water, and the primer is one of polyethyleneimine or polyvinyl alcohol;

[0030] The B liquid includes a modifier and ether, and the modifier is one or more of maleic anhydride, phthalic anhydride, biphenyl dianhydride and 4,4'-biphenyl ether dianhydride.

[0031] Specifically, in step S1, the primer and water are mixed and stirred for 30 to 60 minutes, and the mass ratio of the primer to water is (10 to 50):50.

[0032] Specifically, in step S2, the modifier and ether are mixed and stirred for 30 to 60 minutes, and the mass ratio of the modifier to ether is (5 to 20):100.

[0033] In the prior art, the anti-slip coating on the surface of ceramic tiles is usually made of polyurethane resin materials or silicone resin materials, and the initial dry static friction coefficient is usually in the range of 0.55 to 0.65, but the timeliness is poor. In the double 85 (85% humidity, 85°C) test, the anti-slip effect is greatly reduced within 48 hours. In real life, the durability is usually only 1-3 months.

[0034] This solution uses polyethyleneimine or polyvinyl alcohol to undergo interfacial polymerization with aromatic dianhydride to form an anti-slip coating, such as Figure 1 As shown, the anhydride hydrolyzes and ring-opens to form -COOH, which reacts and polymerizes with the amino group -NH. At the same time, the rigid structure of the benzene ring forms hard and stable protrusions, forming an anti-slip coating with a micron-scale protrusion structure on the surface of the tile. When in a humid environment (humidity ≥ 80%), part of the -CO-NH- undergoes hydrolysis, the chemical bonds are broken, and -COOH and -NH are produced, so that the surface coating becomes looser, forming a cilia-like structure, the surface becomes rougher, and there is a slight pulling effect, so that in a humid environment, the friction is increased and the anti-slip effect is greatly improved. Furthermore, after standing in a dry place, -COOH and -NH undergo a condensation reaction again, returning to the initial stable state, and having the ability to self-repair, thereby further extending the timeliness of the anti-slip coating prepared by this scheme.

[0035] It should be noted that when epoxy resins or silicone resins commonly used on the market are polished, as the solvent dries, the resins agglomerate, and the solvent solidifies prematurely, which is prone to wax marks and wax traces, affecting the appearance. After the primer polyethyleneimine or polyvinyl alcohol of this scheme is mixed with water, it is waxed with a hand polishing machine. It is good to polish until there is a layer of water film on the surface. The aqueous solution polishing method can be used to evenly disperse polyethyleneimine on the brick surface due to water infiltration, which can avoid the phenomenon of wax marks and wax prints; further, aromatic dianhydride is used as a modifier by spraying, which is conducive to the formation of a thinner film layer, and aromatic dianhydride is mixed with ether and sprayed with an oily solution. The interfacial polymerization reaction reacts on the water-oil critical layer, and the reaction speed is fast, so a film layer with a thickness of about 0.2μm can be formed. The film layer is thin and the reaction is rapid. The reaction speed is within 1min, which is suitable for the production line speed. The anti-slip coating in the prior art is usually thicker, generally more than 20μm.

[0036] The aromatic dianhydride used in this scheme has a more stable roughness than long chains due to its rigid benzene ring structure. On the other hand, the polyanhydride structure can increase the reaction sites and help form a wrinkled morphology across amino groups, thereby improving the timeliness of the anti-slip coating.

[0037] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.

[0038] The test methods used in all embodiments and comparative examples of this application are as follows:

[0039] 1. The initial dry static friction coefficient is tested using 4S rubber and EVA materials in accordance with the test method and standard of "Determination of Friction Coefficient" in GB / T4100-2015;

[0040] 2. Double 85 aging test: Place in a constant temperature and humidity chamber with the temperature adjusted to 85°C and the relative humidity to 80%.

[0041] 3. Test under simulated actual conditions: simulate a humid environment with 80% relative humidity and place at room temperature.

[0042] Example 1

[0043] A preparation process of anti-slip tiles comprises the following steps:

[0044] S1. Mix 250g of polyethyleneimine and 250g of water and stir for 30min to obtain liquid A. Apply liquid A on the surface of the finished tile and apply it with a hand polishing machine until a layer of water film is formed on the surface;

[0045] S2, 140g of 4,4'-biphenyl ether dianhydride and 500mL of ether were mixed and stirred for 30min to obtain liquid B, and liquid B was sprayed on the surface of the tile treated in step S1;

[0046] S3, putting the ceramic tile into an oven and baking it at 80° C. for 60 seconds, then taking it out, rinsing the surface with water, and draining the surface water to obtain the anti-slip ceramic tile.

[0047] The prepared anti-slip tiles were cut into samples of 100×100mm size for inspection, and were subjected to initial dry static friction coefficient test, double 85 aging test, and simulation of actual conditions test.

[0048] Example 2

[0049] A preparation process of anti-slip tiles comprises the following steps:

[0050] S1. Mix 150g of polyvinyl alcohol and 350g of water and stir for 45min to obtain liquid A. Apply liquid A on the surface of the finished tile and apply it with a hand polishing machine until a layer of water film is formed on the surface;

[0051] S2, 280g of maleic anhydride and 500mL of ether were mixed and stirred for 45min to obtain liquid B, and liquid B was sprayed on the surface of the tile treated in step S1;

[0052] S3, putting the ceramic tile into an oven and baking it at 80° C. for 40 seconds, then taking it out, rinsing the surface with water, and draining the surface water to obtain the anti-slip ceramic tile.

[0053] The prepared anti-slip tiles were cut into samples of 100×100mm size for inspection, and were subjected to initial dry static friction coefficient test, double 85 aging test, and simulation of actual conditions test.

[0054] Example 3

[0055] A preparation process of anti-slip tiles comprises the following steps:

[0056] S1. Mix 200g of polyethyleneimine and 300g of water and stir for 60min to obtain liquid A. Apply liquid A on the surface of the finished tile and apply it with a hand polishing machine until a layer of water film is formed on the surface;

[0057] S2, 135g of biphenyl dianhydride and 500mL of ether were mixed and stirred for 60min to obtain liquid B, and liquid B was sprayed on the surface of the tile treated in step S1;

[0058] S3, putting the ceramic tile into an oven and baking it at 75° C. for 75 seconds, then taking it out, rinsing the surface with water, and draining the surface water to obtain the anti-slip ceramic tile.

[0059] The prepared anti-slip tiles were cut into samples of 100×100mm size for inspection, and were subjected to initial dry static friction coefficient test, double 85 aging test, and simulation of actual conditions test.

[0060] Example 4

[0061] A preparation process of anti-slip tiles comprises the following steps:

[0062] S1. Mix 250g of polyvinyl alcohol and 250g of water and stir for 30min to obtain liquid A. Apply liquid A on the surface of the finished tile and apply it with a hand polishing machine until a layer of water film is formed on the surface;

[0063] S2, 150g of phthalic anhydride and 500mL of ether were mixed and stirred for 30min to obtain liquid B, and liquid B was sprayed on the surface of the tile treated in step S1;

[0064] S3, putting the ceramic tile into an oven and baking it at 70° C. for 90 seconds, then taking it out, rinsing the surface with water, and draining the surface water to obtain the anti-slip ceramic tile.

[0065] The prepared anti-slip tiles were cut into samples of 100×100mm size for inspection, and were subjected to initial dry static friction coefficient test, double 85 aging test, and simulation of actual conditions test.

[0066] Comparative Example 1

[0067] In this comparative example, 30% SJ909, 4% curing agent, 60% n-butanol, 5% DBE, and 1% tetrabutyl titanate are used on the surface of the finished ceramic tile. A super-cleaning machine is used to add wax water for brush polishing and then dry polishing. After water spraying and cooling for 1 minute, diluted wax water is added for brush polishing. The product is sent into an oven at 350° and kept warm for 1 minute to obtain a ceramic tile product with a polyurethane coating.

[0068] SJ909 is purchased from Sanjin Company, and its main component is isocyanate.

[0069] Comparative Example 2

[0070] In this comparative example, 70% M-9450 and 30% water were used on the surface of the finished ceramic tile, and the surface was polished with a super-cleaning machine and wax water, and then the surface was put into an oven at 350° and kept warm for 1 minute to obtain a ceramic tile product with a water-based silicone resin coating.

[0071] M-9450 was purchased from Chuying New Materials Technology Co., Ltd., and its main component is water-based silicone resin.

[0072] Comparative Example 3

[0073] In this comparative example, 50% M-9120 and 50% ethyl orthosilicate were used on the surface of the finished ceramic tile, and after being brushed and polished with wax water using an ultra-cleaning machine, the finished ceramic tile was placed in an oven at 350° and kept warm for 1 minute to obtain a ceramic tile product with a silicone resin coating.

[0074] M-9120 was purchased from Chuying New Materials Technology Co., Ltd., and its main component is silicone resin.

[0075] The anti-slip tiles prepared in Comparative Examples 1 to 3 were cut into samples of 100×100 mm in size for testing, and were subjected to initial dry static friction coefficient test, double 85 aging test, and simulated actual condition test.

[0076] The initial dry static friction coefficient test results are shown in Table 1.

[0077] Table 1

[0078]

[0079] The double 85 aging test results are shown in Table 2.

[0080] Table 2

[0081]

[0082]

[0083] Note: When the dry static friction coefficient is less than 0.5, it is lower than the national standard.

[0084] The test results of simulating actual conditions are shown in Table 3.

[0085] Table 3

[0086]

[0087] As can be seen from Table 1, the anti-skid tiles prepared by this scheme have different anti-skid effects for different materials. For contact with soft materials such as EVA, PU, ​​leather, and skin, the anti-skid effect is significantly better than that of harder materials such as 4S rubber, PVE, and ABS. Since this scheme is prepared by interfacial polymerization, the anti-skid coating on the surface of the tile is very thin. The micron-scale protrusion structure on the surface of the film layer has a stronger fit than hard materials when the soft material is squeezed, and can form a larger shear force. Therefore, the static friction coefficient of the anti-skid tiles described in this scheme for soft materials is higher than that for hard materials. EVA is a common slipper material at present, which means that the anti-skid tiles prepared by the present invention are more suitable for the anti-skid effect of home scenes.

[0088] As can be seen from Table 2, the anti-aging results of different embodiments are also different. The anti-aging time of Embodiment 1 and Embodiment 3 is long, and the anti-aging effect of Embodiment 2 and Embodiment 4 is slightly worse than that of Embodiment 1 and Embodiment 3, but the timeliness of Embodiments 1 to 4 is better than that of Comparative Examples 1 to 3. This shows that the anti-aging performance of the common wax products on the market used in Comparative Examples 1 to 3 is short, which is mainly manifested in the decline in the anti-slip effect, which is lower than the national standard and is considered to be invalid. In the destruction experiment under continuous high temperature and high humidity environment, the lifespan shown by Embodiment 1 is more durable, and the timeliness can be as long as one and a half years in real life.

[0089] In Table 2, after the 24h double 85 test, the dry static friction coefficient of Examples 1 to 4 was left to stand in a dry environment for 5 days, and then returned to the initial dry static friction coefficient, indicating that the anti-slip tiles prepared by this scheme have a certain self-repairing ability in a dry environment, and can maintain a long-term good anti-slip performance, with a longer timeliness. After complete failure, that is, after the 168h double 85 test, the surface became smooth and slippery due to the complete shedding of the modifier, and would not return to the initial state.

[0090] As can be seen from Table 3, in the test simulating actual conditions, the dry static friction coefficient of Examples 1 to 4 increased from the initial to 48 hours, indicating that the anti-slip performance increased, and the water contact angle decreased, indicating that the amide group decomposed to expose hydrophilic groups such as amino and carboxyl groups. At the same time, in a humid environment, the dry static friction coefficient of Comparative Examples 1 and 3 was almost unchanged. It is further illustrated that the technical solution described in the present application has obvious advantages in anti-slip performance in humid places such as bathrooms.

[0091] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A process for preparing anti-slip tiles, characterized in that: The steps include: S1. Apply liquid A on the surface of the finished ceramic tile to form a water film on the surface of the ceramic tile; S2, spraying liquid B on the surface of the tile treated in step S1; S3, baking the finished ceramic tile obtained in step S2, taking it out, washing the surface with water, and draining the water to obtain the anti-slip ceramic tile; The A liquid includes a primer and water, and the primer is one of polyethyleneimine or polyvinyl alcohol; The B liquid includes a modifier and ether, and the modifier is one or more of maleic anhydride, phthalic anhydride, biphenyl dianhydride and 4,4'-biphenyl ether dianhydride.

2. The process for preparing a non-slip tile according to claim 1, characterized in that: In the step S1, the primer and water are mixed and stirred for 30 to 60 minutes, and the mass ratio of the primer to water is (10 to 50):

50.

3. The process for preparing a non-slip tile according to claim 1, characterized in that: In the step S2, the modifier and diethyl ether are mixed and stirred for 30 to 60 minutes, and the mass ratio of the modifier to diethyl ether is (5 to 20):

100.

4. The process for preparing a non-slip tile according to claim 1, characterized in that: The baking temperature is 60° C. to 80° C., and the baking time is 40s to 90s.

5. The process for preparing a non-slip tile according to claim 1, characterized in that: The primer is polyethyleneimine, and the modifier is 4,4'-biphenyl ether dianhydride. 6.An anti-slip tile, characterized in that: The anti-slip ceramic tile is prepared by the preparation process of any one of claims 1 to 5.

Citation Information

Patent Citations

  • Ceramic tile surface antiskid agent and preparing method thereof

    CN101445393A

  • Brick surface antiskid agent

    CN108707451A

  • Safe and harmless ceramic tile anti-skid agent and preparation method thereof

    CN111040491A

  • Anti-slip stain-resistant ceramic tile and preparation method thereof

    CN115784780A

  • Wear-resistant ceramic tile and preparation process thereof

    CN117964401A