Acrylic resin for high-acid-resistance high-depth-ratio photoresist film for high-precision electroforming plate and preparation method of acrylic resin

By employing a high-pressure process and a specific acrylic resin formulation, the problems of acid resistance and aspect ratio of photoresist on high-precision electroformed plates were solved, achieving high aspect ratio and ultra-thick film formation performance, making it suitable for photoresist films on high-precision electroformed plates.

CN118894955APending Publication Date: 2024-11-05SHANGHAI RAILI ELECTRONIC MATERIALS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410819095.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing photoresists cannot simultaneously achieve acid resistance, high aspect ratio, and ultra-thick film formation performance, thus failing to meet the requirements of high-precision electroformed plates.

Method used

An acrylic resin formulation employing a high-pressure process and specific components, including methyl methacrylate, styrene, butyl acrylate, benzyl methacrylate, and an initiator, controls the reaction temperature and dropping time by extending the dropping time and adding the initiator multiple times, thereby improving the resin's conversion rate and molecular weight.

Benefits of technology

It achieves high acid resistance, high aspect ratio and ultra-thick film formation performance, and is suitable for photoresist films on high-precision electroformed plates. It improves light transmittance and interlayer curing uniformity, and is suitable for the preparation of ultra-thick films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
Patent Text Reader

Abstract

The invention relates to the technical field of photoetching acrylic resin, in particular to the field of IPC C08F236, and more particularly relates to acrylic resin for a high-acid-resistance and high-depth-ratio photoresist film for a high-precision electroforming plate and a preparation method of the acrylic resin. The adhesive comprises the following components: methyl methacrylate, styrene, butyl acrylate, methacrylic acid, benzyl methacrylate, an initiator and a solvent. A high-pressure process is adopted, an optimal acrylic monomer and initiator system is preferably adjusted, azodiisobutyronitrile is selected as an initiator, at a lower reaction temperature of 90 DEG C, the resin has a high conversion rate which reaches 99% by a method of prolonging the dropwise adding time, replenishing the initiator for multiple times and then preserving heat, and the reaction temperature and the dropwise adding time are controlled at the same time, so that the yield of the resin is greatly improved. The molecular weight of the resin is controlled at a relatively high level and the film-forming property of the resin is not influenced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photolithography acrylic resin, in particular to the field of IPC C08F236, and more specifically to an acrylic resin for a photoresist film with high acid resistance and high aspect ratio for a high-precision electroplated plate and a preparation method thereof. Background Art

[0002] High-precision electroformed plates have extremely low hole wall roughness, and the opening shape can be flexibly adjusted to facilitate demolding; and the hardness of electroformed plates is 30% higher than that of ordinary steel sheets, and the service life is long. High-precision electroformed plates are widely used in the printing process of conductive pastes, inks, etc. in industries such as solar energy, semiconductor IC chip packaging, and SMT. Electroformed plates are manufactured by long-term, high-temperature acid electroplating, and the process requires the use of highly acid-resistant, high-aspect-ratio, and ultra-thick photoresist films. It is difficult for products on the market to simultaneously take into account acid resistance, high aspect ratio, and ultra-thick film-forming properties.

[0003] CN117784519A discloses a photoresist, which comprises, by mass percentage, 40%-60% of acrylic ester photosensitive material, 10%-15% of ester solvent, 5%-10% of isophorone, 5%-10% of calcium carbonate, 10%-15% of barium sulfate, 3%-5% of photoinitiator, 1%-3% of photosensitizer and auxiliary agent. The photoresist has stable performance and can be used in the etching process. It has excellent acid resistance after exposure and curing, especially strong tolerance to nitric acid, can protect the product surface in the etching process, can stably exist in acidic etching solution for a long time, and has strong adhesion to the product surface. However, it does not have high aspect ratio and ultra-thick film-forming performance, and cannot be applied to electroplated plates. Summary of the invention

[0004] The first aspect of the present invention provides an acrylic resin for a high acid-resistant, high aspect ratio photoresist film for a high-precision electroplated plate, the components of which include: methyl methacrylate, styrene, butyl acrylate, methacrylic acid, benzyl methacrylate, an initiator and a solvent.

[0005] Preferably, the components include, by weight percentage: 5-15% methyl methacrylate, 5-15% styrene, 2-10% butyl acrylate, 5-10% methacrylic acid, 2-10% benzyl methacrylate, 0.5-5% initiator, and the solvent makes up the balance.

[0006] Further preferably, the components include, by weight percentage: 5-11% methyl methacrylate, 8-15% styrene, 5-10% butyl acrylate, 7-10% methacrylic acid, 4-10% benzyl methacrylate, 0.5-3% initiator, and the solvent makes up the balance.

[0007] More preferably, the components include, by weight percentage: 8-11% methyl methacrylate, 12% styrene, 7% butyl acrylate, 10% methacrylic acid, 3-6% benzyl methacrylate, 0.5-3% initiator, and the balance is made up by solvent.

[0008] The initiator includes at least one of azobisisovaleronitrile, benzoyl peroxide and azobisisobutyronitrile.

[0009] Preferably, the initiator comprises azobisisobutyronitrile.

[0010] The solvent includes at least one of ethyl acetate, cyclohexanone, butanone, acetone, methyl isobutyl ketone, isophorone and tetrahydrofuran.

[0011] The solvent includes ethyl acetate and butanone.

[0012] The solid content of the acrylic resin is greater than 40 wt %.

[0013] The viscosity of the acrylic resin at 25° C. is 2500-4000 mPa·s.

[0014] The second aspect of the present invention provides a method for preparing an acrylic resin for a high acid-resistant, high aspect ratio photoresist film for a high-precision electroformed plate, comprising the following steps:

[0015] Step 1: Add 40-60 wt% of solvent into a high-pressure reaction device, heat while stirring, pressurize and heat the reaction device;

[0016] Step 2: Methyl methacrylate, styrene, butyl acrylate, methacrylic acid, benzyl methacrylate, 60-80 wt % of an initiator, and 5-15 wt % of a solvent are uniformly mixed, and then added dropwise to a high pressure reaction device;

[0017] Step 3: After the dropwise addition is completed, a heat preservation reaction is carried out, and then 10-20wt% of the initiator is added, a second heat preservation reaction is carried out, and the remaining initiator is added, and a third heat preservation reaction is carried out. After the heat preservation is completed, the remaining solvent is added and stirred evenly to obtain the product.

[0018] Preferably, the method for preparing the acrylic resin for a high acid-resistant, high aspect ratio photoresist film for a high-precision electroplated plate comprises the following steps:

[0019] Step 1: Add 50% of the total amount of butanone into the high-pressure reaction device, heat while stirring, the stirring rate is 180r / min, the reaction device is pressurized to 0.1MPa, and when the temperature rises to 90-95°C, prepare to start adding the mixed monomers;

[0020] Step 2: Mix methyl methacrylate, styrene, butyl acrylate, methacrylic acid, benzyl methacrylate, part of the initiator, and part of butanone evenly, and add them together into a dropping tank;

[0021] Step 3: When the temperature of the reaction device in step (1) is 90-95°C, the mixture in step (2) is added dropwise, and the mixture is pumped into the high-pressure reaction device at a uniform speed by a dropping pump. The addition is completed in 4-5 hours, and the mixture is kept warm for 1-2 hours after the addition is completed. Then, an additional portion of initiator is added, and the mixture is kept warm for 1-2 hours. Then, an additional portion of initiator is added, and the mixture is kept warm for 1-2 hours. After the insulation is completed, the remaining butanone is added to dilute the mixture, and the mixture is stirred for 5-10 minutes to obtain the mixture (stirring speed is 180 r / min throughout the process).

[0022] The reaction device is pressurized to 0.1-0.5 MPa and heated to 90-95°C.

[0023] The dropping time is 4-5h.

[0024] The present application has found that the components include 8-11% methyl methacrylate, 12% styrene, 7% butyl acrylate, 10% methacrylic acid, and 3-6% benzyl methacrylate, which can improve acid resistance and depth ratio performance. Since the acrylic resin of the present application is applied to photoresist liquid, and it needs to withstand acid for a long time during the electroplating process of electroforming plate, and the acrylic resin is used for thick film (>100 microns), it is also necessary to have high depth ratio performance, improve the penetration ability of light between resin layers, avoid the bottom wide phenomenon (footing), and may be a compounded monomer system, which improves the dispersion performance of the system, maintains high light transmittance, and regulates the uniformity of the curing rate between layers. The present invention has further found that the high pressure process is adopted, azobisisobutyronitrile is selected as the initiator, and at a lower reaction temperature, the resin has a high conversion rate of 99% by extending the dripping time and repeatedly adding the initiator and then keeping warm again, and the reaction temperature and the dripping time are controlled at the same time, so that the resin molecular weight is controlled at a higher level without affecting the film-forming performance of the resin.

[0025] Beneficial effects:

[0026] 1. High pressure technology is adopted, and the best acrylic monomer and initiator system are selected and adjusted. Azobisisobutyronitrile is selected as the initiator. At a relatively low reaction temperature of 90°C, the resin has a high conversion rate of 99% by extending the dropwise addition time and adding the initiator several times before heat preservation. At the same time, the reaction is controlled.

[0027] The temperature and the dropping time can control the molecular weight of the resin at a higher level without affecting the film-forming properties of the resin.

[0028] 2. The acrylic resin of the present application has a moderate solid content and viscosity and is easy to process. The photoresist and film prepared therein have excellent film-forming properties and uniform thickness, and can be coated into ultra-thick films (>100 microns). It has excellent properties such as high acid resistance and high aspect ratio, and can be used for the preparation of ultra-thick, narrow-opening iron-nickel electroplated plates.

[0029] 3. The components include 8-11% of methyl methacrylate, 12% of styrene, 7% of butyl acrylate, 10% of methacrylic acid, and 3-6% of benzyl methacrylate, which can improve the acid resistance and depth ratio performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 These are SEM images of Example 2 and Example 3 after development and slicing, wherein the left side is Example 3 and the right side is Example 2.

[0031] Figure 2 This is the infrared spectrum of the acrylic resin in Example 1. DETAILED DESCRIPTION

[0032] Example 1

[0033] The invention discloses an acrylic resin for a photoresist film with high acid resistance and high aspect ratio for high-precision electroforming plates. The components thereof are, by weight percentage, 8% methyl methacrylate, 12% styrene, 7% butyl acrylate, 10% methacrylic acid, 6% benzyl methacrylate, 2% initiator, and the balance is made up of solvent.

[0034] The initiator is azobisisobutyronitrile.

[0035] The solvents are butanone and ethyl acetate.

[0036] A method for preparing an acrylic resin for a high-acid-resistant, high-aspect-ratio photoresist film for a high-precision electroformed plate comprises the following steps:

[0037] (1) Add 495 g of butanone into a high pressure reaction device, pressurize to 0.1 MPa, stir at 180 r / min and heat to 90° C.;

[0038] (2) 144 g of methyl methacrylate, 216 g of styrene, 126 g of butyl acrylate, 180 g of methacrylic acid, 108 g of benzyl methacrylate, 25.2 g of initiator, and 90 g of butanone were mixed uniformly and added to a dropping tank;

[0039] (3) When the temperature of the high-pressure reaction device in step (1) reaches 90° C., the mixed monomer and initiator in step (2) are added dropwise through a dropping pump for 4 hours. After the addition is completed, the mixture is kept warm for 1 hour. After the heat preservation is completed, 36 grams of ethyl acetate and 5.4 grams of azobisisobutyronitrile are added. The mixture is kept warm for another 1 hour. After the heat preservation is completed, 36 grams of ethyl acetate and 5.4 grams of azobisisobutyronitrile are added. The mixture is kept warm for another 1 hour. After the heat preservation is completed, 333 grams of butanone are added and stirred for 5 minutes to obtain the product.

[0040] Example 2

[0041] The invention discloses an acrylic resin for a photoresist film with high acid resistance and high aspect ratio for high-precision electroforming plates. The components thereof are, by weight percentage, 11% of methyl methacrylate, 12% of styrene, 7% of butyl acrylate, 10% of methacrylic acid, 3% of benzyl methacrylate, 2% of an initiator, and the balance is made up of a solvent.

[0042] The initiator is azobisisobutyronitrile.

[0043] The solvents are butanone and ethyl acetate.

[0044] A method for preparing an acrylic resin for a high-acid-resistant, high-aspect-ratio photoresist film for a high-precision electroformed plate comprises the following steps:

[0045] (1) Add 495 g of butanone into a high pressure reaction device, pressurize to 0.1 MPa, stir at 180 r / min and heat to 90° C.;

[0046] (2) 198 g of methyl methacrylate, 216 g of styrene, 126 g of butyl acrylate, 180 g of methacrylic acid, 54 g of benzyl methacrylate, 25.2 g of initiator, and 90 g of butanone were mixed evenly and added to a dropping tank;

[0047] (3) When the temperature of the high-pressure reaction device in step (1) reaches 90° C., the mixed monomer and initiator in step (2) are added dropwise through a dropping pump for 4 hours. After the addition is completed, the mixture is kept warm for 1 hour. After the heat preservation is completed, 36 grams of ethyl acetate and 5.4 grams of azobisisobutyronitrile are added. The mixture is kept warm for another 1 hour. After the heat preservation is completed, 36 grams of ethyl acetate and 5.4 grams of azobisisobutyronitrile are added. The mixture is kept warm for another 1 hour. After the heat preservation is completed, 333 grams of butanone are added and stirred for 5 minutes to obtain the product.

[0048] Example 3

[0049] The invention discloses an acrylic resin for a photoresist film with high acid resistance and high aspect ratio for high-precision electroforming plates. The components thereof are, by weight percentage, 8% of methyl methacrylate, 12% of styrene, 7.5% of butyl acrylate, 10% of methacrylic acid, 6% of benzyl methacrylate, 1.5% of an initiator, and the balance is made up of a solvent.

[0050] The initiator is azobisisobutyronitrile.

[0051] The solvents are butanone and ethyl acetate.

[0052] A method for preparing an acrylic resin for a high-acid-resistant, high-aspect-ratio photoresist film for a high-precision electroformed plate comprises the following steps:

[0053] (1) Add 495 g of butanone into a high pressure reaction device, pressurize to 0.1 MPa, stir at 180 r / min and heat to 90° C.;

[0054] (2) 144 g of methyl methacrylate, 216 g of styrene, 135 g of butyl acrylate, 180 g of methacrylic acid, 108 g of benzyl methacrylate, 16.2 g of initiator, and 90 g of butanone were mixed uniformly and added to a dropping tank;

[0055] (3) When the temperature of the high-pressure reaction device in step (1) reaches 90° C., the mixed monomer and initiator in step (2) are added dropwise through a dropping pump for 4 hours. After the addition is completed, the mixture is kept warm for 1 hour. After the heat preservation is completed, 36 grams of ethyl acetate and 5.4 grams of azobisisobutyronitrile are added. The mixture is kept warm for another 1 hour. After the heat preservation is completed, 36 grams of ethyl acetate and 5.4 grams of azobisisobutyronitrile are added. The mixture is kept warm for another 1 hour. After the heat preservation is completed, 333 grams of butanone are added and stirred for 5 minutes to obtain the product.

[0056] Performance Testing Methods

[0057] 1. Test the solid content and conversion rate of acrylic resin in the examples (infrared, such as Figure 2 The test data are listed in Table 1.

[0058] 2. Apply the acrylic resin in the example to a PET substrate with a thickness of 100 μm and then use a DI exposure machine at 60 mj / cm 2 The exposure was used to make analysis and adhesion tests, and the test data are listed in Table 2.

[0059] 3. Coat Example 2 and Example 3 on a PET substrate with a thickness of 100 microns, and then use a DI exposure machine at 60 mj / cm 2 Exposure, development, sectioning and SEM analysis. Figure 1 As shown, the photoresist circuit of the formulation of Example 3 has a bottom widening phenomenon (footing).

[0060] Performance test data

[0061] Table 1

[0062] Viscosity mPa·s Conversion Rate % Solid content wt% Example 1 3500 99 45 Example 2 3000 99 45 Example 3 1800 95 42.8

[0063] Table 2

[0064] Analysis μm Adhesion μm Example 1 35 40 Example 2 30 45 Example 3 45 55

Claims

1. An acrylic resin for a high acid-resistant, high aspect ratio photoresist film for a high-precision electroformed plate, characterized in that: The components include: methyl methacrylate, styrene, butyl acrylate, methacrylic acid, benzyl methacrylate, initiator and solvent.

2. The highly acid-resistant, high aspect ratio acrylic resin for photoresist film for high-precision electroformed plates according to claim 1, characterized in that: The components include, by weight percentage, 5-15% of methyl methacrylate, 5-15% of styrene, 2-10% of butyl acrylate, 5-10% of methacrylic acid, 2-10% of benzyl methacrylate, 0.5-5% of initiator, and the balance is made up of solvent.

3. The highly acid-resistant, high aspect ratio acrylic resin for photoresist film for high-precision electroformed plates according to claim 2, characterized in that: The components include, by weight percentage, 5-11% of methyl methacrylate, 8-15% of styrene, 5-10% of butyl acrylate, 7-10% of methacrylic acid, 4-10% of benzyl methacrylate, 0.5-3% of initiator, and the balance is made up of solvent.

4. The highly acid-resistant, high aspect ratio acrylic resin for photoresist film for high-precision electroformed plates according to claim 1 or 3, characterized in that: The initiator includes at least one of azobisisovaleronitrile, benzoyl peroxide and azobisisobutyronitrile.

5. The highly acid-resistant, high aspect ratio acrylic resin for photoresist film for high-precision electroformed plates according to claim 4, characterized in that: The solvent includes at least one of ethyl acetate, cyclohexanone, butanone, acetone, methyl isobutyl ketone, isophorone and tetrahydrofuran.

6. The highly acid-resistant, high aspect ratio acrylic resin for photoresist film for high-precision electroformed plates according to claim 5, characterized in that: The solid content of the acrylic resin is greater than 40 wt %.

7. The highly acid-resistant, high aspect ratio acrylic resin for photoresist film for high-precision electroformed plates according to claim 6, characterized in that: The viscosity of the acrylic resin at 25° C. is 2500-4000 mPa·s.

8. A method for preparing an acrylic resin for a high acid-resistant, high aspect ratio photoresist film for a high-precision electroformed plate according to any one of claims 1 to 7, characterized in that: The following steps are involved: Step 1: Add 40-60 wt% of solvent into a high-pressure reaction device, heat while stirring, pressurize and heat the reaction device; Step 2: Methyl methacrylate, styrene, butyl acrylate, methacrylic acid, benzyl methacrylate, 60-80 wt % of an initiator, and 5-15 wt % of a solvent are uniformly mixed, and then added dropwise to a high pressure reaction device; Step 3: After the dropwise addition is completed, a heat preservation reaction is carried out, and then 10-20wt% of the initiator is added, a second heat preservation reaction is carried out, and the remaining initiator is added, and a third heat preservation reaction is carried out. After the heat preservation is completed, the remaining solvent is added and stirred evenly to obtain the product.

9. The method for preparing the acrylic resin for a high acid-resistant, high aspect ratio photoresist film for a high-precision electroformed plate according to claim 8, characterized in that: The reaction device is pressurized to 0.1-0.5 MPa and heated to 90-95°C.

10. The method for preparing the acrylic resin for a high acid-resistant, high aspect ratio photoresist film for a high-precision electroformed plate according to claim 9, characterized in that: The dropping time is 4-5h.

Citation Information

Patent Citations

  • Photoresist and preparation method thereof, shell preparation method and electronic equipment