Highly low demolding monomer based on modified polyester resin and preparation process thereof

By introducing glycidyl methacrylate modification into the polyester resin and using silane coupling agents to form modified polyester resin, the problem of poor mold release performance in the preparation of high-thickness lenses is solved. , which achieves lower mold release rate and stronger adhesion force, and improves the yield and production efficiency of the lens.

CN118894970APending Publication Date: 2024-11-05JIANGSU XINDA FINE CHEM TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410974704.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

During the lens manufacturing process, traditional polyester resins have poor mold release performance when preparing high-thickness lenses, resulting in high mold release rate and affecting the quality of the finished product.

Method used

Using highly low-mold release monomers based on modified polyester resin and their preparation process, the formation of more Strong bonding and stable chemical bonding to reduce the demolding rate.

Benefits of technology

It significantly reduces the demolding rate of the lens, improves the yield rate, reduces damage and defects in the production process, and reduces the production costs of the enterprise.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a highly low-demoulding monomer based on modified polyester resin and a preparation process thereof, the highly low-demoulding monomer is applied to a preparation process of a high-thickness lens, and the monomer comprises the following components in parts by weight: 70-80 parts of basic polyester resin; 10 to 15 parts of polyethylene glycol modified by glycidyl methacrylate; 3 to 5 parts of a silane coupling agent; 0.5 to 1 part of an accelerant; 0.5 to 1 part of an initiator; the basic polyester resin is unsaturated polyester resin obtained by reaction of ethylene glycol and maleic anhydride. Glycidyl methacrylate is introduced for modification, so that damage to the product in the production process is reduced. And the modified polyester resin shows stronger binding power, so that the reduction of falling of high-thickness lenses in the production process is facilitated, and the damage and defects caused by falling are effectively avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of a demoulding monomer, and more particularly to a highly low demoulding monomer based on a modified polyester resin and a preparation process thereof. Background Art

[0002] With the continuous advancement of modern science and technology, lenses are increasingly used in the fields of optics, medicine, photography, and precision instruments. The demand for high-quality, high-performance lenses is increasing, which places higher demands on their preparation process and materials. In the manufacturing process of lenses, demoulding is a key step, especially when preparing thick lenses. If the resin bonding force is not enough, the lenses will fall off, affecting the quality of the final product.

[0003] In the traditional lens manufacturing process, polyester resin is often used as the main material. Polyester resin has excellent mechanical properties and chemical stability, but its demoulding performance is not ideal when preparing high-thickness lenses, resulting in a high demoulding rate. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the present invention provides a highly low demoulding monomer based on modified polyester resin and a preparation process thereof, and the specific scheme is as follows:

[0005] A highly low demoulding monomer based on modified polyester resin is used in the preparation process of high-thickness lenses. The monomer comprises the following components in parts by weight: basic polyester resin: 70-80 parts; polyethylene glycol modified with glycidyl methacrylate: 10-15 parts; silane coupling agent: 3-5 parts; accelerator: 0.5-1 part; initiator: 0.5-1 part; the basic polyester resin is an unsaturated polyester resin obtained by the reaction of ethylene glycol and maleic anhydride.

[0006] Furthermore, the molecular weight of the polyethylene glycol modified with glycidyl methacrylate is 400-600, and the modification steps are as follows:

[0007] S1: Add polyethylene glycol and dichloromethane (DCM) and stir with a stirrer until completely dissolved;

[0008] S2: adding p-toluenesulfonic acid as a catalyst to the solution and continuing stirring;

[0009] S3: adding glycidyl methacrylate, slowly dropping it into the reaction mixture using a dropping funnel, and the dropping time is controlled within about 30 minutes to ensure uniform reaction;

[0010] S4: During the reaction, the flask was connected to a condenser, the reaction temperature was controlled at about 60°C, and stirring was maintained; the reaction time was controlled at about 6 hours;

[0011] S5: After the reaction is completed, the reaction mixture is cooled to room temperature; distilled water is slowly added to the reaction mixture and stirred to terminate the reaction;

[0012] S6. Extract, purify and dry to obtain dry modified polyethylene glycol.

[0013] Furthermore, the accelerator is at least one of diethyldiaminomethylbenzene, dimethylaniline and N,N-dimethyl-p-toluidine.

[0014] Furthermore, the initiator is at least one of benzoyl peroxide, methyl ethyl ketone peroxide and hydrogen peroxide.

[0015] A preparation process of a highly low demoulding monomer based on modified polyester resin, the preparation process comprising the following steps:

[0016] S1: Add 70-80 parts of base polyester resin into a reaction kettle;

[0017] S2: slowly add 10-15 parts of polyethylene glycol and stir evenly at a stirring speed of 500-600 rpm for 30 minutes;

[0018] S3: Add 3 to 5 parts of silane coupling agent and continue stirring at a speed of 300 to 400 rpm for 15 minutes;

[0019] S4: heating the uniformly stirred mixture to 80-100° C., maintaining the temperature for 30-60 minutes to ensure that the modifier is fully reacted; cooling to room temperature to obtain a modified polyester resin prepolymer;

[0020] S5: Add 0.5-1 part of accelerator to the prepolymer, stirring at a speed of 200-300 rpm for 10 minutes;

[0021] S6: Add 0.5 to 1 part of initiator and continue stirring at a speed of 200 to 300 rpm for 10 minutes.

[0022] Further, the method of using the monomer is as follows:

[0023] S1: Choose a mold for high-thickness lenses and ensure that the mold surface is smooth and clean;

[0024] S2: Apply a layer of release agent evenly on the surface of the mold to prevent the lens from sticking to the mold;

[0025] S3: injecting the prepared modified polyester resin into the mold, and controlling the injection speed to prevent the generation of bubbles;

[0026] S4: placing the mold injected with resin in a constant temperature box for a curing time of 2-4 hours;

[0027] S5: After the initial curing, move the mold to room temperature and continue curing for 24 hours to ensure that the resin is fully cured.

[0028] Furthermore, the injection rate of the modified polyester resin in S3 is 0.1-0.3 L / min.

[0029] Furthermore, the curing temperature of the resin in S4 is 60-80°C.

[0030] Beneficial effects:

[0031] The present invention provides a highly low demoulding monomer based on modified polyester resin and a preparation process thereof, which has the following advantages:

[0032] (1) By introducing glycidyl methacrylate for modification, polyethylene glycol introduces free radicals into its molecular structure, which help to form more stable chemical bonds with the surface of the lens mold. This enhanced adhesion allows the product to be released from the mold more smoothly during the demolding process, reducing damage to the product during the production process. The modified polyester resin also shows stronger adhesion, which helps to reduce the shedding of high-thickness lenses during the production process, thereby effectively avoiding damage and defects caused by shedding.

[0033] (2) The lower demoulding rate and stronger bonding force work together to greatly improve the yield of lenses and reduce the company's production costs. DETAILED DESCRIPTION

[0034] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.

[0035] Embodiment 1:

[0036] (1) Material preparation:

[0037] Base polyester resin: 75 parts

[0038] Polyethylene glycol modified with glycidyl methacrylate: 12 parts

[0039] Silane coupling agent: 4 parts

[0040] Accelerator: 0.8 parts of diethyl diamino methyl benzene

[0041] Initiator: 0.8 parts benzoyl peroxide

[0042] (2) Modification steps:

[0043] Polyethylene glycol modification:

[0044] S1: Add 400 molecular weight polyethylene glycol and dichloromethane into a flask and stir with a stirrer until completely dissolved.

[0045] S2: Add p-toluenesulfonic acid as a catalyst and continue stirring.

[0046] S3: Slowly add glycidyl methacrylate dropwise through a dropping funnel, and the dropping time is controlled within 30 minutes.

[0047] S4: Connect the flask to a condenser, control the reaction temperature at 60°C, and stir for 6 hours.

[0048] S5: After the reaction is completed, cool to room temperature and slowly add distilled water to terminate the reaction.

[0049] S6: extracting, purifying and drying to obtain dry modified polyethylene glycol.

[0050] (3) Preparation process:

[0051] S1: 75 parts of base polyester resin were added into a reaction kettle.

[0052] S2: Slowly add 12 parts of modified polyethylene glycol, stirring at 550 rpm for 30 minutes.

[0053] S3: Add 4 parts of silane coupling agent and continue stirring at a speed of 350 rpm for 15 minutes.

[0054] S4: heating to 90° C., maintaining for 45 minutes, and cooling to room temperature to obtain a modified polyester resin prepolymer.

[0055] S5: Add 0.8 parts of accelerator, stir at 250 rpm, and stir for 10 minutes.

[0056] S6: Add 0.8 parts of initiator and continue stirring at a stirring speed of 250 rpm for 10 minutes.

[0057] Embodiment 2:

[0058] (1) Material preparation:

[0059] Base polyester resin: 70 parts

[0060] Polyethylene glycol modified with glycidyl methacrylate: 10 parts

[0061] Silane coupling agent: 3 parts

[0062] Accelerator: 1 part N,N-dimethyl-p-toluidine

[0063] Initiator: 0.5 parts hydrogen peroxide

[0064] (2) Modification steps:

[0065] Polyethylene glycol modification:

[0066] S1: Add 600 molecular weight polyethylene glycol and dichloromethane into a flask and stir with a stirrer until completely dissolved.

[0067] S2: Add p-toluenesulfonic acid as a catalyst and continue stirring.

[0068] S3: Slowly add glycidyl methacrylate dropwise through a dropping funnel, and the dropping time is controlled within 30 minutes.

[0069] S4: Connect the flask to a condenser, control the reaction temperature at 60°C, and stir for 6 hours.

[0070] S5: After the reaction is completed, cool to room temperature and slowly add distilled water to terminate the reaction.

[0071] S6: extracting, purifying and drying to obtain dry modified polyethylene glycol.

[0072] (3) Preparation process:

[0073] S1: 70 parts of base polyester resin were added into a reaction kettle.

[0074] S2: Slowly add 10 parts of modified polyethylene glycol, stirring at 500 rpm for 30 minutes.

[0075] S3: Add 3 parts of silane coupling agent and continue stirring at a speed of 300 rpm for 15 minutes.

[0076] S4: heating to 80° C., maintaining for 60 minutes, and cooling to room temperature to obtain a modified polyester resin prepolymer.

[0077] S5: Add 1 part of accelerator, stir at 200 rpm, and stir for 10 minutes.

[0078] S6: Add 0.5 parts of initiator and continue stirring at a speed of 200 rpm for 10 minutes.

[0079] Embodiment 3:

[0080] (1) Material preparation:

[0081] Base polyester resin: 80 parts

[0082] Polyethylene glycol modified with glycidyl methacrylate: 15 parts

[0083] Silane coupling agent: 5 parts

[0084] Accelerator: 0.5 parts of dimethylaniline

[0085] Initiator: 1 part methyl ethyl ketone peroxide

[0086] (2) Modification steps:

[0087] Polyethylene glycol modification:

[0088] S1: Add 500 molecular weight polyethylene glycol and dichloromethane into a flask and stir with a stirrer until completely dissolved.

[0089] S2: Add p-toluenesulfonic acid as a catalyst and continue stirring.

[0090] S3: Slowly add glycidyl methacrylate dropwise through a dropping funnel, and the dropping time is controlled within 30 minutes.

[0091] S4: Connect the flask to a condenser, control the reaction temperature at 60°C, and stir for 6 hours.

[0092] S5: After the reaction is completed, cool to room temperature and slowly add distilled water to terminate the reaction.

[0093] S6: extracting, purifying and drying to obtain dry modified polyethylene glycol.

[0094] (3) Preparation process:

[0095] S1: 80 parts of base polyester resin were added into a reaction kettle.

[0096] S2: Slowly add 15 parts of modified polyethylene glycol, stirring at 600 rpm for 30 minutes.

[0097] S3: Add 5 parts of silane coupling agent and continue stirring at a speed of 400 rpm for 15 minutes.

[0098] S4: heating to 100° C., maintaining for 30 minutes, and cooling to room temperature to obtain a modified polyester resin prepolymer.

[0099] S5: Add 0.5 parts of accelerator, stir at 300 rpm, and stir for 10 minutes.

[0100] S6: Add 1 part of initiator and continue stirring at a speed of 300 rpm for 10 minutes.

[0101] Comparative Example:

[0102] Using traditional resin monomer.

[0103] The resin monomers of Examples 1 to 3 and the comparative example were applied to the demoulding of high-thickness lenses, and the demoulding rates were tested. The test data are as follows:

[0104] Sample Type Release rate Example 1 8% Example 2 5% Example 3 7% Comparative Example 45%

[0105] Compared with the comparative example, the demoulding rates of Examples 1 to 3 are greatly reduced, indicating that the bonding force of the modified polyester resin is significantly enhanced, thereby preventing high-thickness lenses from falling off and damaging the lenses during the manufacturing process.

[0106] As a further improvement, the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A highly low release monomer based on modified polyester resin, characterized in that: Applicable to the preparation process of high-thickness lenses, the monomers include the following components in parts by weight: basic polyester resin: 70-80 parts; polyethylene glycol modified by glycidyl methacrylate: 10-15 parts; silane coupling agent: 3-5 parts; accelerator: 0.5-1 part; Initiator: 0.5-1 part; the base polyester resin is an unsaturated polyester resin obtained by the reaction of ethylene glycol and maleic anhydride.

2. A highly low release monomer based on modified polyester resin according to claim 1, characterized in that: The molecular weight of the polyethylene glycol modified with glycidyl methacrylate is 400-600, and the modification steps are as follows: S1: Add polyethylene glycol and dichloromethane (DCM) and stir with a stirrer until completely dissolved; S2: adding p-toluenesulfonic acid as a catalyst to the solution and continuing stirring; S3: adding glycidyl methacrylate, slowly dropping it into the reaction mixture using a dropping funnel, and the dropping time is controlled within about 30 minutes to ensure uniform reaction; S4: During the reaction, the flask was connected to a condenser, the reaction temperature was controlled at about 60°C, and stirring was maintained; the reaction time was controlled at about 6 hours; S5: After the reaction is completed, the reaction mixture is cooled to room temperature; distilled water is slowly added to the reaction mixture and stirred to terminate the reaction; S6. Extract, purify and dry to obtain dry modified polyethylene glycol.

3. The highly low mold release monomer based on modified polyester resin according to claim 1, characterized in that: The accelerator is at least one of diethyldiaminomethylbenzene, dimethylaniline and N,N-dimethyl-p-toluidine.

4. The highly low mold release monomer based on modified polyester resin according to claim 1, characterized in that: The initiator is at least one of benzoyl peroxide, methyl ethyl ketone peroxide and hydrogen peroxide.

5. A process for preparing a highly low demoulding monomer based on modified polyester resin, characterized in that: The preparation process comprises the following steps: S1: Add 70-80 parts of base polyester resin into a reaction kettle; S2: slowly add 10-15 parts of polyethylene glycol and stir evenly at a stirring speed of 500-600 rpm for 30 minutes; S3: Add 3 to 5 parts of silane coupling agent and continue stirring at a speed of 300 to 400 rpm for 15 minutes; S4: heating the uniformly stirred mixture to 80-100° C., maintaining the temperature for 30-60 minutes to ensure that the modifier is fully reacted; cooling to room temperature to obtain a modified polyester resin prepolymer; S5: Add 0.5-1 part of accelerator to the prepolymer, stirring at a speed of 200-300 rpm for 10 minutes; S6: Add 0.5 to 1 part of initiator and continue stirring at a speed of 200 to 300 rpm for 10 minutes.

6. The highly low mold release monomer based on modified polyester resin according to claim 1, characterized in that: The monomer is used as follows: S1: Choose a mold for high-thickness lenses and ensure that the mold surface is smooth and clean; S2: Apply a layer of release agent evenly on the surface of the mold to prevent the lens from sticking to the mold; S3: injecting the prepared modified polyester resin into the mold, and controlling the injection speed to prevent the generation of bubbles; S4: placing the mold injected with resin in a constant temperature box for a curing time of 2-4 hours; S5: After the initial curing, move the mold to room temperature and continue curing for 24 hours to ensure that the resin is fully cured.

7. A highly low release monomer based on modified polyester resin according to claim 6, characterized in that: The injection rate of the modified polyester resin in S3 is 0.1-0.3 L / min.

8. The highly low mold release monomer based on modified polyester resin according to claim 6, characterized in that: The curing temperature of the resin in S4 is 60 to 80°C.