Washable polyurethane high polymer material and preparation method thereof

By adjusting the component ratio and reaction steps in the polyurethane material, a polyurethane polymer material with high water washing resistance and mechanical properties is formed, which solves the problem of insufficient hydrolysis resistance of polyurethane materials after water washing, extends the service life of the material and enhances the Its stability.

CN118894979APending Publication Date: 2024-11-05NANTONG YOUNUO TEXTILE CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411400296.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing polyurethane polymer materials have insufficient hydrolysis resistance and water washing after washing, resulting in unstable molecular chains, losing their original strength and elasticity, and may even cause deterioration and damage of the material.

Method used

Polypropylene glycol, polytetrahydrofuran glycol, isocyanate, catalyst, crosslinking agent and additive are used to form prepolymers and emulsify and cure through adjustment of the proportion and reaction steps, thereby increasing the hydrolysis resistance and mechanical properties of the material.

Benefits of technology

It significantly improves the water washing resistance of polyurethane polymer materials, extends the service life of the material, avoids damage after washing, and enhances the thermal stability and mechanical properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894979A_ABST
    Figure CN118894979A_ABST
Patent Text Reader

Abstract

According to the washable polyurethane high polymer material and the preparation method thereof, polypropylene glycol, polytetrahydrofuran glycol, isocyanate, a catalyst, a cross-linking agent and an additive are combined, permeation and contact of water molecules in the high polymer material are reduced, and the washing resistance of the polyurethane high polymer material can be improved; damage after water washing is avoided, and the defect that in the prior art, a polyurethane high polymer material is insufficient in hydrolysis resistance and water washing performance is overcome; the hydrolysis-resistant substance can significantly improve the stability of the material in a wet environment, can reduce the erosion of water molecules to molecular chains of the material, prolongs the service life of the material, and improves the washing resistance of the polyurethane high polymer material; the curing method in S5 is one or more of drying curing and radiation curing, both drying curing and radiation curing are effective curing methods, rapid curing can be achieved on the surface of the material or at a specific depth, the thermal stability of the material can be improved through drying curing, and therefore the heat resistance of the material is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of polyurethane polymer materials, in particular to a polyurethane material prepared by reactions other than carbon-carbon unsaturated bonds, and in particular to a water-washable polyurethane polymer material and a preparation method thereof. Background Art

[0002] Polyurethane is a polymer material, and its full name is polyurethane. It is a polymer with repeating structural units of carbamate segments formed by polycondensation reaction of isocyanate and polyol under certain conditions. Polyurethane has large elongation, wide hardness range, large formula adjustment range, excellent wear resistance and mechanical properties. The main chain of polyurethane contains more carbamate groups, which is the basis of its unique properties. Polyurethane has excellent processing technology, is easy to put into industrial production, is easy to use and cures quickly.

[0003] Polyurethane is a polymer material containing ester groups and amino groups, which are easily hydrolyzed in water. The hydrolysis reaction will cause the molecular chain of the polyurethane material to break, thus destroying its original structure and performance.

[0004] The prior art CN 107488252 A discloses a washable slow-rebound polyurethane foam and its preparation method and application. By optimizing the formula and preparation process, the polyurethane foam has the characteristics of good air permeability, slow rebound speed and quick dehydration and drying after washing, so that such products can be used continuously and for a long time, save resources, reduce environmental pollution, and maintain home hygiene. The polyurethane foam produced by this formula and process has mesh openings and is washable. The pore size range of the polyurethane foam is (20-50) PPI; the opening rate is 85%-95%, the slow rebound time is (1-5) seconds, and the density range is (40-65) kg / m 3 However, during use, hydrolysis reaction still occurs when it can dry quickly, making the molecular chain of the polyurethane material unstable, losing its original strength and elasticity, and may even cause deterioration and damage of the material.

[0005] Therefore, it is necessary to improve the polyurethane polymer material in the prior art to solve the above problems. Summary of the invention

[0006] The present invention overcomes the deficiencies of the prior art and provides a water-washable polyurethane polymer material and a preparation method thereof, aiming to solve the defects of the prior art polyurethane polymer material in terms of insufficient hydrolysis resistance and water washability.

[0007] To achieve the above object, the technical solution adopted by the present invention is: a water-washable polyurethane polymer material, composed of component A, component B and component C, wherein: The A component comprises polypropylene glycol and polytetrahydrofuran diol, and the ratio between the polypropylene glycol and the polytetrahydrofuran diol is 1:1; The B component is an isocyanate, and the isocyanate includes one or more of hexamethylene diisocyanate and isophorone diisocyanate; The C component includes: a catalyst, a cross-linking agent and an additive, wherein the mass ratio of the catalyst, the cross-linking agent and the additive is 1-10:10-50:100-500; The mass ratio of the A component, the B component and the C component is 10-20:5-10:1-3.

[0008] In a preferred embodiment of the present invention, the component A and the component B further include hydrolysis-resistant substances, respectively. The hydrolysis-resistant substances include fluorocarbon diol and silane diol. The ratio between the fluorocarbon diol and the silane diol is 1:2-4.

[0009] In a preferred embodiment of the present invention, the mass ratio of the hydrolysis-resistant substance in the component A and the component B is consistent with the mass ratio between the component A and the component B, and the mass of the hydrolysis-resistant substance accounts for 5-15% of the total mass of the component A and the component B.

[0010] In a preferred embodiment of the present invention, the catalyst is dibutyltin dilaurate.

[0011] In a preferred embodiment of the present invention, the cross-linking agent is one of trimethylolpropane or isocyanate trimer.

[0012] In a preferred embodiment of the present invention, the additive comprises a carbodiimide stabilizer and a hindered phenol antioxidant, and the carbodiimide stabilizer and the hindered phenol antioxidant are of the same quality.

[0013] To achieve the above object, the second technical solution adopted by the present invention is: a method for preparing a water-washable polyurethane polymer material, comprising the following steps: S1: Add the A component and the catalyst into a container, introduce nitrogen and stir, the reaction temperature is 70-85° C., the reaction time is 2-4 hours, and a prepolymer is formed; S2: Add the B component into the container, the reaction temperature is 70-80°C, and the reaction time is 1-2h; S3: adding the crosslinking agent into the container, the reaction temperature is 75-85°C, and the reaction time is 2-3h; S4: adding the additive into the container, the reaction temperature is 75-85°C, and the reaction time is 0.5-1h; S5: placing the reactants at a temperature of 80-120° C. for curing for 3-4 hours.

[0014] In a preferred embodiment of the present invention, between S4 and S5, the reactants are emulsified, an emulsifier solution is added to the reactants, the emulsification temperature is 30-40° C., and the emulsification time is 1-2 h.

[0015] In a preferred embodiment of the present invention, in the emulsifier solution, the solute is one of a nonionic emulsifier and an anionic emulsifier, the solute accounts for 2%-4% of the mass of the reactants, and the concentration of the emulsifier solution is 30-45%.

[0016] In a preferred embodiment of the present invention, in S5, the curing method is one or more of drying curing and radiation curing.

[0017] The present invention solves the defects existing in the background technology and has the following beneficial effects: (1) The present application provides a water-washable polyurethane polymer material, which combines polypropylene glycol, polytetramethylene glycol, isocyanate, a catalyst, a cross-linking agent and an additive to reduce the penetration and contact of water molecules in the polymer material. Compared with the polyurethane polymer material in the prior art, the water-washing resistance of the polyurethane polymer material is improved, damage after washing is avoided, and the defects of the polyurethane polymer material in the prior art, that is, insufficient hydrolysis resistance and water washability, are solved.

[0018] (2) In the present invention, polypropylene glycol, polytetramethylene glycol and isocyanate are all provided with hydrolysis-resistant substances, which can significantly improve the stability of the materials in a humid environment. Compared with the prior art, the hydrolysis-resistant substances can reduce the erosion of water molecules on the molecular chains of the materials, extend the service life of the materials, and improve the water washability of the polyurethane polymer materials.

[0019] (3) In the present invention, the curing method of S5 is one or more of drying curing and radiation curing. Both drying curing and radiation curing are effective curing methods that can accelerate the transformation of materials from liquid to solid. Compared with the prior art, they can improve production efficiency and achieve rapid curing on the surface of the material or at a specific depth. Drying curing can improve the thermal stability of the material, thereby enhancing its heat resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work. Figure 1 It is a method step diagram of a preferred embodiment of the present invention. DETAILED DESCRIPTION

[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.

[0023] To achieve the above object, the technical solution adopted by the present invention is: a water-washable polyurethane polymer material, composed of component A, component B and component C, wherein: Component A includes polypropylene glycol and polytetramethylene glycol, and the ratio between polypropylene glycol and polytetramethylene glycol is 1:1.

[0024] The B component is isocyanate, and the isocyanate includes one or more of hexamethylene diisocyanate and isophorone diisocyanate.

[0025] Component C includes: a catalyst, a cross-linking agent and an additive, and the mass ratio of the catalyst, the cross-linking agent and the additive is 1-10:10-50:100-500.

[0026] The mass ratio between component A, component B and component C is 10-20:5-10:1-3. By adjusting the ratio of component A and component B, the formation rate of the prepolymer and the degree of crosslinking of the final product can be controlled, thereby affecting the mechanical properties and chemical stability of the material. By adjusting the ratio of components A, B and C, the mechanical properties of the material such as hardness, elasticity and tensile strength can be optimized to meet the needs of different application scenarios. By adjusting the component ratio, the thermal stability of the material can be affected to ensure better heat resistance during processing and use.

[0027] Component A and component B also include hydrolysis-resistant substances, which include fluorocarbon diol and silane diol, and the ratio between fluorocarbon diol and silane diol is 1:2-4. Hydrolysis-resistant substances can significantly improve the stability of materials in a humid environment, reduce the erosion of water molecules on the molecular chains of materials, and extend the service life of materials. Fluorocarbon diol and silane diol have high chemical stability, can resist the erosion of a variety of chemical substances, and improve the durability of materials in harsh chemical environments. The introduction of hydrolysis-resistant substances can affect the mechanical properties of materials, such as improving tensile strength, wear resistance and tear resistance, which depends on the interaction between the chemical structure of fluorocarbon diol and silane diol and the polyurethane chain. Fluorocarbon diol is a hydrolysis-resistant substance, and silane diol is a hydrocarbon dialkoxy silane.

[0028] The mass ratio of the hydrolysis-resistant substance in component A and component B is consistent with the mass ratio between component A and component B, and the mass of the hydrolysis-resistant substance accounts for 5-15% of the sum of the mass of component A and component B. The consistent mass ratio of the hydrolysis-resistant substance helps to maintain the uniformity of the material, thereby ensuring the performance consistency of the material throughout the use process. By controlling the ratio of the hydrolysis-resistant substance, the hydrolysis resistance of the material can be accurately adjusted to avoid performance problems caused by excess or deficiency.

[0029] The catalyst is dibutyltin dilaurate. Dibutyltin dilaurate is an effective catalyst that can significantly increase the reaction rate of isocyanate and alcohol and shorten the production cycle. Through catalysis, the conversion rate of raw materials can be increased, the unreacted raw material residue can be reduced, and the purity and performance of the material can be improved. Dibutyltin dilaurate can improve the mechanical properties of polyurethane, such as increasing its hardness, strength and wear resistance. Dibutyltin dilaurate helps to improve the hydrolysis resistance of the material, especially its performance in humid environments.

[0030] The crosslinking agent is one of trimethylolpropane or isocyanate trimer. The crosslinking agent can increase the connection points between the polyurethane molecular chains, improve the crosslinking degree of the material, and thus enhance its mechanical properties. Through crosslinking, the hardness, strength, wear resistance and tear resistance of the material can be improved. The crosslinking structure helps to improve the stability of the material in a humid environment and reduce the impact of hydrolysis on the material properties.

[0031] The additives include carbodiimide stabilizers and hindered phenolic antioxidants, and the carbodiimide stabilizers and hindered phenolic antioxidants are of the same quality. By using two different types of additives in equal amounts, a balance of performance can be achieved, avoiding the problems caused by excessive or insufficient amounts of a single additive. The two additives have a synergistic effect, working together on the material to provide better protection than either additive alone. The carbodiimide stabilizer helps to improve the stability of the material in a humid environment and reduce hydrolysis.

[0032] like Figure 1 As shown, in order to achieve the above-mentioned purpose, the second set of technical solutions adopted by the present invention is: a method for preparing a water-washable polyurethane polymer material, comprising the following steps: S1: Add component A and catalyst into a container, introduce nitrogen and stir, the reaction temperature is 70-85°C, the reaction time is 2-4h, and a prepolymer is formed; S2: Add component B into the container, the reaction temperature is 70-80°C, and the reaction time is 1-2h; S3: adding a cross-linking agent to the container, the reaction temperature is 75-85°C, and the reaction time is 2-3h; S4: Add additives to the container, the reaction temperature is 75-85°C, and the reaction time is 0.5-1h; S5: placing the reactants at a temperature of 80-120° C. for curing for 3-4 hours.

[0033] Between S4 and S5, the reactants are emulsified by adding an emulsifier solution to the reactants at an emulsification temperature of 30-40°C for 1-2 hours. In the emulsifier solution, the solute is one of a nonionic emulsifier and an anionic emulsifier, and the solute accounts for 2%-4% of the reactant mass. The concentration of the emulsifier solution is 30-45%.

[0034] Emulsifiers can improve the dispersibility of reactants, make different components evenly distributed in the system, and improve the quality of the final product. Emulsifiers help to form a stable emulsion system and prevent the reactants from phase separation before curing. Emulsifiers can improve the surface properties of materials, such as improving surface smoothness and reducing surface tension. Non-ionic emulsifiers are sucrose stearate and anionic emulsifiers are sodium lauryl sulfate, both of which have good emulsifying ability.

[0035] In S5, the curing method is one or more of drying curing and radiation curing. Both drying curing and radiation curing are effective curing methods, which can accelerate the transformation of materials from liquid to solid and improve production efficiency. Radiation curing, especially ultraviolet or electron beam curing, can achieve rapid curing on the surface of the material or at a specific depth, and is suitable for applications with specific requirements on the curing depth. Drying curing can improve the thermal stability of the material because it allows the material to be cured at a higher temperature, thereby enhancing its heat resistance. Radiation curing is usually carried out at room temperature or lower temperatures, which can reduce energy consumption and thermal impact on the environment.

[0036] Radiation curing uses a radiation source such as ultraviolet light or electron beam, with a radiation intensity of 200-300mJ / cm 2 Ultraviolet radiation at room temperature for 3-4 hours can effectively cure the material. Embodiment 1

[0037] This embodiment provides a water-washable polyurethane polymer material, and the preparation method comprises the following steps: S1: adding polypropylene glycol and polytetrahydrofuran diol in a container, wherein the ratio of polypropylene glycol to polytetrahydrofuran diol is 1:1, and adding dibutyltin dilaurate, wherein the mass ratio of polypropylene glycol, polytetrahydrofuran diol and dibutyltin dilaurate is 10:10:1, introducing nitrogen and stirring, the reaction temperature is 80° C., the reaction time is 3 h, and a prepolymer is formed; S2: adding hexamethylene diisocyanate to the container, the mass of the added hexamethylene diisocyanate is 50% of the mass of the prepolymer, and adding a hydrolysis-resistant substance, the hydrolysis-resistant substance is bishydroxy fluoroalcohol and hydrocarbon dialkoxysilane, the mass ratio of bishydroxy fluoroalcohol and hydrocarbon dialkoxysilane is 1:3, the mass ratio of the hydrolysis-resistant substance to the prepolymer is 1:10, the reaction temperature is 70°C, and the reaction time is 2h; S3: adding trimethylolpropane to the container, the mass ratio of trimethylolpropane to the reactant is 1:20, the reaction temperature is 75°C, and the reaction time is 2h; S4: adding diimine stabilizer and hindered phenol antioxidant to the container, the mass ratio between diimine stabilizer and hindered phenol antioxidant and reactant is 1:100, the reaction temperature is 85°C, and the reaction time is 0.5h; S5: Add 40% sodium dodecyl sulfate solution to the container for emulsification treatment, the emulsification temperature is 30°C, the solute in the sodium dodecyl sulfate solution accounts for 2% of the reactant mass, and the emulsification time is 1 hour. After emulsification treatment, the reactant is placed at a temperature of 120°C for drying and curing, and the curing time is 4 hours to obtain a washable polyurethane polymer material. Embodiment 2

[0038] This embodiment provides a water-washable polyurethane polymer material, and the preparation method comprises the following steps: S1: adding polypropylene glycol and polytetrahydrofuran diol in a container, wherein the ratio of polypropylene glycol to polytetrahydrofuran diol is 1:1, and adding dibutyltin dilaurate, wherein the mass ratio of polypropylene glycol, polytetrahydrofuran diol and dibutyltin dilaurate is 10:10:1, introducing nitrogen and stirring, the reaction temperature is 80° C., the reaction time is 3 h, and a prepolymer is formed; S2: adding hexamethylene diisocyanate to the container, the mass of the added hexamethylene diisocyanate is 50% of the mass of the prepolymer, and adding a hydrolysis-resistant substance, the hydrolysis-resistant substance is bishydroxy fluoroalcohol and hydrocarbon dialkoxysilane, the mass ratio of bishydroxy fluoroalcohol and hydrocarbon dialkoxysilane is 1:3, the mass ratio of the hydrolysis-resistant substance to the prepolymer is 1:15, the reaction temperature is 70°C, and the reaction time is 2h; S3: adding trimethylolpropane to the container, the mass ratio of trimethylolpropane to the reactant is 1:20, the reaction temperature is 75°C, and the reaction time is 2h; S4: adding diimine stabilizer and hindered phenol antioxidant to the container, the mass ratio between diimine stabilizer and hindered phenol antioxidant and reactant is 1:100, the reaction temperature is 85°C, and the reaction time is 0.5h; S5: Add 40% sodium dodecyl sulfate solution to the container for emulsification treatment, the emulsification temperature is 30°C, the solute in the sodium dodecyl sulfate solution accounts for 2% of the reactant mass, and the emulsification time is 1 hour. After emulsification treatment, the reactant is placed at a temperature of 120°C for drying and curing, and the curing time is 4 hours to obtain a washable polyurethane polymer material. Embodiment 3

[0039] This embodiment provides a water-washable polyurethane polymer material, and the preparation method comprises the following steps: S1: adding polypropylene glycol and polytetrahydrofuran diol in a container, wherein the ratio of polypropylene glycol to polytetrahydrofuran diol is 1:1, and adding dibutyltin dilaurate, wherein the mass ratio of polypropylene glycol, polytetrahydrofuran diol and dibutyltin dilaurate is 10:10:1, introducing nitrogen and stirring, the reaction temperature is 80° C., the reaction time is 3 h, and a prepolymer is formed; S2: adding hexamethylene diisocyanate to the container, the mass of the added hexamethylene diisocyanate is 50% of the mass of the prepolymer, and adding a hydrolysis-resistant substance, the hydrolysis-resistant substance is bishydroxy fluoroalcohol and hydrocarbon dialkoxysilane, the mass ratio of bishydroxy fluoroalcohol and hydrocarbon dialkoxysilane is 1:3, the mass ratio of the hydrolysis-resistant substance to the prepolymer is 1:20, the reaction temperature is 70°C, and the reaction time is 2h; S3: adding trimethylolpropane to the container, the mass ratio of trimethylolpropane to the reactant is 1:20, the reaction temperature is 75°C, and the reaction time is 2h; S4: adding diimine stabilizer and hindered phenol antioxidant to the container, the mass ratio between diimine stabilizer and hindered phenol antioxidant and reactant is 1:100, the reaction temperature is 85°C, and the reaction time is 0.5h; S5: Add 40% sodium dodecyl sulfate solution to the container for emulsification treatment, the emulsification temperature is 30°C, the solute in the sodium dodecyl sulfate solution accounts for 2% of the reactant mass, and the emulsification time is 1 hour. After emulsification treatment, the reactant is placed at a temperature of 120°C for drying and curing, and the curing time is 4 hours to obtain a washable polyurethane polymer material. Embodiment 4

[0040] This embodiment provides a water-washable polyurethane polymer material, and the preparation method comprises the following steps: S1: adding polypropylene glycol and polytetrahydrofuran diol in a container, wherein the ratio of polypropylene glycol to polytetrahydrofuran diol is 1:1, and adding dibutyltin dilaurate, wherein the mass ratio of polypropylene glycol, polytetrahydrofuran diol and dibutyltin dilaurate is 10:10:1, introducing nitrogen and stirring, the reaction temperature is 80° C., the reaction time is 3 h, and a prepolymer is formed; S2: adding hexamethylene diisocyanate to the container, the mass of the added hexamethylene diisocyanate is 50% of the mass of the prepolymer, and adding a hydrolysis-resistant substance, the hydrolysis-resistant substance is bishydroxy fluoroalcohol and hydrocarbon dialkoxysilane, the mass ratio of bishydroxy fluoroalcohol and hydrocarbon dialkoxysilane is 1:3, the mass ratio of the hydrolysis-resistant substance to the prepolymer is 1:25, the reaction temperature is 70°C, and the reaction time is 2h; S3: adding trimethylolpropane to the container, the mass ratio of trimethylolpropane to the reactant is 1:20, the reaction temperature is 75°C, and the reaction time is 2h; S4: adding diimine stabilizer and hindered phenol antioxidant to the container, the mass ratio between diimine stabilizer and hindered phenol antioxidant and reactant is 1:100, the reaction temperature is 85°C, and the reaction time is 0.5h; S5: Add 40% sodium dodecyl sulfate solution to the container for emulsification treatment, the emulsification temperature is 30°C, the solute in the sodium dodecyl sulfate solution accounts for 2% of the reactant mass, and the emulsification time is 1 hour. After emulsification treatment, the reactant is placed at a temperature of 120°C for drying and curing, and the curing time is 4 hours to obtain a washable polyurethane polymer material. Embodiment 5

[0041] This embodiment provides a water-washable polyurethane polymer material, and the preparation method comprises the following steps: S1: adding polypropylene glycol and polytetrahydrofuran diol in a container, wherein the ratio of polypropylene glycol to polytetrahydrofuran diol is 1:1, and adding dibutyltin dilaurate, wherein the mass ratio of polypropylene glycol, polytetrahydrofuran diol and dibutyltin dilaurate is 10:10:1, introducing nitrogen and stirring, the reaction temperature is 80° C., the reaction time is 3 h, and a prepolymer is formed; S2: adding hexamethylene diisocyanate to the container, the mass of the added hexamethylene diisocyanate is 50% of the mass of the prepolymer, and adding a hydrolysis-resistant substance, the hydrolysis-resistant substance is bishydroxy fluoroalcohol and hydrocarbon dialkoxysilane, the mass ratio of bishydroxy fluoroalcohol and hydrocarbon dialkoxysilane is 1:3, the mass ratio of the hydrolysis-resistant substance to the prepolymer is 1:30, the reaction temperature is 70°C, and the reaction time is 2h; S3: adding trimethylolpropane to the container, the mass ratio of trimethylolpropane to the reactant is 1:20, the reaction temperature is 75°C, and the reaction time is 2h; S4: adding diimine stabilizer and hindered phenol antioxidant to the container, the mass ratio between diimine stabilizer and hindered phenol antioxidant and reactant is 1:100, the reaction temperature is 85°C, and the reaction time is 0.5h; S5: Add 40% sodium dodecyl sulfate solution to the container for emulsification treatment, the emulsification temperature is 30°C, the solute in the sodium dodecyl sulfate solution accounts for 2% of the reactant mass, and the emulsification time is 1 hour. After emulsification treatment, the reactant is placed at a temperature of 120°C for drying and curing, and the curing time is 4 hours to obtain a washable polyurethane polymer material. Embodiment 6

[0042] This embodiment provides a water-washable polyurethane polymer material, and the preparation method comprises the following steps: S1: adding polypropylene glycol and polytetrahydrofuran diol in a container, wherein the ratio of polypropylene glycol to polytetrahydrofuran diol is 1:1, and adding dibutyltin dilaurate, wherein the mass ratio of polypropylene glycol, polytetrahydrofuran diol and dibutyltin dilaurate is 10:10:1, introducing nitrogen and stirring, the reaction temperature is 80° C., the reaction time is 3 h, and a prepolymer is formed; S2: adding hexamethylene diisocyanate to the container, the mass of the added hexamethylene diisocyanate is 50% of the mass of the prepolymer, and adding a hydrolysis-resistant substance, the hydrolysis-resistant substance is bishydroxy fluoroalcohol and hydrocarbon dialkoxysilane, the mass ratio of bishydroxy fluoroalcohol and hydrocarbon dialkoxysilane is 1:3, the mass ratio of the hydrolysis-resistant substance to the prepolymer is 1:20, the reaction temperature is 70°C, and the reaction time is 2h; S3: adding trimethylolpropane to the container, the mass ratio of trimethylolpropane to the reactant is 1:20, the reaction temperature is 75°C, and the reaction time is 2h; S4: adding diimine stabilizer and hindered phenol antioxidant to the container, the mass ratio between diimine stabilizer and hindered phenol antioxidant and reactant is 1:100, the reaction temperature is 85°C, and the reaction time is 0.5h; S5: Add 40% sodium dodecyl sulfate solution to the container for emulsification treatment, the emulsification temperature is 30°C, the solute in the sodium dodecyl sulfate solution accounts for 1% of the reactant mass, and the emulsification time is 1 hour. After emulsification treatment, the reactant is placed at a temperature of 120°C for drying and curing, and the curing time is 4 hours to obtain a washable polyurethane polymer material. Embodiment 7

[0043] This embodiment provides a water-washable polyurethane polymer material, and the preparation method comprises the following steps: S1: adding polypropylene glycol and polytetrahydrofuran diol in a container, wherein the ratio of polypropylene glycol to polytetrahydrofuran diol is 1:1, and adding dibutyltin dilaurate, wherein the mass ratio of polypropylene glycol, polytetrahydrofuran diol and dibutyltin dilaurate is 10:10:1, introducing nitrogen and stirring, the reaction temperature is 80° C., the reaction time is 3 h, and a prepolymer is formed; S2: adding hexamethylene diisocyanate to the container, the mass of the added hexamethylene diisocyanate is 50% of the mass of the prepolymer, and adding a hydrolysis-resistant substance, the hydrolysis-resistant substance is bishydroxy fluoroalcohol and hydrocarbon dialkoxysilane, the mass ratio of bishydroxy fluoroalcohol and hydrocarbon dialkoxysilane is 1:3, the mass ratio of the hydrolysis-resistant substance to the prepolymer is 1:20, the reaction temperature is 70°C, and the reaction time is 2h; S3: adding trimethylolpropane to the container, the mass ratio of trimethylolpropane to the reactant is 1:20, the reaction temperature is 75°C, and the reaction time is 2h; S4: adding diimine stabilizer and hindered phenol antioxidant to the container, the mass ratio between diimine stabilizer and hindered phenol antioxidant and reactant is 1:100, the reaction temperature is 85°C, and the reaction time is 0.5h; S5: Add 40% sodium dodecyl sulfate solution to the container for emulsification treatment, the emulsification temperature is 30°C, the solute in the sodium dodecyl sulfate solution accounts for 3% of the reactant mass, and the emulsification time is 1 hour. After emulsification treatment, the reactant is placed at a temperature of 120°C for drying and curing, and the curing time is 4 hours to obtain a washable polyurethane polymer material. Embodiment 8

[0044] This embodiment provides a water-washable polyurethane polymer material, and the preparation method comprises the following steps: S1: adding polypropylene glycol and polytetrahydrofuran diol in a container, wherein the ratio of polypropylene glycol to polytetrahydrofuran diol is 1:1, and adding dibutyltin dilaurate, wherein the mass ratio of polypropylene glycol, polytetrahydrofuran diol and dibutyltin dilaurate is 10:10:1, introducing nitrogen and stirring, the reaction temperature is 80° C., the reaction time is 3 h, and a prepolymer is formed; S2: adding hexamethylene diisocyanate to the container, the mass of the added hexamethylene diisocyanate is 50% of the mass of the prepolymer, and adding a hydrolysis-resistant substance, the hydrolysis-resistant substance is bishydroxy fluoroalcohol and hydrocarbon dialkoxysilane, the mass ratio of bishydroxy fluoroalcohol and hydrocarbon dialkoxysilane is 1:3, the mass ratio of the hydrolysis-resistant substance to the prepolymer is 1:20, the reaction temperature is 70°C, and the reaction time is 2h; S3: adding trimethylolpropane to the container, the mass ratio of trimethylolpropane to the reactant is 1:20, the reaction temperature is 75°C, and the reaction time is 2h; S4: adding diimine stabilizer and hindered phenol antioxidant to the container, the mass ratio between diimine stabilizer and hindered phenol antioxidant and reactant is 1:100, the reaction temperature is 85°C, and the reaction time is 0.5h; S5: Add 40% sodium dodecyl sulfate solution to the container for emulsification treatment, the emulsification temperature is 30°C, the solute in the sodium dodecyl sulfate solution accounts for 4% of the reactant mass, and the emulsification time is 1 hour. After emulsification treatment, the reactant is placed at a temperature of 120°C for drying and curing, and the curing time is 4 hours to obtain a washable polyurethane polymer material. Embodiment 9

[0045] This embodiment provides a water-washable polyurethane polymer material, and the preparation method comprises the following steps: S1: adding polypropylene glycol and polytetrahydrofuran diol in a container, wherein the ratio of polypropylene glycol to polytetrahydrofuran diol is 1:1, and adding dibutyltin dilaurate, wherein the mass ratio of polypropylene glycol, polytetrahydrofuran diol and dibutyltin dilaurate is 10:10:1, introducing nitrogen and stirring, the reaction temperature is 80° C., the reaction time is 3 h, and a prepolymer is formed; S2: adding hexamethylene diisocyanate to the container, the mass of the added hexamethylene diisocyanate is 50% of the mass of the prepolymer, and adding a hydrolysis-resistant substance, the hydrolysis-resistant substance is bishydroxy fluoroalcohol and hydrocarbon dialkoxysilane, the mass ratio of bishydroxy fluoroalcohol and hydrocarbon dialkoxysilane is 1:3, the mass ratio of the hydrolysis-resistant substance to the prepolymer is 1:20, the reaction temperature is 70°C, and the reaction time is 2h; S3: adding trimethylolpropane to the container, the mass ratio of trimethylolpropane to the reactant is 1:20, the reaction temperature is 75°C, and the reaction time is 2h; S4: adding diimine stabilizer and hindered phenol antioxidant to the container, the mass ratio between diimine stabilizer and hindered phenol antioxidant and reactant is 1:100, the reaction temperature is 85°C, and the reaction time is 0.5h; S5: Add 40% sodium dodecyl sulfate solution to the container for emulsification treatment, the emulsification temperature is 30°C, the solute in the sodium dodecyl sulfate solution accounts for 5% of the reactant mass, and the emulsification time is 1 hour. After emulsification treatment, the reactant is placed at a temperature of 120°C for drying and curing, and the curing time is 4 hours to obtain a washable polyurethane polymer material.

[0046] Comparative Example 1 This embodiment provides a polyurethane polymer material, and the preparation method includes the following steps: S1: adding polypropylene glycol and polytetrahydrofuran diol in a container, wherein the ratio of polypropylene glycol to polytetrahydrofuran diol is 1:1, and adding dibutyltin dilaurate, wherein the mass ratio of polypropylene glycol, polytetrahydrofuran diol and dibutyltin dilaurate is 10:10:1, introducing nitrogen and stirring, the reaction temperature is 80° C., the reaction time is 3 h, and a prepolymer is formed; S2: Add hexamethylene diisocyanate to the container, the mass of the added hexamethylene diisocyanate is 50% of the mass of the prepolymer, the reaction temperature is 75°C, and the reaction time is 2h; S3: adding trimethylolpropane to the container, the mass ratio of trimethylolpropane to the reactant is 1:20, the reaction temperature is 70°C, and the reaction time is 2h; S4: adding diimine stabilizer and hindered phenol antioxidant to the container, the mass ratio between diimine stabilizer and hindered phenol antioxidant and reactant is 1:100, the reaction temperature is 85°C, and the reaction time is 0.5h; S5: Add 40% sodium dodecyl sulfate solution to the container for emulsification treatment, the emulsification temperature is 30°C, the solute in the sodium dodecyl sulfate solution accounts for 3% of the reactant mass, and the emulsification time is 1 hour. After emulsification treatment, the reactant is placed at a temperature of 120°C for drying and curing, and the curing time is 4 hours to obtain a polyurethane polymer material.

[0047] Comparative Example 2 This embodiment provides a polyurethane polymer material, and the preparation method includes the following steps: S1: adding polypropylene glycol and polytetrahydrofuran diol in a container, wherein the ratio of polypropylene glycol to polytetrahydrofuran diol is 1:1, and adding dibutyltin dilaurate, wherein the mass ratio of polypropylene glycol, polytetrahydrofuran diol and dibutyltin dilaurate is 10:10:1, introducing nitrogen and stirring, the reaction temperature is 80° C., the reaction time is 3 h, and a prepolymer is formed; S2: adding hexamethylene diisocyanate to the container, the mass of the added hexamethylene diisocyanate is 50% of the mass of the prepolymer, and adding a hydrolysis-resistant substance, the hydrolysis-resistant substance is bishydroxy fluoroalcohol and hydrocarbon dialkoxysilane, the mass ratio of bishydroxy fluoroalcohol and hydrocarbon dialkoxysilane is 1:3, the mass ratio of the hydrolysis-resistant substance to the prepolymer is 1:20, the reaction temperature is 70°C, and the reaction time is 2h; S3: adding trimethylolpropane to the container, the mass ratio of trimethylolpropane to the reactant is 1:20, the reaction temperature is 75°C, and the reaction time is 2h; S4: adding diimine stabilizer and hindered phenol antioxidant to the container, the mass ratio between diimine stabilizer and hindered phenol antioxidant and reactant is 1:100, the reaction temperature is 85°C, and the reaction time is 0.5h; S5: The reactants are placed at a temperature of 120° C. for drying and curing for 4 hours to obtain a polyurethane polymer material.

[0048] The samples in Examples 1 to 9 and Comparative Examples 1 to 2 were respectively recorded for initial resilience and initial tensile strength, and washed 28 times, each time for 5 minutes. The samples were placed at room temperature to dry between adjacent washing times. After all washing steps, the resilience after washing and the tensile strength after washing were recorded. The resilience retention rate was the ratio between the resilience after washing and the initial resilience, and the tensile strength retention rate was the ratio between the tensile strength after washing and the initial tensile strength. The water washing resistance test data of the samples are shown in Table 1: Table 1 Water wash resistance test data of samples in Examples 1 to 9 and Comparative Examples 1 to 2

[0049] As can be seen from Table 1, in Example 1 to Example 5, the mass ratio of the hydrolysis-resistant substance to the prepolymer gradually increases, and the resilience retention rate and the tensile strength retention rate first increase and then decrease. When the mass ratio of the hydrolysis-resistant substance to the prepolymer gradually increases, the cross-linking density of the material will also increase, providing better network structure support, and the resilience and tensile strength of the material can be maintained. However, when the mass ratio of the hydrolysis-resistant substance to the prepolymer is too high, excessive cross-linking will occur, making the material too rigid, thereby reducing the stability of its resilience, and reducing the uniformity inside the material, resulting in stress concentration, thereby reducing the stability of the tensile strength. The preferred embodiment is Example 3.

[0050] In Example 3 and Examples 6 to 9, the solute in the sodium dodecyl sulfate solution accounts for a gradually increased mass proportion of the reactants, and the resilience retention rate and the tensile strength retention rate both increase first and then decrease. The increase of sodium dodecyl sulfate improves the compatibility between the polyurethane and other components, thereby improving the stability of the resilience and tensile strength. However, if the solute in the sodium dodecyl sulfate solution accounts for too high a mass proportion of the reactants, it will cause excessive emulsification, and excessive emulsification will destroy the stability of the emulsion, causing the emulsion to separate or form large droplets, which will reduce the uniformity and compatibility of the material, thereby reducing the stability of the resilience and tensile strength. The preferred embodiment is Example 7.

[0051] In Examples 1 to 9 and Comparative Examples 1 to 2, the stability of the resilience and tensile strength in Examples 1 to 9 are higher than those in Comparative Example 1 and Comparative Example 2, and the preparation method of the washable polyurethane polymer material in the present application has superiority.

[0052] The above is based on the ideal embodiment of the present invention. Through the above description, relevant personnel can make various changes and modifications without departing from the technical concept of the present invention. The technical scope of the present invention is not limited to the content in the specification, and the technical scope must be determined according to the scope of the claims.

Claims

1. A washable polyurethane polymer material, It is characterized in that It consists of component A, component B and component C, wherein: The A component comprises polypropylene glycol and polytetrahydrofuran diol, and the ratio between the polypropylene glycol and the polytetrahydrofuran diol is 1:1; The B component is an isocyanate, and the isocyanate includes one or more of hexamethylene diisocyanate and isophorone diisocyanate; The C component includes: a catalyst, a cross-linking agent and an additive, wherein the mass ratio of the catalyst, the cross-linking agent and the additive is 1-10:10-50:100-500; The mass ratio of the A component, the B component and the C component is 10-20:5-10:1-3.

2. A washable polyurethane polymer material according to claim 1, Features: The component A and the component B also include hydrolysis-resistant substances, respectively. The hydrolysis-resistant substances include fluorocarbon diol and silane diol. The ratio between the fluorocarbon diol and the silane diol is 1:2-4.

3. A washable polyurethane polymer material according to claim 2, Features: The mass ratio of the hydrolysis-resistant substance in the A component and the B component is consistent with the mass ratio between the A component and the B component, and the mass of the hydrolysis-resistant substance accounts for 5-15% of the total mass of the A component and the B component.

4. A washable polyurethane polymer material according to claim 1, Features: The catalyst is dibutyltin dilaurate.

5. A washable polyurethane polymer material according to claim 1, Features: The cross-linking agent is one of trimethylolpropane or isocyanate trimer.

6. A washable polyurethane polymer material according to claim 1, Features: The additives include a carbodiimide stabilizer and a hindered phenol antioxidant, and the carbodiimide stabilizer and the hindered phenol antioxidant have the same quality.

7. A method for preparing a water-washable polyurethane polymer material, based on the water-washable polyurethane polymer material according to any one of claims 1 to 6, It is characterized in that The following steps are involved: S1: Add the A component and the catalyst into a container, introduce nitrogen and stir, the reaction temperature is 70-85° C., the reaction time is 2-4 hours, and a prepolymer is formed; S2: Add the B component into the container, the reaction temperature is 70-80°C, and the reaction time is 1-2h; S3: adding the crosslinking agent into the container, the reaction temperature is 75-85°C, and the reaction time is 2-3h; S4: adding the additive into the container, the reaction temperature is 75-85°C, and the reaction time is 0.5-1h; S5: curing the reactants at a temperature of 80-120° C. for 3-4 hours to obtain a water-washable polyurethane polymer material.

8. A method for preparing a water-washable polyurethane polymer material according to claim 7, Features: Between S4 and S5, the reactants are emulsified by adding an emulsifier solution to the reactants. The emulsification temperature is 30-40° C. and the emulsification time is 1-2 hours.

9. A method for preparing a water-washable polyurethane polymer material according to claim 8, Features: In the emulsifier solution, the solute is one of a nonionic emulsifier and an anionic emulsifier, the solute accounts for 2%-4% of the mass of the reactants, and the concentration of the emulsifier solution is 30-45%.

10. The method for preparing a water-washable polyurethane polymer material according to claim 7, Features: In S5, the curing method is one or more of drying curing and radiation curing.

Citation Information

Patent Citations

  • Method for preparing side-chain non-ion aqueous polyurethane emulsion

    CN101638472A

  • Fluorine-containing polyurethane and preparation method thereof

    CN102115524A

  • Wet type polyurethane resin, production process and application method thereof

    CN102993398A

  • Improved polyurethane, preparation method and application thereof

    CN103289047A

  • Method for preparing fluorescent polyurethane emulsion

    CN104177585A