CuTEP-PPV-COF polymer as well as preparation method and application thereof

CuTEP-PPV-COF polymer is used as a catalyst to solve the problem of difficulty in recycling the catalyst and the use of precious metals, and achieves efficient and stable catalytic performance and low-cost benzyl alcohol oxidation reaction, which has good recycling and environmental protection.

CN118894988AActive Publication Date: 2024-11-05SHANDONG NORMAL UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410944870.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-05
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

In the existing catalytic oxidation methods, catalysts are difficult to recycle and reuse, resulting in pollution and waste, and precious metals are often required, and the synthesis steps are complicated and it is difficult to achieve large-scale industrial production.

Method used

CuTEP-PPV-COF polymer was used as catalyst by using 5,10,15,20-tetrakis(4-ethynylphenyl)porphyrin copper and 1,4-bis[(6-azidohexyl)oxy] -2,5-Diiodobenzene is frozen-thawed and circulated to degass in a mixed solution of dimethyl sulfoxide and water, and undergoes solvothermal reactions to prepare CuTEP-PPV-COF with high crystallinity and porous structure. The catalyst is used for the oxidation reaction of benzyl alcohol.

Benefits of technology

CuTEP-PPV-COF polymer has efficient and stable catalytic properties. The yield of catalyzed benzaldehyde can reach 99%, and the catalytic yield of more than 95% is maintained after six cycles. It is cheap and easy to separate. 实验过程中无特殊或有毒有害试剂使用,反应条件温和。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894988A_ABST
    Figure CN118894988A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of porous organic polymer materials, in particular to a CuTEP-PPV-COF polymer, a preparation method of the CuTEP-PPV-COF polymer and application of the CuTEP-PPV-COF polymer as a catalyst to catalysis of benzyl alcohol to synthesize benzaldehyde. When the CuTEP-PPV-COF polymer provided by the invention is used as a main catalyst and tetramethylpiperidine oxide (TEMPO) is used as a cocatalyst to catalyze benzyl alcohol to synthesize benzaldehyde, the yield can reach 99%. Meanwhile, after six times of circular reaction of the CuTEP-PPV-COF polymer, the catalytic yield still keeps 95% or above, so that the CuTEP-PPV-COF polymer provided by the invention can be proved to have efficient and stable catalytic performance and can be recycled for multiple times. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of porous organic polymer materials, and in particular to a CuTEP-PPV-COF polymer and a preparation method thereof, and application of the CuTEP-PPV-COF polymer as a catalyst in catalyzing benzyl alcohol to synthesize benzaldehyde. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Benzaldehyde is widely used as an important chemical intermediate in industries such as medicine and pesticides. Its preparation methods are mainly toluene oxidation method and benzyl alcohol oxidation method. Compared with toluene, benzyl alcohol has low toxicity, low price and high reaction efficiency. Therefore, benzyl alcohol oxidation method has become the most feasible method for preparing benzaldehyde. The traditional oxidation reaction of benzyl alcohol uses permanganate and dichromate as oxidants, which not only produces a large amount of environmentally unfriendly heavy metal waste, but also has poor selectivity of the oxidation reaction. Therefore, chemists have developed a large number of catalytic oxidation methods, using metal as catalyst and molecular oxygen as oxidant to avoid the use of toxic strong oxidants, which provides a green way for the selective oxidation of benzyl alcohol.

[0004] However, in the reported catalytic oxidation methods, most are homogeneous reactions, and the catalyst cannot be recycled, which is easy to cause pollution and waste. Compared with homogeneous catalysis, heterogeneous catalysis has the advantages of stable and recyclable catalysts, which is more in line with the requirements of sustainable synthetic chemistry. However, in the existing disclosed heterogeneous catalytic technology, it is often necessary to use precious metals such as Ru, Pt, Pd, Au, Rh, etc. as catalysts, and the catalyst synthesis steps are complicated, making it difficult to achieve large-scale industrial production.

[0005] Covalent organic framework materials (COFs) are emerging porous crystalline polymers in two-dimensional conjugated network materials. They have size-adjustable nanopores, high specific surface area, good chemical stability, and uniformly dispersed catalytic active sites. Therefore, they have good development prospects in the field of catalytic oxidation of benzyl alcohol. Summary of the invention

[0006] In order to overcome the above problems, the present invention provides a CuTEP-PPV-COF polymer and a preparation method thereof, and use of the CuTEP-PPV-COF polymer as a catalyst in catalyzing the synthesis of benzyl alcohol into benzaldehyde.

[0007] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:

[0008] The first aspect of the present invention provides a CuTEP-PPV-COF polymer, the structural formula of which is shown in formula (I):

[0009]

[0010] The second aspect of the present invention provides a method for preparing the above-mentioned CuTEP-PPV-COF polymer, comprising:

[0011] The ligands 5,10,15,20-tetrakis(4-ethynylphenyl)porphyrin copper (CuTEP) and 1,4-bis[(6-azidohexyl)oxy]-2,5-diiodobenzene (PPV-N 3 ) is dispersed in a mixed solution of dimethyl sulfoxide (DMSO) and water, and then sodium ascorbate and anhydrous copper sulfate are added as catalysts. The mixed solution is placed in a liquid nitrogen bath for freeze-thaw and cyclic degassing, and then sealed for solvothermal reaction to obtain CuTEP-PPV-COF polymer;

[0012] The reaction process is:

[0013]

[0014] The third aspect of the present invention provides the use of the above-mentioned CuTEP-PPV-COF polymer as a catalyst.

[0015] The beneficial effects of the present invention are:

[0016] (1) The CuTEP-PPV-COF polymer prepared in the present invention has the properties of high crystallinity, large porosity, and good chemical stability, and therefore has the potential to be used as a catalyst.

[0017] (2) When the CuTEP-PPV-COF polymer provided by the present invention is used as the main catalyst and tetramethylpiperidinyl oxide (TEMPO) is used as the co-catalyst to catalyze the synthesis of benzaldehyde from benzyl alcohol, the yield can be as high as 99%. At the same time, after six cycles of reaction, the CuTEP-PPV-COF polymer still maintains a catalytic yield of more than 95%, which proves that the CuTEP-PPV-COF polymer provided by the present invention has efficient and stable catalytic performance and can be recycled multiple times.

[0018] (3) The CuTEP-PPV-COF polymer provided by the present invention is used as a catalyst for catalyzing the oxidation reaction of benzyl alcohol. The catalyst is low in price, high in yield and purity, and easy to separate. No special, toxic or harmful reagents are used during the experiment, and the reaction conditions are mild. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0020] Figure 1 This is a scanning electron microscope image of the CuTEP-PPV-COF prepared in Example 3 of the present invention;

[0021] Figure 2 This is the thermogravimetric diagram of CuTEP-PPV-COF prepared in Example 3 of the present invention;

[0022] Figure 3 The experimental and simulated PXRD patterns of CuTEP-PPV-COF prepared in Example 3 of the present invention;

[0023] Figure 4 is the N of CuTEP-PPV-COF prepared in Example 3 of the present invention 2 Adsorption map;

[0024] Figure 5 This is the PXRD pattern of the CuTEP-PPV-COF prepared in Example 3 of the present invention after catalysis for 5 times. DETAILED DESCRIPTION

[0025] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0026] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0027] The first typical embodiment of the present invention provides a CuTEP-PPV-COF polymer, the structural formula of which is shown in formula (I):

[0028]

[0029] A second typical embodiment of the present invention provides a method for preparing the above-mentioned CuTEP-PPV-COF polymer, comprising:

[0030] The ligands 5,10,15,20-tetrakis(4-ethynylphenyl)porphyrin copper (CuTEP) and 1,4-bis[(6-azidohexyl)oxy]-2,5-diiodobenzene (PPV-N 3 ) is dispersed in a mixed solution of dimethyl sulfoxide (DMSO) and water, and then sodium ascorbate and anhydrous copper sulfate are added as catalysts. The mixed solution is placed in a liquid nitrogen bath for freeze-thaw and cyclic degassing, and then sealed for solvothermal reaction to obtain CuTEP-PPV-COF polymer;

[0031] The reaction process is:

[0032]

[0033] In one or more embodiments, the ligands 5,10,15,20-tetrakis(4-ethynylphenyl)porphyrin copper (CuTEP) and 1,4-bis[(6-azidohexyl)oxy]-2,5-diiodobenzene (PPV-N 3 ) is 1:1.8 to 2.2, preferably 1:2.

[0034] In one or more embodiments, in the mixed solution of dimethyl sulfoxide and water, the volume ratio of dimethyl sulfoxide to water is 1.8 to 2.2:1, preferably 2:1.

[0035] In one or more embodiments, the concentration of the ligand copper 5,10,15,20-tetrakis(4-ethynylphenyl)porphyrin (CuTEP) in a mixed solution of dimethyl sulfoxide (DMSO) and water is 2-4 mmol / L, preferably 3 mmol / L.

[0036] In one or more embodiments, the molar ratio of the ligand 5,10,15,20-tetrakis(4-ethynylphenyl)porphyrin copper (CuTEP) and sodium ascorbate to anhydrous copper sulfate is 5:0.8-1.2:0.8:-1.2, preferably 5:1:1.

[0037] In one or more embodiments, the temperature of the solvothermal reaction is 110-130° C., preferably 120° C.; the time of the solvothermal reaction is 90-100 h, preferably 94 h.

[0038] In one or more embodiments, the preparation method of the ligand 5,10,15,20-tetrakis(4-ethynylphenyl)porphyrin copper (CuTEP) comprises:

[0039] (1) Compound 1 was dissolved in dichloromethane, and then pyrrole and boron trifluoride ether were added. After reacting at room temperature for 2 to 4 hours, tetrachlorobenzoquinone was added and reacted at 35 to 45° C. for 0.5 to 2 hours. After the reaction was completed, the solvent was removed and the compound 2 was obtained after purification;

[0040] (2) Compound 2 and tetrabutylammonium fluoride are added to tetrahydrofuran, and the mixture is reacted at room temperature for 2 to 4 hours. After the reaction, water is added, the filtrate is collected by filtration, and the solvent is removed and dried to obtain compound 3;

[0041] (3) Copper acetate was dissolved in methanol, and added into dichloromethane together with compound 3, and stirred at room temperature for 10 to 15 hours. After the reaction, dichloromethane extraction, sodium bicarbonate solution washing, dehydration and drying were performed in sequence, and then rotary evaporation and drying were performed to obtain 5,10,15,20-tetrakis(4-ethynylphenyl)porphyrin copper (CuTEP).

[0042] The reaction process is:

[0043]

[0044] In one or more embodiments, 1,4-bis[(6-azidohexyl)oxy]-2,5-diiodobenzene (PPV-N 3 ) comprises:

[0045] (1)N 2 Under atmosphere, 1,4-diiodobenzene, 18-crown-6, 1,6-dibromohexane and K 2 CO 3 Add acetone and react at 75-85°C for 70-80h; after the reaction is completed, add deionized water to quench the reaction, extract the product with dichloromethane, collect the organic phase, remove the solvent, and purify to obtain 1,4-bis[(6-bromohexyl)oxy]-2,5-diiodobenzene (PPV-Br);

[0046] (2) PPV-Br and sodium azide are added to a mixed solution of N,N-dimethylacetamide, dichloromethane and water, and reacted at 85-95°C for 10-14 hours. After the reaction is completed, the mixture is cooled to room temperature, ice water is added to the reaction solution, and the solid obtained by filtration is 1,4-bis[(6-azidohexyl)oxy]-2,5-diiodobenzene (PPV-N 3 );

[0047] The reaction process is:

[0048]

[0049] Preferably, in step (1), 1,4-diiodobenzene, 18-crown-6, 1,6-dibromohexane and K 2 CO 3 The molar ratio is 9-11:0.9-1.1:155-170:50-60, preferably 10:1:160:54.

[0050] Preferably, in step (2), the molar ratio of PPV-Br to sodium azide is 1:8-12, preferably 1:10.

[0051] The third aspect of the present invention provides the use of the above-mentioned CuTEP-PPV-COF polymer as a catalyst.

[0052] In one or more embodiments, the application includes catalyzing the synthesis of benzyl alcohol into benzaldehyde.

[0053] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.

[0054] Example 1

[0055] Preparation of ligand 5,10,15,20-tetrakis(4-ethynylphenyl)porphyrin copper (CuTEP):

[0056] (1) Compound 1 (4.0 mmol, 810 mg) was weighed and placed in a 500 mL three-necked flask. Dichloromethane (350 mL) was added, and pyrrole (4.0 mmol, 280 μL) and boron trifluoride ether (0.9 mmol, 140 μL) were added dropwise. After stirring at room temperature for 3 h, tetrachlorobenzoquinone (3.1 mmol, 760 mg) was added and stirred at 40° C. for 1 h. After the reaction was completed, the reaction solution changed from brown to black. The solution was dried by rotary evaporation and purified by column chromatography to obtain compound 2.

[0057] (2) Compound 2 (1.0 mmol, 670 mg) was weighed and placed in a 100 mL flask. Tetrabutylammonium fluoride (1.5 mL) and tetrahydrofuran (40 mL) were added and stirred at room temperature for 3 h. After the reaction was completed, the filtrate was collected, rotary evaporated, and dried to obtain compound 3.

[0058] (3) Dissolve copper acetate (0.74 mmol, 147 mg) in 70 mL of methanol, place it together with compound 3 (0.075 mmol, 53 mg) in a 250 mL flask, add dichloromethane (30 mL), and stir at room temperature for 12 h. After the reaction, evaporate the solvent in vacuo, extract the product with dichloromethane, wash with 10% NaHCO3 solution, and dry it with anhydrous MgSO4. After filtering, rotary evaporation and vacuum drying, the product is obtained. Ligand 5,10,15,20-tetrakis(4-ethynylphenyl)porphyrin copper (CuTEP).

[0059] The reaction process is:

[0060]

[0061] Example 2

[0062] 1,4-Bis[(6-azidohexyl)oxy]-2,5-diiodobenzene (PPV-N 3 ) Preparation:

[0063] (1)N 2 Under atmosphere, 1,4-diiodobenzene (2.5 mmol, 0.9 mg), 18-crown-6 (0.25 mmol, 72.8 mg), K 2 CO 3 (13.5mmol, 1.4mg) was added to a 100mL flask, and 1,6-dibromohexane (40.0mmol, 10.0g) and 25mL acetone were added, and the reaction was carried out at 80°C for 72h. After the reaction was completed, 25mL H 2 O to quench the reaction, extract the product with dichloromethane, dry it with anhydrous magnesium sulfate, remove the solvent in vacuo, and use dichloromethane / petroleum ether (1:5) as the eluent to obtain a white solid, which is 1,4-bis[(6-bromohexyl)oxy]-2,5-diiodobenzene (PPV-Br).

[0064] (2) PPV-Br (0.3 mmol, 200.0 mg) and sodium azide (3.0 mmol, 195.0 mg) were placed in a 50 mL flask, and 7.5 mL DMF, 2 mL CH 2 Cl 2 and 2 mL H 2 O, react at 90°C for 12 hours. After the reaction is completed, cool to room temperature, add ice water to the reaction solution, and a white crystalline solid precipitates. Filter to obtain the solid, wash the solid with water first, and finally wash the solid with anhydrous ethanol for 3 times, and dry it naturally to obtain a white crystalline product. That is 1,4-bis[(6-azidohexyl)oxy]-2,5-diiodobenzene (PPV-N 3 ).

[0065] The reaction process is:

[0066]

[0067] Example 3

[0068] Preparation of CuTEP-PPV-COF polymer:

[0069] The ligands 5,10,15,20-tetrakis(4-ethynylphenyl)porphyrin copper (CuTEP) (0.01 mmol, 8.0 mg) and 1,4-bis[(6-azidohexyl)oxy]-2,5-diiodobenzene (PPV-N 3) (0.02mmol, 12.24mg) was placed in a pressure-resistant glass tube, sodium ascorbate (0.002mmol, 0.3mg) and anhydrous copper sulfate (0.002mmol, 0.32mg) were added as catalysts, and then 3mL of dimethyl sulfoxide aqueous solution (volume ratio of 2:1) was added, and the mixed solution was placed in a liquid nitrogen bath for freeze-thaw and cyclic degassing for 3 times, and then sealed and placed in an oven. The temperature was raised from room temperature to 120°C within 24h by programmed heating. After reacting at 120°C for 96h, the heating was stopped, and after the oven temperature dropped to room temperature, the solid in the glass tube was taken out and lysed with DMF and H 2 After being completely washed with O and tetrahydrofuran (THF), the mixture was dried in vacuo to obtain a red crystalline powder, which was the product CuTEP-PPV-COF.

[0070] The CuTEP-PPV-COF polymer prepared in this example was characterized. Figure 1 This is the scanning electron microscope image of CuTEP-PPV-COF polymer. Figure 2 Thermogravimetric image of CuTEP-PPV-COF polymer. Figure 3 PXRD pattern of CuTEP-PPV-COF polymer. Figure 4 N of CuTEP-PPV-COF polymer 2 Attach the image. Figure 1 , Figure 3 and Figure 4 It can be seen from the graph that the CuTEP-PPV-COF polymer prepared in this example has a porous structure. Figure 2-3 It can be seen that the CuTEP-PPV-COF polymer is a crystalline porous material with high thermal stability.

[0071] Experimental Example 1

[0072] The CuTEP-PPV-COF polymer prepared in Example 3 of the present invention is used as a catalyst to catalyze the oxidation reaction of benzyl alcohol.

[0073] The preparation process is as follows: benzyl alcohol (0.21mmol, 20μL), CuTEP-PPV-COF (1mmol%, 0.01mmol, 20.0mg), and tetramethylpiperidinium oxide (Tempo) (1mmol%, 0.01mmol, 1.56mg) are added to a 25mL reaction bottle, 2mL of xylene is added as a solvent, and the reaction is carried out at 130°C for 30h. After the reaction is completed, the temperature is lowered to room temperature, and CuTEP-PPV-COF is separated by centrifugation. The reaction yield is determined by gas chromatography-mass spectrometry (GC-MS).

[0074] The specific reaction equation is as follows:

[0075]

[0076] The reaction was tracked by TLC. After the reaction was completed, the catalyst was recovered by centrifugation and directly put into the next cycle reaction. According to the above conditions, the catalyst was used for six cycles. The reaction solution was separated and the yield was calculated. The catalytic effect is shown in Table 1. Figure 5 The PXRD pattern of the catalyst after 5 cycles. Figure 5 It can be seen that after the catalyst was cycled 5 times, the CuTEP-PPV-COF framework did not change. As can be seen from Table 1, the yield of the product remained basically the same, and after six cycles, it only showed a slight downward trend, reflecting the excellent stability of the catalyst, which can be reused more than six times, can significantly improve the utilization rate of the catalyst, and reduce production costs.

[0077] Table 1 Catalytic effect of CuTEP-PPV-COF multiple cycle reactions

[0078]

[0079] When the CuTEP-PPV-COF polymer provided by the present invention is used as the main catalyst and tetramethylpiperidinyl oxide (TEMPO) is used as the co-catalyst to catalyze the synthesis of benzaldehyde from benzyl alcohol, the yield can be as high as 99%. At the same time, after six cycles of reaction, the CuTEP-PPV-COF polymer still maintains a catalytic yield of more than 95%, which proves that the CuTEP-PPV-COF polymer provided by the present invention has efficient and stable catalytic performance and can be recycled for multiple times.

[0080] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A CuTEP-PPV-COF polymer, characterized in that The structural formula is shown in formula (I):

2. The method for preparing the CuTEP-PPV-COF polymer according to claim 1, characterized in that: include: The ligand 5,10,15,20-tetrakis(4-ethynylphenyl)porphyrin copper and 1,4-bis[(6-azidohexyl)oxy]-2,5-diiodobenzene are dispersed in a mixed solution of dimethyl sulfoxide and water, and then sodium ascorbate and anhydrous copper sulfate are added as catalysts. The mixed solution is placed in a liquid nitrogen bath for freeze-thaw and cyclic degassing, and then sealed for solvothermal reaction to obtain a CuTEP-PPV-COF polymer. The reaction process is:

3. The preparation method according to claim 2, characterized in that: The molar ratio of the ligand 5,10,15,20-tetrakis(4-ethynylphenyl)porphyrin copper to 1,4-bis[(6-azidohexyl)oxy]-2,5-diiodobenzene is 1:1.8-2.2, preferably 1:2; Alternatively, in the mixed solution of dimethyl sulfoxide and water, the volume ratio of dimethyl sulfoxide to water is 1.8 to 2.2:1, preferably 2:

1.

4. The preparation method according to claim 2, characterized in that: The concentration of the ligand 5,10,15,20-tetrakis(4-ethynylphenyl)porphyrin copper in a mixed solution of dimethyl sulfoxide (DMSO) and water is 2-4 mmol / L, preferably 3 mmol / L; Alternatively, the molar ratio of the ligand 5,10,15,20-tetrakis(4-ethynylphenyl)porphyrin copper and sodium ascorbate to anhydrous copper sulfate is 5:0.8-1.2:0.8:-1.2, preferably 5:1:

1.

5. The preparation method according to claim 2, characterized in that: The temperature of the solvent thermal reaction is 110-130° C., preferably 120° C.; the time of the solvent thermal reaction is 90-100 h, preferably 94 h.

6. The preparation method according to claim 2, characterized in that: The preparation method of the ligand 5,10,15,20-tetrakis(4-ethynylphenyl)porphyrin copper comprises: (1) Compound 1 was dissolved in dichloromethane, and then pyrrole and boron trifluoride ether were added. After reacting at room temperature for 2 to 4 hours, tetrachlorobenzoquinone was added and reacted at 35 to 45° C. for 0.5 to 2 hours. After the reaction was completed, the solvent was removed and the compound 2 was obtained after purification; (2) Compound 2 and tetrabutylammonium fluoride were added to tetrahydrofuran, and the mixture was reacted at room temperature for 2 to 4 hours. After the reaction, water was added, and the filtrate was collected by filtration. The solvent was removed and dried to obtain compound 3; (3) dissolving copper acetate in methanol, adding the mixture together with compound 3 into dichloromethane, stirring and reacting at room temperature for 10 to 15 hours, and after the reaction, extracting with dichloromethane, washing with sodium bicarbonate solution, removing water and drying, and then rotary evaporating and drying to obtain 5,10,15,20-tetrakis(4-ethynylphenyl)porphyrin copper (CuTEP); 7. The preparation method according to claim 2, characterized in that: The preparation method of 1,4-bis[(6-azidohexyl)oxy]-2,5-diiodobenzene comprises: (1) Under N2 atmosphere, 1,4-diiodobenzene, 18-crown ether-6, 1,6-dibromohexane and K2CO3 were added to acetone and reacted at 75-85°C for 70-80 hours; after the reaction was completed, deionized water was added to quench the reaction, the product was extracted with dichloromethane, the organic phase was collected, the solvent was removed, and 1,4-bis[(6-bromohexyl)oxy]-2,5-diiodobenzene (PPV-Br) was obtained after purification; (2) PPV-Br and sodium azide are added to a mixed solution of N,N-dimethylacetamide, dichloromethane and water, and reacted at 85-95° C. for 10-14 hours. After the reaction is completed, the mixture is cooled to room temperature, ice water is added to the reaction solution, and the solid obtained by filtration is 1,4-bis[(6-azidohexyl)oxy]-2,5-diiodobenzene; The reaction process is:

8. The preparation method according to claim 7, characterized in that: In step (1), the molar ratio of 1,4-diiodobenzene, 18-crown ether-6, 1,6-dibromohexane and K2CO3 is 9-11:0.9-1.1:155-170:50-60, preferably 10:1:160:54; Alternatively, in step (2), the molar ratio of PPV-Br to sodium azide is 1:8 to 12, preferably 1:

10.

9. Use of the CuTEP-PPV-COF polymer according to claim 1 as a catalyst.

10. The use according to claim 9, characterized in that The application includes catalyzing the synthesis of benzaldehyde from benzyl alcohol.

Citation Information

Patent Citations

  • (R)-CuTAPBP-COF polymer as well as preparation method and application thereof

    CN113201108A

  • CuTEP-COF polymer as well as preparation method and application thereof

    CN117777416A