Preparation method of carbon black-carbon fiber hybrid reinforced shape memory composite material

By loading titanium dioxide on carbon black and combining with carbon fiber, a carbon black-carbon fiber hybrid shape memory composite material is prepared, which solves the problems of low mechanical properties and insufficient shape recovery in the prior art, and achieves high performance in the aerospace field Shape memory material.

CN118895006AInactive Publication Date: 2024-11-05金丰良
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411095844.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The application of existing shape memory materials in the aerospace field is limited by the problems of low mechanical properties and insufficient shape recovery. Especially polymer shape memory materials based on polymer materials and shape memory composite materials are not performed in this field. good.

Method used

By loading titanium dioxide on carbon black and combining with carbon fiber, a carbon black-carbon fiber hybrid enhanced shape memory composite material is prepared, and the mechanical properties and shape memory properties of the material are improved by using specific processing steps and chemical agent ratios. Specific steps include dispersing the carbon black in an organic solvent and loading titanium dioxide, modifying the carbon fiber, and impregnating it in the epoxy resin to cure to form the composite material.

Benefits of technology

It significantly improves the thermal response rate and mechanical properties of composite materials, enhances shape memory performance, and has wide application prospects in aerospace, automobiles and other fields. It also improves the interface bonding and wetting properties of the materials through modification treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895006A_ABST
    Figure CN118895006A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a carbon black-carbon fiber hybrid reinforced shape memory composite material, which comprises the following steps: dispersing carbon black in an organic solvent, then adding epoxy resin and a curing agent, and dissolving to obtain a matrix solution; carbon fibers are infiltrated into the matrix solution, heating and curing are carried out, and the carbon black-carbon fiber hybrid reinforced shape memory composite material is obtained. The carbon black adopted by the invention has excellent heat-conducting property, and the thermal response rate of the carbon fiber reinforced shape memory composite material can be remarkably improved by adding the carbon black into the carbon fiber reinforced shape memory composite material, so that the shape memory property of the composite material can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of shape memory materials, and in particular to a method for preparing a carbon black-carbon fiber hybrid reinforced shape memory composite material. Background Art

[0002] Shape memory materials refer to intelligent materials that can recover from their current form to their initial shape when subjected to external stimuli such as heat, electricity, magnetism, light, and humidity. They are widely used in biomedical materials, aerospace, automobiles, textiles, and self-repair. Common shape memory materials include shape memory alloys, shape memory polymers, and shape memory composites. Shape memory alloys have the advantages of small size, high strength, and a wide range of applications, but they have high manufacturing costs, limited recovery deformation, and large system vibrations when unfolded. Polymer-based shape memory materials (shape memory polymers) based on polymer materials have the advantages of large recoverable deformation, strong memory, light weight, and simple processing and molding, but the deformation recovery force is small, and the modulus and strength of the material are poor. These shortcomings affect their application, especially in aerospace applications. The shape memory composite material obtained by adding disordered short fibers and particle reinforcement materials to the polymer inherits the excellent shape memory properties of the shape memory polymer, but its mechanical properties are still low and cannot be used in the aerospace field. Therefore, it is necessary to develop a method for preparing a carbon black-carbon fiber hybrid reinforced shape memory composite material. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a carbon black-carbon fiber hybrid reinforced shape memory composite material to solve the problems existing in the above-mentioned prior art.

[0004] To achieve the above object, the present invention is implemented according to the following technical solutions:

[0005] In one aspect, the present invention comprises the following steps:

[0006] (1) After titanium dioxide is loaded on carbon black, the treated carbon black is dispersed in an organic solvent, wherein the mass ratio of the carbon black to the organic solvent is 1:(9-10), and then epoxy resin and curing agent are added, wherein the mass ratio of the carbon black, epoxy resin and curing agent is (5-8):(50-60):(18-20), and after dissolution, a matrix solution is obtained;

[0007] The loading method specifically includes:

[0008] Dispersing carbon black in water and adjusting the pH to 1 to 2 to obtain a carbon black solution;

[0009] Titanium tetrachloride is added to the carbon black solution, and ammonium sulfate is added after heating, and the solution is kept warm for a reaction. Then, the pH value is adjusted to 3.5-4.0 with ammonia water, and the solution is kept warm for a second reaction. Finally, the solution is washed, dried, and calcined to obtain carbon black loaded titanium dioxide.

[0010] (2) The modified carbon fiber is impregnated in a matrix solution, heated and cured to obtain the carbon black-carbon fiber hybrid reinforced shape memory composite material.

[0011] Furthermore, the temperature of the first insulation reaction is 45-50°C, and the time is 2-3h; the temperature of the second insulation reaction is 25-35°C, and the time is 1-2h; the temperature of the calcination is 600-650°C, and the time is 1-1.5h.

[0012] Furthermore, the mass ratio of the carbon black, titanium tetrachloride and ammonium sulfate is 5:1:3.

[0013] Furthermore, the epoxy resin is selected from any one of epoxy resin E-44, epoxy resin E51, and hydroxyethylated bisphenol A epoxy resin; the curing agent is selected from any one of 4,4-diaminodiphenylmethane, trimethylolpropane tris(3-mercaptopropionate), 4-methyl-metaphenylenediamine, and ethylenediamine; and the organic solvent is dichloromethane.

[0014] The carbon fiber modification treatment method specifically includes: dissolving a silane coupling agent in ethanol, adjusting the pH to 8.0-9.0, then adding carbon fiber, stirring continuously for 3-4 hours, taking out, and drying to obtain modified carbon fiber.

[0015] Furthermore, the mass ratio of the silane coupling agent to the carbon fiber is (1-1.5):(15-20).

[0016] Furthermore, the mass ratio of the epoxy resin to the carbon fiber is (50-60):(15-20); the heating curing specifically includes: first curing at 10-15°C for 8-10 hours, then curing at 140-160°C for 3-4 hours, and finally curing at 180-200°C for 0.5-1 hour.

[0017] Furthermore, the carbon black is carbon black N110; and the carbon fiber is carbon fiber T300B.

[0018] On the other hand, a carbon black-carbon fiber hybrid reinforced shape memory composite material prepared by the preparation method.

[0019] The beneficial effects of the present invention are:

[0020] The present invention is a decoction for invigorating qi, nourishing blood and promoting testicles. Compared with the prior art, the present invention has the following technical effects:

[0021] (1) Carbon black has excellent thermal conductivity. Adding carbon black to carbon fiber reinforced shape memory composites can significantly increase their thermal response rate, thereby improving the shape memory properties of the composites.

[0022] (2) The shape memory composite material prepared by the present invention using carbon black and carbon fiber as reinforcement not only has excellent mechanical properties, but also has good shape memory properties. This material has broad application prospects in the fields of aerospace, weapons and equipment, and automobile industry.

[0023] (3) The present invention further improves the mechanical properties and shape recovery rate of the shape memory composite material by loading titanium dioxide on the surface of carbon black; and the present invention modifies the carbon fiber to increase the contact area between the carbon fiber and the matrix solution, thereby improving the wettability and interfacial bonding strength of the carbon fiber and the epoxy resin, thereby significantly improving the mechanical properties of the shape memory composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The present invention is a schematic diagram of a process for preparing a carbon black-carbon fiber hybrid reinforced shape memory composite material. DETAILED DESCRIPTION

[0025] The present invention is further described below by means of specific embodiments. The illustrative embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.

[0026] like Figure 1 As shown, the carbon black used in the following embodiments and comparative examples of the present invention is carbon black N110, the carbon fiber is carbon fiber T300B, and the silane coupling agent is silane coupling agent KH550.

[0027] Example 1

[0028] A method for preparing a carbon black-carbon fiber hybrid reinforced shape memory composite material:

[0029] (1) 6 g of carbon black was dispersed in 500 mL of dichloromethane, and then 55 g of epoxy resin (epoxy resin E-44) and 18 g of curing agent (4,4-diaminodiphenylmethane) were added and dissolved to obtain a matrix solution.

[0030] (2) 18 g of carbon fiber was impregnated in the matrix solution, first cured at 12°C for 8 h, then cured at 150°C for 3.5 h, and finally cured at 180°C for 1 h to obtain a carbon black-carbon fiber hybrid reinforced shape memory composite material.

[0031] Example 2

[0032] A method for preparing a carbon black-carbon fiber hybrid reinforced shape memory composite material:

[0033] (1) Disperse 5 g of carbon black in 600 mL of dichloromethane, then add 60 g of epoxy resin (epoxy resin E51) and 20 g of curing agent (trimethylolpropane tris(3-mercaptopropionate)), and after dissolution, obtain a matrix solution.

[0034] (2) 15 g of carbon fiber was impregnated in the matrix solution, first cured at 10°C for 10 h, then cured at 160°C for 3 h, and finally cured at 180°C for 1 h to obtain a carbon black-carbon fiber hybrid reinforced shape memory composite material.

[0035] Example 3

[0036] A method for preparing a carbon black-carbon fiber hybrid reinforced shape memory composite material:

[0037] (1) Disperse 8 g of carbon black in 500 mL of dichloromethane, then add 50 g of epoxy resin (hydroxyethylated bisphenol A type epoxy resin) and 18 g of curing agent (4-methyl-metaphenylenediamine), and after dissolving, obtain a matrix solution.

[0038] (2) 20 g of carbon fiber was impregnated in the matrix solution, first cured at 15°C for 8 h, then cured at 140°C for 4 h, and finally cured at 200°C for 0.5 h to obtain a carbon black-carbon fiber hybrid reinforced shape memory composite material.

[0039] Example 4

[0040] A method for preparing a carbon black-carbon fiber hybrid reinforced shape memory composite material:

[0041] (1) Disperse 6 g of carbon black in 200 mL of water, adjust the pH to 1 with hydrochloric acid to obtain a carbon black solution; add 1.2 g of titanium tetrachloride to the carbon black solution, heat to 40°C, then add 3.6 g of ammonium sulfate, and carry out a heat preservation reaction (temperature is 45°C, time is 2.5 h), then adjust the pH to 4.0 with 9.5 g / 100 mL of ammonia water, carry out a second heat preservation reaction (temperature is 30°C, time is 2 h), finally filter, wash, and dry (60°C, 24 h), and calcine at a temperature of 600°C for 1.5 h to obtain carbon black-loaded titanium dioxide.

[0042] (2) All the carbon black-loaded titanium dioxide prepared in step (1) was dispersed in 500 mL of dichloromethane, and then 55 g of epoxy resin (epoxy resin E-44) and 18 g of curing agent (4,4-diaminodiphenylmethane) were added and dissolved to obtain a matrix solution.

[0043] (3) 18 g of carbon fiber was impregnated in the matrix solution, first cured at 12°C for 8 h, then cured at 150°C for 3.5 h, and finally cured at 180°C for 1 h to obtain a carbon black-carbon fiber hybrid reinforced shape memory composite material.

[0044] Example 5

[0045] The same as Example 4, except that step (1) is specifically as follows: 6 g of carbon black is dispersed in 200 mL of water, and the pH is adjusted to 2 with hydrochloric acid to obtain a carbon black solution; 1.2 g of titanium tetrachloride is added to the carbon black solution, heated to 40°C, and then 3.6 g of ammonium sulfate is added, and a heat preservation reaction is carried out once (temperature is 50°C, time is 2h), and then the pH is adjusted to 3.5 with ammonia water having a concentration of 9.5 g / 100 mL, and a second heat preservation reaction is carried out (temperature is 35°C, time is 1h), and finally filtered, washed, and dried (60°C, 24h), and calcined at a temperature of 650°C for 1h to obtain carbon black-loaded titanium dioxide.

[0046] Example 6

[0047] A method for preparing a carbon black-carbon fiber hybrid reinforced shape memory composite material:

[0048] (1) 6 g of carbon black was dispersed in 500 mL of dichloromethane, and then 55 g of epoxy resin (epoxy resin E-44) and 18 g of curing agent (4,4-diaminodiphenylmethane) were added and dissolved to obtain a matrix solution.

[0049] (2) Dissolve 1 g of silane coupling agent in 100 mL of ethanol at 70° C., adjust the pH to about 8.5, then add 18 g of carbon fiber, continue stirring for 4 h, take out, and dry to obtain modified carbon fiber.

[0050] (3) The modified carbon fiber prepared in step (2) is completely impregnated in the matrix solution prepared in step (1), first cured at 12° C. for 8 h, then cured at 150° C. for 3.5 h, and finally cured at 180° C. for 1 h to obtain a carbon black-carbon fiber hybrid reinforced shape memory composite material.

[0051] Example 7

[0052] The same as Example 6, except that step (2) is specifically as follows: dissolve 1.5 g of silane coupling agent in 100 mL of ethanol at 70° C., adjust the pH to about 9.0, then add 18 g of carbon fiber, continue stirring for 3 hours, take out, and dry to obtain modified carbon fiber.

[0053] Example 8

[0054] A method for preparing a carbon black-carbon fiber hybrid reinforced shape memory composite material:

[0055] (1) Disperse 6 g of carbon black in 200 mL of water, adjust the pH to 1 with hydrochloric acid to obtain a carbon black solution; add 1.2 g of titanium tetrachloride to the carbon black solution, heat to 40°C, then add 3.6 g of ammonium sulfate, and carry out a heat preservation reaction (temperature is 45°C, time is 2.5 h), then adjust the pH to 4.0 with 9.5 g / 100 mL of ammonia water, carry out a second heat preservation reaction (temperature is 30°C, time is 2 h), finally filter, wash, and dry (60°C, 24 h), and calcine at a temperature of 600°C for 1.5 h to obtain carbon black-loaded titanium dioxide.

[0056] (2) All the carbon black-loaded titanium dioxide prepared in step (1) was dispersed in 500 mL of dichloromethane, and then 55 g of epoxy resin (epoxy resin E-44) and 18 g of curing agent (4,4-diaminodiphenylmethane) were added and dissolved to obtain a matrix solution.

[0057] (3) Dissolve 1 g of silane coupling agent in 100 mL of ethanol at 70° C., adjust the pH to about 8.5, then add 18 g of carbon fiber, continue stirring for 4 h, take out, and dry to obtain modified carbon fiber.

[0058] (4) The modified carbon fiber prepared in step (3) is completely impregnated in the matrix solution prepared in step (2), first cured at 12°C for 8 hours, then cured at 150°C for 3.5 hours, and finally cured at 180°C for 1 hour to obtain a carbon black-carbon fiber hybrid reinforced shape memory composite material.

[0059] Comparative Example 1

[0060] The same as Example 1, except that the carbon black in step (1) is replaced by carbon nanotubes (Fuller tubes) of equal mass.

[0061] Comparative Example 2

[0062] The same as Example 1, except that the carbon fiber in step (2) is replaced by ceramic fiber (ceramic fiber 1600) of equal mass.

[0063] Comparative Example 3

[0064] The same as Example 1, except that step (2) is specifically as follows: 18 g of carbon fiber is impregnated in the matrix solution, and cured at 150° C. for 6 h to obtain a carbon black-carbon fiber hybrid reinforced shape memory composite material.

[0065] Comparative Example 4

[0066] Same as Example 8, except that the silane coupling agent in step (3) is replaced with an equal mass of titanate coupling agent 201.

[0067] Effect Example 1

[0068] The properties of the shape memory composite materials prepared in Examples 1 to 8 of the present invention and Comparative Examples 1 to 4 were measured, and the results are shown in Table 1.

[0069] (1) Mechanical properties

[0070] The tensile strength and elongation at break were measured on a universal tensile testing machine according to GB1040-79 standard, with a tensile speed of 50 mm / min.

[0071] (2) Shape retention and recovery rate

[0072] The shape memory composite materials prepared in Examples 1 to 8 and Comparative Examples 1 to 4 were cut into a size of 20×10×2 mm, and the transition temperature was determined to be Tr. The shape memory composite materials were heated to Tr+20°C, and stretched at a stretching rate of 10 mm / min until the deformations reached 100%, 300% and 500%, respectively. The displacement was fixed at a constant temperature for 5 minutes, at which point the maximum deformation m was reached. The temperature was then lowered to Tr-20°C and maintained for 5 minutes. The unloading force was zero, and the deformation u was recorded at this time. The temperature was set again to keep the sample stress at zero, and the recovery deformation p was recorded when the temperature was raised to Tr+20°C. Four cycles were repeated and the average value was calculated. Shape retention rate (R f ) and shape recovery rate (R r )The formula is as follows:

[0073]

[0074] Table 1 Properties of shape memory composites

[0075]

[0076]

[0077] It can be seen from Table 1 that the shape memory composite material with the best performance can be obtained by loading carbon dioxide on carbon black and modifying carbon fiber. The excellent performance of the shape memory composite material of the present invention is achieved by the combined effect of raw materials and preparation method.

[0078] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a carbon black-carbon fiber hybrid reinforced shape memory composite material, characterized in that: The following steps are involved: (1) After titanium dioxide is loaded on carbon black, the treated carbon black is dispersed in an organic solvent, wherein the mass ratio of the carbon black to the organic solvent is 1:(9-10), and then epoxy resin and curing agent are added, wherein the mass ratio of the carbon black, epoxy resin and curing agent is (5-8):(50-60):(18-20), and after dissolution, a matrix solution is obtained; The loading method specifically includes: Dispersing carbon black in water and adjusting the pH to 1 to 2 to obtain a carbon black solution; Titanium tetrachloride is added to the carbon black solution, and ammonium sulfate is added after heating, and the reaction is carried out by heat preservation once, and then the pH is adjusted to 3.5-4.0 with ammonia water, and the reaction is carried out by heat preservation twice, and finally washing, drying and calcining are carried out to obtain carbon black loaded carbon dioxide; (2) The modified carbon fiber is impregnated in a matrix solution, heated and cured to obtain the carbon black-carbon fiber hybrid reinforced shape memory composite material.

2. The preparation method according to claim 1, characterized in that: The temperature of the first insulation reaction is 45-50°C, and the time is 2-3h; the temperature of the second insulation reaction is 25-35°C, and the time is 1-2h; the temperature of the calcination is 600-650°C, and the time is 1-1.5h.

3. The preparation method according to claim 1, characterized in that: The mass ratio of the carbon black, titanium tetrachloride and ammonium sulfate is 5:1:

3.

4. The preparation method according to claim 1, characterized in that: The epoxy resin is selected from any one of epoxy resin E-44, epoxy resin E51, and hydroxyethylated bisphenol A epoxy resin; the curing agent is selected from any one of 4,4-diaminodiphenylmethane, trimethylolpropane tris(3-mercaptopropionate), 4-methyl-metaphenylenediamine, and ethylenediamine; and the organic solvent is dichloromethane.

5. The preparation method according to claim 1, characterized in that: The carbon fiber modification treatment method specifically includes: dissolving a silane coupling agent in ethanol, adjusting the pH to 8.0-9.0, then adding carbon fiber, continuously stirring for 3-4 hours, taking out, and drying to obtain modified carbon fiber.

6. The preparation method according to claim 5, characterized in that: The mass ratio of the silane coupling agent to the carbon fiber is (1-1.5):(15-20).

7. The preparation method according to claim 1, characterized in that: The mass ratio of the epoxy resin to the carbon fiber is (50-60):(15-20); the heating curing specifically includes: first curing at 10-15°C for 8-10 hours, then curing at 140-160°C for 3-4 hours, and finally curing at 180-200°C for 0.5-1 hour.

8. A carbon black-carbon fiber hybrid reinforced shape memory composite material prepared by the preparation method according to any one of claims 1 to 7.