Compression-resistant and folding-resistant hydrophilic three-dimensional fiber aerogel and preparation method thereof

Through the combination of gelatin and polymer matrix, electrospinning and crosslinking technology, a hydrophilic three-dimensional fiber aerogel that is resistant to compression and folding is prepared, solving the insufficient structure and hydrophilicity of existing fiber materials. Problem, effective application in tissue engineering and disease treatment.

CN118895054APending Publication Date: 2024-11-05SHANGHAI RUINING BIOTECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411058111.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing fiber materials are difficult to form suitable three-dimensional structures, cannot effectively fill, isolate or protect tissues, and lack toughness and hydrophilicity, limiting their application in tissue engineering and disease treatment.

Method used

Micro- or nano-scale fibers are prepared by electrospinning process using a combination of gelatin and polymer matrix, combined with homogenization dispersion-freeze-drying-high-temperature cross-linking and chemical cross-linking to form three-dimensional fibers with excellent hydrophilic properties and mechanical toughness. Aerogel.

Benefits of technology

The compression and folding resistance of three-dimensional fiber aerogel is achieved, which meets the needs of biomedical experiments, and improves the hydrophilicity and mechanical properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention relates to the field of aerogel (IPC classification number: B01J), in particular to compression-resistant and folding-resistant hydrophilic three-dimensional fiber aerogel and a preparation method thereof. The preparation raw materials of the aerogel at least comprise a high polymer material; the high polymer material is a combination of gelatin and a polymer base material; the mass ratio of the gelatin to the polymer base material is (1-10): 1. The three-dimensional fiber aerogel provided by the invention has excellent hydrophilic performance, small water contact angle and good wettability; after being compressed and folded for multiple times, the three-dimensional fiber aerogel can still maintain the complete appearance, and the operation requirements during biomedical experiment use can be met; the aerogel material prepared by the invention is safe and environment-friendly, has excellent compression resistance, folding resistance and good hydrophilicity, is simple and convenient in preparation process and wide in method selectivity, and has a very good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of aerogels (IPC classification number: B01J), and in particular to a compression-resistant and folding-resistant hydrophilic three-dimensional fiber aerogel and a preparation method thereof. Background Art

[0002] Research has found that three-dimensional fiber materials can largely mimic the environment of the natural extracellular matrix, allowing cells to maintain a moist environment while proliferating, growing, and migrating within a three-dimensional porous structure similar to natural tissue. This helps improve tissue pathology, promote tissue regeneration, and ultimately alleviate and treat diseases. Based on the properties of three-dimensional fiber materials, developing three-dimensional fiber materials with high water absorption, fiber structures similar to the natural extracellular matrix, and good cell compatibility is extremely important in the fields of tissue engineering and medicine.

[0003] However, most existing fiber materials are one-dimensional bundles or two-dimensional membranes, which are difficult to form suitable three-dimensional structures to match the physicochemical properties of tissues, resulting in their inability to effectively fill, isolate or protect tissues. Taking fibers prepared by electrospinning as an example, electrospinning is a commonly used and effective fiber preparation method that can stably prepare micron or nanofiber membrane materials in large quantities. However, the above-mentioned fiber materials have some typical characteristics, such as a narrow fiber diameter distribution and a high specific surface area of ​​the membrane. Most electrospun fiber membranes are not suitable for direct use in tissue engineering or disease treatment. The main reasons are: 1. Conventional fiber membranes are thin and cannot provide effective support and protection to cover, fill or isolate tissues; 2. The method of increasing the thickness of conventional fiber membranes by long-term spinning often leads to serious material stratification due to uneven solvent evaporation on the surface of the fiber membrane, which can easily cause material structure and performance defects; 3. Conventional fiber membranes have dense fibers and small pores, which are not conducive to the penetration and exchange of gases and liquids; 4. Two-dimensional membrane materials can easily cause adverse effects on cells. For example, cells cannot form aggregates or cell clusters on two-dimensional membranes, cell-cell and cell-matrix interactions are missing, and cell polarity and function are weakened or inhibited. This also greatly limits the application of fiber materials in the in vivo environment. Therefore, it is very necessary to develop three-dimensional fiber aerogel materials.

[0004] In addition, medical applications such as tissue engineering or disease treatment have certain requirements for the hydrophilicity of three-dimensional fiber materials. Most hydrophilic materials have good biocompatibility, high water absorption, material exchange capacity, cell adhesion and a certain degree of antibacterial properties. At the same time, hydrophilicity is beneficial to promote wound healing, improve drug utilization and reduce thrombosis. However, for the sake of material mechanics, most fiber materials contain a high proportion of artificial polymers, which often reduces the hydrophilicity of the fiber materials and is not conducive to medical applications. Therefore, for fiber materials in the medical field, hydrophilicity is also a very important challenging indicator. In addition, due to the difficulty in forming tight connections between fibers, the mechanical properties of three-dimensional fiber materials are often insufficient, resulting in a lack of toughness of the three-dimensional fiber materials, which are easily broken when folded or compressed and cannot meet the needs of surgical operations. Existing fiber materials cannot meet the needs of the medical field well.

[0005] Finally, the current process for manufacturing three-dimensional fiber aerogels remains a major challenge. At present, the methods for preparing electrospun 3D nanofiber aerogels can be listed as multilayer electrospinning, liquid-assisted collection, template-assisted collection, addition of porogens, self-assembly and post-processing. The above technologies all have disadvantages and limitations, such as: multilayer electrospinning and liquid-assisted collection are time-consuming processes, and the ambient humidity, spinning rate and receiving distance during the spinning process will cause changes in fiber diameter or beading (caused by poor solvent volatilization), which will affect the structure and properties of the final material; template-assisted collection usually requires specific collectors or complex techniques; porogens such as salts need to be washed away; self-assembly often requires specific conditions (such as solution viscosity, collectors, electrostatic fields) to prepare three-dimensional fiber aerogels. These shortcomings also limit the use of three-dimensional fiber aerogels.

[0006] Chinese patent CN117258780A discloses a preparation method and application of electrospun Ag-loaded SiO2 nanofiber aerogel. The Ag-loaded SiO2 nanofiber aerogel imparts high porosity and surface area to the material, improving the aerogel's adsorption efficiency and reactivity. Chinese patent CN116212111B discloses a gelatin-polycaprolactone protein peptide composite aerogel for cartilage repair and its preparation method. By introducing gelatin and polycaprolactone electrospun materials, the original morphology of the collagen peptide is altered, forming a unique nano-network structure that promotes cartilage regeneration. However, these existing technologies still fail to simultaneously address the aforementioned technical issues.

[0007] Based on this, providing a three-dimensional fiber aerogel with simple process, good material mechanical properties and strong hydrophilicity has become a technical problem to be solved urgently in this field. Summary of the Invention

[0008] The first aspect of the present invention provides a compression-resistant and folding-resistant hydrophilic three-dimensional fiber aerogel, the preparation raw materials of which include at least a polymer material; the polymer material is a combination of gelatin and a polymer base material; the mass ratio of the gelatin to the polymer base material is (1-10):1, which can be listed as 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1.

[0009] Preferably, the mass ratio of the gelatin to the polymer base is (2-8):1; more preferably (4-6):1.

[0010] In some preferred embodiments, the polymer base material includes at least one of polylactic acid (PLA), polyglycolic acid (PGA), polycaprolactone (PCL), polyethylene oxide (PEO), polyvinyl alcohol (PVA), polymethyl methacrylate (PMMA), polyetheretherketone (PEEK), polyethersulfone (PES), and polyimide (PI).

[0011] Preferably, the gelatin has a gel strength of ˜100 g Bloom.

[0012] Preferably, the intrinsic viscosity of the polylactic acid is 0.2-5 dL / g.

[0013] In order to solve the above problems, the present invention preferably uses gelatin and materials such as PLA and PCL as aerogel raw materials, prepares micron or nanometer-scale fibers through an electrospinning process, and then uses slurry dispersion-freeze drying-high-temperature crosslinking and chemical crosslinking to obtain a three-dimensional fiber aerogel with significantly improved performance. The obtained three-dimensional fiber aerogel has excellent hydrophilic properties, a small water contact angle, and good wettability; and after multiple compressions and foldings, the three-dimensional fiber aerogel can still maintain its complete shape, which can meet the operational requirements when used in biomedical experiments. The obtained material forms a gelatin / polymer network with a suitable pore structure, which can give the aerogel good surface activity. The capillary effect inside the aerogel can make the material hydrophilic. At the same time, the fiber material enhances the aerogel's ability to resist external stress, improves its mechanical toughness, and can still return to its original shape after being compressed and folded by external forces, and has excellent shape memory properties.

[0014] The second aspect of the present invention provides a method for preparing a compression-resistant and folding-resistant hydrophilic three-dimensional fiber aerogel, the specific preparation steps comprising:

[0015] S1. dissolving a polymer material in a solvent to prepare an electrospinning solution;

[0016] S2. Preparing a first fiber material by an electrospinning process;

[0017] S3. The first fiber material is fragmented and mixed with the dispersion for homogenization; and then freeze-dried to obtain a second fiber material;

[0018] S4. Take the second fiber material and perform high-temperature cross-linking to obtain a first cross-linked product;

[0019] S5. Taking the first cross-linked product and chemically cross-linking it to obtain a second cross-linked product;

[0020] S6. freeze-drying the second cross-linked product to obtain a finished hydrophilic three-dimensional fiber aerogel.

[0021] Preferably, the solvent in step S1 is a highly polar solvent, which may be hexafluoroisopropanol, methanol, ethanol, propanol, acetonitrile, trifluoroethanol and acetic acid, etc.; more preferably, it is a combination of hexafluoroisopropanol or trifluoroethanol and acetic acid.

[0022] In some preferred embodiments, the total concentration of the polymer material in the electrospinning solution is 8wt%-20wt%; it can be listed as 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%.

[0023] In some preferred embodiments, the conditions of the electrospinning process in step S2 are set as follows: voltage 8-30 kV, receiving distance 5-20 cm, flow rate 1-10 mL / h, and humidity 30%-80%.

[0024] Preferably, the propulsion rate of the electrospinning solution is 0.5-5 mL / h; more preferably, the propulsion rate is 2 mL / h.

[0025] In some preferred embodiments, the fragmentation in step S3 is specifically as follows: cutting the first fiber material into pieces of 0.1-5 cm 2 The size of the fragments; for example, 0.5cm×0.5cm, 2cm×2cm pieces.

[0026] In some preferred embodiments, the homogenization process in step S3 is specifically as follows: a rotation speed of 8000-15000 rpm, and a homogenization time of 20-50 min, more preferably a rotation speed of 12000 rpm, and a homogenization time of 30 min.

[0027] In some embodiments, the dispersion in step S3 can be flexibly selected as an inorganic phase or an organic phase according to needs.

[0028] The inorganic phase may be pure water, buffer solution, etc.

[0029] Examples of buffers include, but are not limited to, phosphate buffer systems, acetate buffer systems, glycine buffer systems, and citric acid buffer systems.

[0030] The organic phase is preferably an alcohol solvent, such as tert-butanol, ethanol, propanol, etc.

[0031] Preferably, the dispersion liquid is ice water.

[0032] In some preferred embodiments, the mixing ratio of the first fiber material and the dispersion is (1-10) g / 200 mL, preferably 5 g / 200 mL.

[0033] In some preferred embodiments, the temperature of the high-temperature cross-linking in step S4 is set to be in the range of 0-50° C. higher than the melting point of the polymer.

[0034] More preferably, the high-temperature cross-linking conditions in step S4 are: 50-300° C. for 0.5-4 h; preferably 160-240° C. for 1-3 h.

[0035] More preferably, the high temperature cross-linking condition is: 200° C. for 1.5 h.

[0036] In some preferred embodiments, the chemical crosslinking in step S5 is specifically as follows: immersing the first crosslinked product in a pre-crosslinking agent for 0.2-4 hours, then adding a chemical crosslinking agent and stirring for 0.2-4 hours, and washing with distilled water to obtain a second crosslinked product.

[0037] More preferably, the adding of the chemical crosslinking agent and stirring in step S5 are carried out in two steps: first, the first chemical crosslinking agent is added and stirred for 0.5-2 hours, and then the second chemical crosslinking agent is added and stirred for 1-3 hours.

[0038] In some preferred embodiments, the pre-crosslinking agent is an aqueous solution of a macromolecular substance; the macromolecular substance includes at least one of hyaluronic acid, silk fibroin, chitosan, cellulose, chondroitin, heparin, gum arabic, xanthan gum, pectin, and guar gum; preferably hyaluronic acid.

[0039] Preferably, the concentration of the macromolecular substance in the pre-crosslinking agent is 1-10 wt %.

[0040] In some preferred embodiments, the molecular weight of the hyaluronic acid is 1*10 5 -2*10 6 kDa.

[0041] Preferably, when the macromolecular substance is hyaluronic acid, the concentration of hyaluronic acid in the pre-crosslinking agent is 2-4 wt %.

[0042] In some preferred embodiments, the first chemical cross-linking agent and the second chemical cross-linking agent are independently selected from any one of EDC (1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride)), NHS (N-hydroxysuccinimide), GA (glutaraldehyde), and ET (ethanol).

[0043] Preferably, the first chemical cross-linking agent is EDC; preferably, the second chemical cross-linking agent is NHS.

[0044] To enhance crosslinking, the present invention preferably employs high-temperature crosslinking followed by chemical crosslinking to achieve an internally homogeneous and stable crosslinked product. Furthermore, the present invention offers significant flexibility in controlling crosslinking conditions. High-temperature crosslinking requires only controlling the crosslinking temperature to 0-50°C above the polymer melting point to achieve efficient crosslinking, ultimately yielding a hydrophilic, compression-resistant, and folding-resistant three-dimensional fiber aerogel.

[0045] The electrospinning can be carried out by methods commonly used in the art, and can also be carried out by liquid-assisted collection, template-assisted collection, addition of porogens, self-assembly, and the like.

[0046] A third aspect of the present invention provides the use of the hydrophilic three-dimensional fiber aerogel or its preparation method as described above. The compression-resistant and folding-resistant hydrophilic three-dimensional fiber aerogel and its preparation method are used to prepare biomedical materials.

[0047] Beneficial effects:

[0048] On the one hand, the three-dimensional fiber aerogel provided by the present invention has excellent hydrophilic properties, a small water contact angle, and good wettability; and after multiple compressions and foldings, the three-dimensional fiber aerogel can still maintain its complete shape, which can meet the operational requirements when used in biomedical experiments; the aerogel material prepared by the present invention is safe and environmentally friendly and has excellent compression resistance, folding resistance, and good hydrophilicity, and has high practical value.

[0049] On the other hand, the method for preparing three-dimensional fiber aerogels of the present invention has universal applicability, which is mainly reflected in the following aspects: (1) in the preparation of fiber materials, the present invention has a wider range of preparation methods than conventional fiber spinning, and can use various methods such as electrospinning, liquid-assisted collection, template-assisted collection, addition of porogens, self-assembly and post-treatment to obtain fiber materials. (2) in the electrospinning step, the present invention has a wider range of requirements for the control of spinning conditions than conventional fiber spinning, and can use fiber materials under adverse conditions such as high ambient humidity and high spinning rate. (3) in the slurry dispersion step, the present invention has a wider range of requirements for the solvent used than conventional methods, and can use any solvent including water, buffer or organic solvent. (4) in the high-temperature crosslinking step, the present invention has a wider range of requirements for the treatment temperature than conventional methods, and can use a temperature range of 160°C-240°C for treatment, and the treatment time of high-temperature crosslinking can be adjusted according to needs. (5) In the chemical crosslinking step, the present invention allows for a wider range of crosslinking materials than conventional materials, and can use a variety of materials including hyaluronic acid, silk fibroin, chitosan, cellulose, chondroitin, heparin, gum arabic, xanthan gum, and pectin. It is applicable to fibers prepared from a variety of materials and by different methods. (6) The method for preparing aerogels of the present invention is simple, easy to implement, and has a very high application prospect. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 Figure 1 shows the preparation of the hydrophilic three-dimensional fiber aerogel according to Example 1; (a is a gelatin / polylactic acid fiber membrane, b is a membrane fragment, c is a dispersion, d is a second fiber material, e is a thermally cross-linked aerogel, f is a chemically cross-linked aerogel, and g is a finished hydrophilic three-dimensional fiber aerogel)

[0051] Figure 2 Scanning electron micrograph of the hydrophilic three-dimensional fiber aerogel of Example 1; (a in the figure is a gelatin / polylactic acid fiber membrane, b is a dispersion, c is a second fiber material, d is a thermally cross-linked aerogel, and e is a chemically cross-linked aerogel)

[0052] Figure 3 Water contact angle test of the hydrophilic three-dimensional fiber aerogel of Example 1;

[0053] Figure 4 Compression folding diagram of the product of step S3 of Example 1 (uncrosslinked aerogel); (from left to right: raw material, folded 0°, folded 90°, folded 180°, and released aerogel state)

[0054] Figure 5Compression folding diagram of the product (cross-linked aerogel) of step S6 of Example 1; (from left to right: raw material, folded 0°, folded 90°, folded 180°, and aerogel state upon release)

[0055] Figure 6 Effect of different molecular weights of hyaluronic acid on solution viscosity in Example 1 and Example 2; (the left figure is Example 2, the right figure is Example 1)

[0056] Figure 7 Example 3 Fourier infrared images of hydrophilic three-dimensional fiber aerogel and gelatin and pure polycaprolactone; (red line: Example 3, black line: polycaprolactone, blue line: gelatin)

[0057] Figure 8 . Example 3 material compression folding diagram see Figure 8 ; (In the figure, a is gelatin / polycaprolactone fiber membrane, b is the three-dimensional fiber aerogel product, c is the material sample before immersion in liquid (the liquid is water), d is the material sample at t=0s, e is the material sample at t=2s, f is the material sample at t=4s (top view), and g is the material sample at t=4s (main view)). DETAILED DESCRIPTION

[0058] Example 1

[0059] This embodiment provides a compression-resistant and folding-resistant hydrophilic three-dimensional fiber aerogel, and its preparation method and application. The raw materials for preparing the fiber aerogel are polymer materials, specifically gelatin and PLA (L-lactic acid) in a mass ratio of 4:1.

[0060] The gelatin is porcine gelatin with a gel strength of 100g Bloom, sourced from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0061] The PLA has an intrinsic viscosity of 0.8-1.5 dL / g and is sourced from Suzhou Qihang Biotechnology Co., Ltd.

[0062] The preparation method of the hydrophilic three-dimensional fiber aerogel specifically comprises the following steps:

[0063] S1. The polymer material was dissolved in a solvent (hexafluoroisopropanol) at a concentration of 15 wt% to prepare an electrospinning solution;

[0064] S2. Prepare a first fiber material by an electrospinning process. Specifically, the electrospinning solution was drawn into a syringe, the syringe pump was controlled to advance at a rate of 2 mL / h, a high voltage of 20 kV was connected to the syringe needle, and the prepared fiber material was received using aluminum foil at a receiving distance of 10 cm. The ambient humidity was 30%. After spinning, the solvent was evaporated in a fume hood overnight to obtain the first fiber material (gelatin / polylactic acid fiber membrane).

[0065] S3. The first fiber material was cut into 2 cm × 2 cm fragments. 5 g of the fragments were mixed with 200 mL of a dispersion solution (ice water) and homogenized in a high-speed mill at 12,000 rpm for 30 min to pulverize the fiber membrane into a uniform dispersion (short fiber) solution. The short fiber solution was transferred to a mold and frozen at -80°C overnight, followed by freeze-drying for 48 h to obtain a second fiber material.

[0066] S4. The second fiber material was cross-linked at high temperature, specifically by heating in an oven at 200°C for 1.5 hours, followed by natural cooling to obtain a first cross-linked product (thermally cross-linked aerogel);

[0067] S5. The first cross-linked product was chemically cross-linked by immersing the first cross-linked product in a pre-cross-linking agent (a 2 wt % hyaluronic acid aqueous solution) for 2 h, then adding EDC and stirring for 0.5 h, followed by adding NHS and stirring for 2 h, and washing with distilled water to obtain a second cross-linked product (chemically cross-linked aerogel);

[0068] S6. freeze-drying the second cross-linked product to obtain a finished hydrophilic three-dimensional fiber aerogel.

[0069] The molecular weight of the hyaluronic acid is 150w, and it comes from Liyang Bio.

[0070] Example 2

[0071] This embodiment provides a compression-resistant and folding-resistant hydrophilic three-dimensional fiber aerogel and its preparation method and application. The specific implementation method is the same as that of Example 1; the difference is that the molecular weight of the hyaluronic acid is 20w and is sourced from Shandong Liyang Biotechnology Co., Ltd.

[0072] Example 3

[0073] This embodiment provides a compression-resistant and folding-resistant hydrophilic three-dimensional fiber aerogel, and a preparation method and application thereof. The raw materials for preparing the fiber aerogel are polymer materials, specifically gelatin and PCL (polycaprolactone) in a mass ratio of 2:1.

[0074] The gelatin is porcine gelatin with a gel strength of 100g Bloom, sourced from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0075] The molecular weight of the PCL is 8w, and it is sourced from Suzhou Qihang Biotechnology Co., Ltd.

[0076] The preparation method of the hydrophilic three-dimensional fiber aerogel specifically comprises the following steps:

[0077] S1. The polymer material was dissolved in a solvent (trifluoroethanol and acetic acid in a volume ratio of 500:1) at a concentration of 10 wt% to prepare an electrospinning solution;

[0078] S2. Prepare a first fiber material by an electrospinning process. Specifically, the electrospinning solution was drawn into a syringe, the syringe pump was controlled to advance at a rate of 3 mL / h, a high voltage of 20 kV was connected to the syringe needle, and the prepared fiber material was received using aluminum foil at a receiving distance of 15 cm. The ambient humidity was 30%. After spinning, the solvent was evaporated in a fume hood overnight to obtain the first fiber material (gelatin / polycaprolactone fiber membrane).

[0079] S3. The first fiber material was cut into 2 cm × 2 cm fragments. 5 g of the fragments were mixed with 200 mL of a dispersion solution (ice water) and homogenized in a high-speed grinder at 12,000 rpm for 30 min to pulverize the fiber membrane into a uniform short fiber solution. The short fiber solution was transferred to a mold and frozen at -80°C overnight, followed by freeze-drying for 48 h to obtain a second fiber material.

[0080] S4. Take the second fiber material and perform high-temperature crosslinking, specifically heating in an oven at 70°C for 2 hours, followed by natural cooling to obtain a first crosslinked product;

[0081] S5. The first cross-linked product was chemically cross-linked by immersing the first cross-linked product in a pre-cross-linking agent (a 2 wt % hyaluronic acid aqueous solution) for 2 h, then adding EDC and stirring for 0.5 h, followed by adding NHS and stirring for 2 h, and then washing with distilled water to obtain a second cross-linked product;

[0082] S6. freeze-drying the second cross-linked product to obtain a finished hydrophilic three-dimensional fiber aerogel.

[0083] The molecular weight of the hyaluronic acid is 150w, and it is sourced from Shandong Liyang Biotechnology Co., Ltd.

[0084] Performance Testing

[0085] 1. Physical picture: The physical picture of the hydrophilic three-dimensional fiber aerogel preparation of Example 1 is shown in Figure 1 ; The hydrophilic three-dimensional fiber aerogel scanning electron microscope image of Example 1 is shown in Figure 2 .

[0086] 2. Hydrophilicity: The water contact angle test of the hydrophilic three-dimensional fiber aerogel in Example 1 is shown in Figure 3 ;from Figure 3 It can be seen that the three-dimensional fiber aerogel has good hydrophilicity, and the water contact angle has become 0° at 2.5s.

[0087] 3. Compression and folding resistance: The compression and folding diagram of the product (uncrosslinked aerogel) in step S3 of Example 1 is shown in Figure 4 The compressed folding diagram of the product (cross-linked aerogel) of step S6 of Example 1 is shown in FIG. Figure 5 By comparison, it can be seen that the uncross-linked aerogel will break and fracture after being folded 180°; while the aerogel can return to its original shape after high-temperature chemical cross-linking, and has excellent compression and folding resistance.

[0088] 4. The effect of different molecular weights of hyaluronic acid on solution viscosity in Example 1 and Example 2 is shown in Figure 6 ;pass Figure 6 It can be seen that the effects of the first cross-linked product being immersed in hyaluronic acid of different molecular weights are significantly different; after the aerogel is immersed in a low molecular weight hyaluronic acid aqueous solution, the material wetting and cross-linking effects are good, while after being immersed in a high molecular weight hyaluronic acid aqueous solution, hyaluronic acid can hardly penetrate into the aerogel.

[0089] 5. Example 3: Fourier transform infrared images of hydrophilic three-dimensional fiber aerogel, gelatin and PCL pure products Figure 7 .from Figure 7 It can be seen from the characteristic peaks in Figure 3 that the hydrophilic three-dimensional fiber aerogel finally obtained in Example 3 already contains the characteristic peaks of gelatin and PCL (located at 3100-3400 and 1600-1800, respectively). It can be seen that gelatin and PCL have been effectively combined in the hydrophilic three-dimensional fiber aerogel material.

[0090] 6. The compression folding diagram of the material in Example 3 is shown in Figure 8 ,from Figure 8 It can be seen that gelatin / PCL fiber aerogel has good resistance to compression and folding.

Claims

1. A compression-resistant and folding-resistant hydrophilic three-dimensional fiber aerogel, wherein the raw materials for preparation include at least a polymer material; characterized in that: The polymer material is a combination of gelatin and a polymer base material; the mass ratio of the gelatin to the polymer base material is (1-10):

1.

2. The compression-resistant and folding-resistant hydrophilic three-dimensional fiber aerogel according to claim 1, characterized in that: The polymer base material includes at least one of polylactic acid, polyglycolic acid, polycaprolactone, polyethylene oxide, polyvinyl alcohol, polymethyl methacrylate, polyetheretherketone, polyethersulfone and polyimide.

3. A method for preparing the compression-resistant and folding-resistant hydrophilic three-dimensional fiber aerogel according to claim 1 or 2, characterized in that: The specific preparation steps of the hydrophilic three-dimensional fiber aerogel include: S1. dissolving the polymer material in a solvent to prepare an electrospinning solution; S2. Preparing a first fiber material by an electrospinning process; S3. The first fiber material is fragmented, mixed with the dispersion and homogenized; and then freeze-dried to obtain a second fiber material; S4. Taking the second fiber material and cross-linking it at high temperature to obtain a first cross-linked product; S5. Taking the first cross-linked product and chemically cross-linking it to obtain a second cross-linked product; S6. freeze-drying the second cross-linked product to obtain a hydrophilic three-dimensional fiber aerogel product.

4. The method for preparing the compression-resistant and folding-resistant hydrophilic three-dimensional fiber aerogel according to claim 1, characterized in that: The conditions of the electrospinning process in step S2 are set as follows: voltage 8-30 kV, receiving distance 5-20 cm, flow rate 1-10 mL / h, and humidity 30%-80%.

5. The method for preparing the compression-resistant and folding-resistant hydrophilic three-dimensional fiber aerogel according to claim 1, characterized in that: The high temperature cross-linking conditions in step S4 are: 50-300° C. for 0.5-4 h.

6. The method for preparing the compression-resistant and folding-resistant hydrophilic three-dimensional fiber aerogel according to claim 1, characterized in that: The chemical crosslinking in step S5 is specifically as follows: immersing the first crosslinked product in a pre-crosslinking agent for 0.2-4 hours, then adding a chemical crosslinking agent and stirring for 0.2-4 hours, and washing with water to obtain a second crosslinked product.

7. The method for preparing the compression-resistant and folding-resistant hydrophilic three-dimensional fiber aerogel according to claim 1, characterized in that: The pre-crosslinking agent is an aqueous solution of a macromolecular substance; the macromolecular substance includes at least one of hyaluronic acid, silk fibroin, chitosan, cellulose, chondroitin, heparin, gum arabic, xanthan gum, pectin, and guar gum; preferably hyaluronic acid.

8. The method for preparing the compression-resistant and folding-resistant hydrophilic three-dimensional fiber aerogel according to claim 1, characterized in that: The adding of the chemical crosslinking agent and stirring in step S5 are carried out in two steps: first, the first chemical crosslinking agent is added and stirred for 0.5-2 hours, and then the second chemical crosslinking agent is added and stirred for 1-3 hours.

9. The method for preparing the compression-resistant and folding-resistant hydrophilic three-dimensional fiber aerogel according to claim 1, characterized in that: The first chemical crosslinking agent and the second chemical crosslinking agent are independently selected from any one of EDC, NHS, GA and ET.

10. Use of the preparation method of the hydrophilic three-dimensional fiber aerogel according to claim 1 or the hydrophilic three-dimensional fiber aerogel according to claim 3 in the preparation of biomedical materials.