Strong acid group-containing polymer coating with sterilization function as well as preparation method and application of strong acid group-containing polymer coating
By applying a polymer coating with strong acid group-containing polymer formed by electrostatic action on the surface of the object, the problem of low inhibition and bactericidal efficiency of bacteria and fungi in the prior art is solved, effective inhibition and bactericidal of various microorganisms is achieved, and coating is simplified. Layer preparation and application reduces the amount of fungicide used.
Patent Information
- Application Number
- CN202410855772.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-06-28
AI Technical Summary
The prior art has problems with low efficiency, high cost and drug residues in inhibiting the growth and bactericidal of bacteria and fungi, and conventional bactericides have irreversible effects on the environment.
A polymer coating containing strong acid groups based on electrostatic action is developed. By introducing quaternary ammonium groups and strong acid aqueous solution, a polymer coating that can release hydrogen ions is formed to inhibit the growth of bacteria and fungi on the surface of the object.
It has achieved effective inhibition and bactericidal treatment for bacteria such as E. coli, Staphylococcus aureus, Pseudomonas aeruginosa, Helicobacter pylori and Candida, simplified the coating preparation and application process, and reduced the need for high concentration of bactericides. .
Smart Images

Figure CN118895074A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of organic chemistry for preventing and treating bacterial infection of crops, and in particular relates to a polymer coating containing strong acid groups with bactericidal function, and a preparation method and application thereof. Background Art
[0002] Microorganisms such as bacteria and fungi are ubiquitous in the natural environment and the human body, and pathogenic bacteria pose a huge threat to the public's health. Foodborne diseases, urinary tract infections, tuberculosis and other bacterial-derived diseases caused by bacterial contamination of food sources have become a major public health issue. In addition, bacterial adhesion and reproduction have always been a long-standing problem in the biomedical field. Tissue infection and equipment failure caused by bacterial adhesion and reproduction are the main causes of implant failure of medical materials, which not only brings a huge economic burden to patients and society, but also seriously threatens human life and health, and poses a severe challenge to the global medical and health industry.
[0003] The bacterial resistance crisis has forced researchers to avoid the use of antibiotics in material modification. However, bacteria adhering to the surface of the equipment require higher concentrations of fungicides and longer sterilization times to inhibit the growth of bacteria on the surface. Conventional sterilization surfaces require the use of some natural or synthetic organic compounds or heavy metal fungicides. Such fungicides are not only expensive, but also have drug residue problems caused by incomplete cleaning, which have irreversible effects on the body and the biological environment. For a long time, organic acids have played an important role in the preservation of food. Benzoic acid, sorbic acid, etc. are often added to food as preservatives. Acetic acid, lactic acid, fumaric acid, etc. can prevent or delay the growth of pathogenic bacteria or spoilage bacteria. The use of hydrogen ions as antimicrobial fungicides has the advantages of strong, extensive and reusable antimicrobial functions, as well as low production costs, showing great application potential.
[0004] Therefore, preparing a polymer coating containing strong acid groups that can be coated on the surface of any object and can effectively kill bacteria is of great significance for preventing and treating bacterial infections and protecting human health and safety. Summary of the invention
[0005] In order to overcome the deficiencies of the prior art, the present invention aims to provide a polymer coating containing strong acid groups with a bactericidal function that can be formed on the surface of an object based on electrostatic action. The polymer containing strong acid groups can be coated on any surface by introducing a quaternary ammonium group with a certain carbon chain and utilizing hydrophobic forces. The polymer coating containing strong acid groups can release hydrogen ions in a physiological environment where microorganisms exist, making bacteria such as Escherichia coli, Staphylococcus aureus, Pseudomonas aeruginosa, Helicobacter pylori, and fungi such as Candida inactive, thereby achieving the effect of inhibiting the growth of microorganisms and sterilizing.
[0006] Specifically, the first aspect of the present invention is to provide a polymer coating containing strong acid groups with bactericidal function, which has a chemical structure as shown in Formula 1:
[0007]
[0008] Where R1 is a strong acid group - sulfonic acid group (-SO3), sulfuric acid group (-OSO3), benzenesulfonic acid group Any one of: R2 is C n H 2n group (n is an integer greater than or equal to 1); R3 is a methyl group or a hydrogen atom; x and y are degrees of polymerization, each selected from an integer of 30 to 2000 and the ratio of x::y is in the range of 0.1 to 0.95.
[0009] The second aspect of the present invention is to provide a method for preparing the polymer coating according to the first aspect of the present invention and a method for coating a surface of a material using the coating, the steps of which include:
[0010] Step 1, cleaning the solid surface to be coated to obtain a clean solid surface;
[0011] Step 2, preparing a strongly acidic aqueous solution of a strong electrolyte anion polymer, wherein the strong electrolyte anion polymer is one of polyvinyl sulfonic acid or its salt, polyvinyl sulfuric acid or its salt, polystyrene sulfonic acid or its salt, and the pH range of the solution is 0.5 to 1.5;
[0012] Step 3, prepare a strongly acidic aqueous solution of a quaternary ammonium salt compound, wherein the chemical structural formula of the quaternary ammonium salt compound is CH3(CH2): n N(R3)3·X, wherein R3 is a methyl group or a hydrogen atom, n is an integer greater than or equal to 1, and X is Cl - Br - ,I - Any one of the above, the solution pH range is 0.5 to 1.5;
[0013] Step 4, mixing the strongly acidic aqueous solution of the strong electrolyte anion polymer prepared in step 2 with the strongly acidic aqueous solution of the quaternary ammonium salt compound prepared in step 3, and obtaining an aqueous solution of a polymer having a chemical structure as shown in Formula 1 after electrostatic action between the two; or directly mixing the quaternary ammonium salt compound powder described in step 3 with the strongly acidic aqueous solution of the strong electrolyte anion polymer prepared in step 2, and obtaining an aqueous solution of a polymer having a chemical structure as shown in Formula 1 after electrostatic action between the two;
[0014] Step 5, mixing the polymer solution obtained in step 4 with an organic solvent to obtain a polymer coating solution containing an organic solvent;
[0015] Step 6: coating the polymer coating solution prepared in step 5 on the clean solid surface obtained in step 1 to obtain a polymer coating containing strong acid groups having a chemical structure as shown in formula 1.
[0016] In the present invention, the above-mentioned solid materials to be coated include: inorganic non-metallic materials, metal products, wood materials, artificial synthetic or natural polymer materials. Specifically, they may include: inorganic non-metallic materials: single crystal silicon wafers, glass sheets, silicon carbide, etc.; metal products: stainless steel, iron and its alloys, magnesium and its alloys, titanium and its alloys, copper and its alloys, aluminum and its alloys, zinc and its alloys, etc.; artificial synthetic or natural polymer materials: polypropylene (PP), polystyrene (PS), polyurethane (PU), polyester (PET), polyethylene (PE), polyvinyl chloride (PVC), polytetrafluoroethylene (PTFE), polyacrylonitrile, rubber, cotton cloth, silk, etc.
[0017] In the present invention, the weight average molecular weight of the strong electrolyte anion polymer is in the range of 5 to 1000 kDa, and the mass concentration of the strong acid aqueous solution of the strong electrolyte anion polymer is in the range of 0.2 to 20 mg / mL.
[0018] In the present invention, the mass concentration of the quaternary ammonium salt compound in the strongly acidic aqueous solution is 0.2-20 mg / mL or the mass concentration of the quaternary ammonium salt compound in the strongly acidic aqueous solution of the strong electrolyte anion polymer is 0.1-20 mg / mL.
[0019] Preferably, the above-mentioned strongly acidic aqueous solution with a pH value of 0.5 to 1.5 is obtained by adjusting the pH value of a hydrochloric acid solution or a sulfuric acid solution.
[0020] In the present invention, the organic solvent mixed with the polymer aqueous solution having a chemical structure as shown in Formula 1 includes one or more of methanol, ethanol, isopropanol, propanol, ethylene glycol, dimethyl sulfoxide, dimethylformamide, acetonitrile, acetone, chloroform or ethyl acetate.
[0021] Preferably, the volume ratio of the organic solvent to the aqueous solution in the polymer coating solution is in the range of 0.1 to 0.5.
[0022] In the present invention, the coating method of the polymer coating solution includes dipping, spin coating, spraying, electrostatic spinning or inkjet printing.
[0023] In the present invention, the coating time is 10 seconds to 80 minutes, the coating temperature is 10 to 50° C., and the coating frequency is one or more.
[0024] Preferably, the pH range of the strongly acidic aqueous solution of the strong electrolyte anion polymer or the strongly acidic aqueous solution of the quaternary ammonium salt compound is 1 to 1.5.
[0025] Preferably, the mass concentration of the strong acid aqueous solution of the strong electrolyte anion polymer is 0.5-10 mg / mL.
[0026] Preferably, the mass concentration of the strongly acidic aqueous solution of the quaternary ammonium salt compound is 0.5 to 10 mg / mL or the mass concentration of the quaternary ammonium salt compound in the strongly acidic aqueous solution of the strong electrolyte anion polymer is 0.5 to 10 mg / mL.
[0027] Preferably, the coating time is 10 seconds to 60 minutes, the coating temperature is preferably 15 to 40° C., and the coating times are preferably 4 to 8 times.
[0028] The third aspect of the present invention is to use the polymer coating described in the first aspect of the present invention and the method for preparing the polymer coating described in the second aspect of the present invention and the method for coating the surface of a substance with the coating in inhibiting the growth of microorganisms on the surface of an object. Preferably, the microorganisms include Escherichia coli, Staphylococcus aureus, Pseudomonas aeruginosa, Helicobacter pylori or Candida albicans.
[0029] The present invention can achieve the following technical effects:
[0030] 1. The method for preparing the polymer coating and the method for coating the surface of a substance of the present invention are simple and easy to implement;
[0031] 2. The present invention can make the surface of the coated object inactive, such as Escherichia coli, Staphylococcus aureus, Pseudomonas aeruginosa, Helicobacter pylori bacteria and Candida albicans, thereby achieving the effect of inhibiting the growth of microorganisms and killing bacteria. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a comparison diagram of the inhibitory effect of the solid surface containing the polymer coating containing strong acid groups of the present invention and the unmodified coating on the growth of Escherichia coli.
[0033] Figure 2 The figure is a comparison chart of the fungal growth inhibition effect of the solid surface containing the polymer coating containing strong acid groups of the present invention and the unmodified coating on Candida.
[0034] Figure 3 The figure is a comparison of the bactericidal effects of the solid surface containing the polymer coating containing strong acid groups of the present invention and the unmodified coating on Staphylococcus aureus.
[0035] Figure 4 The figure is a comparison of the bactericidal effects of the solid surface containing the polymer coating containing strong acid groups of the present invention and the solid surface without modified coating on Candida. DETAILED DESCRIPTION
[0036] In order to further understand the present invention, the preferred technical scheme of the present invention is described in detail with specific embodiments and test examples. The reagents and raw materials used in the following embodiments and test examples are all industrial pure commodities, and the equipment used are all commonly used equipment and devices in the field.
[0037] Example 1
[0038] Step 1, soaking the silicon wafer in a hydrogen peroxide / concentrated sulfuric acid mixed solution (volume ratio of 1:3) at 90° C. for 4 hours to remove surface impurities, and then ultrasonically cleaning with ultrapure water for multiple times to obtain a clean silicon wafer surface;
[0039] Step 2, using 1M hydrochloric acid solution to prepare a 2 mg / mL, pH=1, strongly acidic aqueous solution of sodium polyethylene sulfonate with a weight average molecular weight of 8 kDa;
[0040] Step 3, prepare a 2 mg / mL, pH=1, strongly acidic aqueous solution of hexyltrimethylammonium bromide using 1M hydrochloric acid solution, the chemical formula of which is CH3(CH2)5N(Br)(CH3)3;
[0041] Step 4, mixing the strongly acidic aqueous solution of sodium polyvinyl sulfonate prepared in step 2 with the strongly acidic aqueous solution of hexyltrimethylammonium bromide prepared in step 3, subjecting the two to electrostatic action for 6 hours, and washing with a saturated sulfur dioxide aqueous solution to obtain an aqueous solution of a polymer having a chemical structure as shown in the following formula (x:y=0.1);
[0042]
[0043] Step 5, mixing the polymer aqueous solution obtained in step 4 with ethanol to obtain a polymer coating solution with an ethanol / water volume ratio of 0.3 and a polymer concentration of 10 mg / mL;
[0044] Step 6. At room temperature, soak the clean silicon wafer obtained in step 1 in the polymer coating solution prepared in step 5 for 30 minutes, and repeat the soaking twice after drying to obtain a polymer coating containing strong acid groups having a chemical structure shown in the above formula formed based on electrostatic action.
[0045] Example 2
[0046] Step 1, soaking the silicon wafer in a hydrogen peroxide / concentrated sulfuric acid mixed solution (volume ratio of 1:3) at 90° C. for 4 hours to remove surface impurities, and then ultrasonically cleaning with ultrapure water for multiple times to obtain a clean silicon wafer surface;
[0047] Step 2, using 1M sulfuric acid solution to prepare a 2 mg / mL, pH=1.3, strongly acidic aqueous solution of polyvinyl potassium sulfate with a weight average molecular weight of 10 kDa;
[0048] Step 3, prepare a 2 mg / mL, pH=1.2 strongly acidic aqueous solution of amyltrimethylammonium chloride using 1M hydrochloric acid solution, the chemical formula of which is CH3(CH2)4N(Cl)(CH3)3;
[0049] Step 4, mixing the strongly acidic aqueous solution of potassium polyvinyl sulfate prepared in step 2 with the strongly acidic aqueous solution of amyltrimethylammonium chloride prepared in step 3, subjecting the two to electrostatic action for 8 hours, and washing with a saturated sulfur dioxide aqueous solution to obtain an aqueous solution of a polymer having a chemical structure as shown in the following formula;
[0050]
[0051] Step 5, mixing the polymer aqueous solution obtained in step 4 with ethylene glycol to obtain a polymer coating solution with a polymer concentration of 5 mg / mL and an ethylene glycol / water volume ratio of 0.4;
[0052] Step 6, soak the clean silicon wafer obtained in step 1 in the polymer coating solution obtained in step 5 at 30°C for 40 minutes, repeat the soaking 4 times after drying, and obtain a polymer coating containing strong acid groups having a chemical structure shown in the above formula formed based on electrostatic action after drying.
[0053] Example 3
[0054] Step 1: Treat the polyurethane sheet in an oxygen environment of a plasma cleaning machine for 10 minutes to remove surface impurities and obtain a clean polyurethane surface;
[0055] Step 2, using 1M sulfuric acid solution to prepare a 10 mg / mL, pH=1, strongly acidic aqueous solution of polystyrene sulfonic acid with a weight average molecular weight of 70 kDa;
[0056] Step 3, directly mixing the decyltrimethylammonium bromide compound powder with the chemical formula CH3(CH2)9N(Br)(CH3)3 with the strongly acidic aqueous solution of polystyrene sulfonic acid prepared in step 2, subjecting the two to electrostatic action for 3 hours, and washing with a saturated sulfur dioxide aqueous solution to obtain an aqueous solution of a polymer with a chemical structure shown in the following formula;
[0057]
[0058] Step 4, mixing the polymer aqueous solution obtained in step 3 with propanol to obtain a polymer coating solution with a propanol / water volume ratio of 0.2 and a polymer concentration of 10 mg / mL;
[0059] Step 5. Use a desktop coating machine to spin-coat the polymer coating solution obtained in step 4 at 35° C. on the clean polyurethane sheet obtained in step 1 for 10 minutes. After air drying, repeat the spin coating once. After drying, a polymer coating containing strong acid groups having a chemical structure shown in the above formula formed based on electrostatic action is obtained.
[0060] Example 4
[0061] Step 1: Treat the polyester fiber in an oxygen environment of a plasma cleaning machine for 10 minutes to remove surface impurities and obtain a clean polyester fiber surface;
[0062] Step 2, using 2M hydrochloric acid solution to prepare a 1 mg / mL, pH=1.2, strongly acidic aqueous solution of polyethylene sulfonic acid with a weight average molecular weight of 20 kDa;
[0063] Step 3: Prepare a 4 mg / mL, pH=1.1 strongly acidic aqueous solution of octadecyltrimethylammonium chloride using 0.5 M sulfuric acid solution. The chemical formula is CH3(CH2): 17 N(Cl)(CH3)3;
[0064] Step 4, the strongly acidic aqueous solution of polyethylene sulfonic acid prepared in step 2 is mixed with the strongly acidic aqueous solution of octadecyltrimethylammonium chloride prepared in step 3, and the two are subjected to electrostatic action for 12 hours, and washed with a saturated sulfur dioxide aqueous solution to obtain an aqueous solution of a polymer having a chemical structure shown in the following formula (x:y=0.2);
[0065]
[0066] Step 5, mixing the polymer aqueous solution obtained in step 4 with an ethanol / propanol mixed solution with a volume ratio of 1:1 to obtain a polymer coating solution with a polymer concentration of 1 mg / mL and an organic mixed solution / water volume ratio of 0.15;
[0067] Step 6: Soak the clean polyester fiber surface obtained in step 1 in the polymer coating solution obtained in step 5 at 15° C. for 20 minutes, repeat the soaking 3 times after drying, and obtain a polymer coating containing strong acid groups having a chemical structure shown in the above formula formed based on electrostatic action after drying.
[0068] Example 5
[0069] Step 1, soaking the glass sheet in a hydrogen peroxide / concentrated sulfuric acid mixed solution (volume ratio of 1:3) at 90° C. for 4 hours to remove surface impurities, and then ultrasonically cleaning the glass sheet with ultrapure water for multiple times to obtain a clean surface of the glass sheet;
[0070] Step 2, using 3M sulfuric acid solution to prepare a 4 mg / mL, pH=1.5, strongly acidic aqueous solution of sodium polystyrene sulfonate with a weight average molecular weight of 1000 kDa;
[0071] Step 3, directly mixing the butyltrimethylammonium bromide compound powder with the chemical formula CH3(CH2)3N(Br)(CH3)3 with the strongly acidic aqueous solution of sodium polystyrene sulfonate prepared in step 2, subjecting the two to electrostatic action for 1 hour, and washing with a saturated sulfur dioxide aqueous solution to obtain an aqueous solution of a polymer with a chemical structure as shown in the following formula (x:y=0.95);
[0072] Step 4, mixing the polymer aqueous solution obtained in step 3 with methanol to obtain a polymer coating solution with a methanol / water volume ratio of 0.5 and a polymer concentration of 7.5 mg / mL;
[0073]
[0074] Step 5, immerse the surface of the clean glass sheet obtained in step 1 in the polymer coating solution obtained in step 4 at 10°C for 10 minutes, repeat the immersion 5 times after drying, and obtain a polymer coating containing strong acid groups having a chemical structure shown in the above formula formed based on electrostatic action after drying.
[0075] Example 6
[0076] Step 1: Treat the aluminum sheet in an oxygen environment of a plasma cleaning machine for 10 minutes to remove surface impurities and obtain a clean aluminum sheet surface;
[0077] Step 2, using 3M hydrochloric acid solution to prepare a 0.5 mg / mL, pH=1, strongly acidic aqueous solution of polyvinyl potassium sulfate with a weight average molecular weight of 15 kDa;
[0078] Step 3: Prepare a 5 mg / mL, pH=1, strongly acidic aqueous solution of octadecyltrimethylammonium bromide using 1M sulfuric acid solution. The chemical formula is CH3(CH2): 17 N(Br)(CH3)3;
[0079] Step 4, the strongly acidic aqueous solution of potassium polyvinyl sulfate prepared in step 2 is mixed with the strongly acidic aqueous solution of octadecyltrimethylammonium bromide prepared in step 3, and the two are subjected to electrostatic action for 18 hours, and then washed with a saturated sulfur dioxide aqueous solution to obtain an aqueous solution of a polymer having a chemical structure shown in the following formula (x:y=0.05);
[0080]
[0081] Step 5, mixing the polymer aqueous solution obtained in step 4 with ethyl acetate to obtain a polymer coating solution with a polymer concentration of 3 mg / mL and an ethyl acetate / water volume ratio of 0.3;
[0082] Step 6, inject the polymer coating solution obtained in step 5 at 20°C into a spray gun and spray it on the surface of the clean aluminum sheet obtained in step 1. The coating time is 1 minute. After drying, the spraying is repeated 4 times. After drying, a polymer coating containing strong acid groups having a chemical structure shown in the above formula formed based on electrostatic action is obtained.
[0083] Example 7
[0084] Step 1: Treat the cotton cloth in an oxygen environment of a plasma cleaning machine for 10 minutes to remove surface impurities and obtain a clean cotton cloth surface;
[0085] Step 2, using 3M sulfuric acid to prepare a 2 mg / mL, pH=1, strongly acidic aqueous solution of sodium polystyrene sulfonate with a weight average molecular weight of 70 kDa and polyethylene sulfonic acid with a weight average molecular weight of 8 kDa (the molar ratio of the two polymers is 1:2);
[0086] Step 3: Prepare a 2.5 mg / mL, pH=1.05, strongly acidic aqueous solution of dodecyltrimethylammonium bromide using a 3M sulfuric acid solution. The chemical formula is CH3(CH2): 11 N(Br)(CH3)3;
[0087] Step 4, mixing the strongly acidic aqueous solution of sodium polystyrene sulfonate-polyethylene sulfonic acid prepared in step 2 with the strongly acidic aqueous solution of dodecyltrimethylammonium bromide prepared in step 3, subjecting the two to electrostatic action for 1 hour, and washing with a saturated sulfur dioxide aqueous solution to obtain two polymer aqueous solutions with chemical structures shown in the following formula (x:y=0.17);
[0088]
[0089] Step 5, mixing the polymer aqueous solution obtained in step 4 with an ethanol / ethylene glycol organic solvent in a volume ratio of 1:2 to obtain a polymer coating solution with an organic solvent / water volume ratio of 0.5 and a polymer concentration of 6 mg / mL;
[0090] Step 6: Use a desktop coating machine to spin-coat the polymer coating solution obtained in step 5 at 17° C. onto the clean cotton cloth obtained in step 1 for 20 minutes. Repeat the spin coating twice after drying to obtain a polymer coating containing strong acid groups having a chemical structure shown in the above formula formed based on electrostatic action.
[0091] Example 8
[0092] Step 1: Treat the wood in an oxygen environment of a plasma cleaning machine for 10 minutes to remove surface impurities and obtain a clean wood surface;
[0093] Step 2, using 1M sulfuric acid solution to prepare a 10 mg / mL, pH=1, strongly acidic aqueous solution of 4 kDa weight average molecular weight polyethylene sulfonate lithium and 12 kDa weight average molecular weight polyethylene sulfuric acid (the molar ratio of the two polymers is 1:3);
[0094] Step 3, prepare a 5 mg / mL, pH=1.2 strongly acidic aqueous solution of octyltrimethylammonium chloride using 1M hydrochloric acid solution, the chemical formula of which is CH3(CH2)7N(Cl)(CH3)3;
[0095] Step 4, the strongly acidic aqueous solution of lithium polyvinyl sulfonate-sodium polyvinyl sulfate prepared in step 2 is mixed with the strongly acidic aqueous solution of octyltrimethylammonium chloride prepared in step 3, and the two are subjected to electrostatic action for 10 hours, and then washed with a saturated sulfur dioxide aqueous solution to obtain two polymer aqueous solutions with chemical structures shown in the following formula (x:y=0.2);
[0096]
[0097] Step 5, mixing the polymer aqueous solution obtained in step 4 with a dimethyl sulfoxide / propanol organic solvent in a volume ratio of 1:3 to obtain a polymer coating solution with an organic solvent / water volume ratio of 0.26 and a polymer concentration of 1 mg / mL;
[0098] Step 6, inject the polymer coating solution prepared in step 5 at 30°C into an inkjet printer, and print on the clean wood surface obtained in step 1. The coating time is 20 minutes. After drying, the printing is repeated 5 times. After drying, a polymer coating containing strong acid groups having a chemical structure shown in the above formula formed based on electrostatic action is obtained.
[0099] Example 9
[0100] Step 1: Treat the polypropylene sheet in an oxygen environment of a plasma cleaning machine for 10 minutes to remove surface impurities and obtain a clean polypropylene surface;
[0101] Step 2, using 2.5M sulfuric acid solution to prepare a 10 mg / mL, pH=1.5, strongly acidic aqueous solution of polystyrene sulfonic acid with a weight average molecular weight of 1000 kDa and polyvinyl sulfate with a weight average molecular weight of 12 kDa (the molar ratio of the two polymers is 3:1);
[0102] Step 3: Prepare a 10 mg / mL, pH=1, strongly acidic aqueous solution of undecyltrimethylammonium chloride using a 2M hydrochloric acid solution, the chemical formula of which is CH3(CH2): 10 N(Cl)(CH3)3;
[0103] Step 4, the strongly acidic aqueous solution of polystyrene sulfonic acid-polyvinyl sulfate prepared in step 2 is mixed with the strongly acidic aqueous solution of undecyltrimethylammonium chloride prepared in step 3, and the two are subjected to electrostatic action for 2 hours, and then washed with a saturated sulfur dioxide aqueous solution to obtain an aqueous solution of two polymers having a chemical structure as shown in the following formula (x:y=0.35);
[0104]
[0105] Step 5, mixing the polymer aqueous solution obtained in step 4 with a chloroform / ethylene glycol organic solvent in a volume ratio of 1:3 to obtain a polymer coating solution in which the organic solvent / water volume ratio is 0.4 and the polymer concentration is 0.8 mg / mL;
[0106] Step 6, inject the polymer coating solution prepared in step 5 at 27°C into the syringe of the electrospinning device, and electrospin the polymer film on the clean polypropylene sheet obtained in step 1. The coating time is 10 minutes, and the film is dried at 50°C. The coating is repeated 3 times. After drying, a polymer coating containing strong acid groups having a chemical structure shown in the above formula formed based on electrostatic action is obtained.
[0107] Example 10
[0108] Step 1: Treat the polytetrafluoroethylene sheet in an oxygen environment of a plasma cleaning machine for 10 minutes to remove surface impurities and obtain a clean polytetrafluoroethylene surface;
[0109] Step 2, using 2M hydrochloric acid solution to prepare a 4 mg / mL, pH=1.1, strongly acidic aqueous solution of polystyrene sulfonic acid with a weight average molecular weight of 70 kDa and polyethylene sulfonic acid with a weight average molecular weight of 7 kDa (the molar ratio of the two polymers is 1:2);
[0110] Step 3: Prepare a 3 mg / mL, pH=1.3, strong acidic aqueous solution of tetradecyltrimethylammonium bromide using a 2M sulfuric acid solution. The chemical formula is CH3(CH2): 13 N(Br)(CH3)3;
[0111] Step 4, the strongly acidic aqueous solution of polystyrene sulfonic acid-polyethylene sulfonic acid prepared in step 2 is mixed with the strongly acidic aqueous solution of tetradecyltrimethylammonium bromide prepared in step 3, and the two are subjected to electrostatic action for 3 hours, and washed with a saturated sulfur dioxide aqueous solution to obtain two polymer aqueous solutions with chemical structures shown in the following formula (x:y=0.45);
[0112]
[0113] Step 5, mixing the polymer aqueous solution obtained in step 4 with an organic solvent of dimethyl sulfoxide / ethanol / isopropanol in a volume ratio of 1:1:2 to obtain a polymer coating solution with an organic solvent / water volume ratio of 0.17 and a polymer concentration of 5 mg / mL;
[0114] Step 6, inject the polymer coating solution obtained in step 5 at 15°C into a spray gun and spray it on the surface of the clean polytetrafluoroethylene sheet obtained in step 1. The coating time is 5 minutes. After drying, the spraying is repeated 4 times. After drying, a polymer coating containing strong acid groups having a chemical structure shown in the above formula formed based on electrostatic action is obtained.
[0115] Embodiment 11
[0116] Step 1: Treat the silk in an oxygen environment of a plasma cleaning machine for 10 minutes to remove surface impurities and obtain a clean silk surface;
[0117] Step 2, using 3M hydrochloric acid solution to prepare a 6 mg / mL, pH=1.2, strongly acidic aqueous solution of polystyrene sulfonic acid with a weight average molecular weight of 500 kDa, polyvinyl sulfuric acid with a weight average molecular weight of 12 kDa, and polyvinyl sulfonic acid with a weight average molecular weight of 8 kDa (the molar ratio of the three polymers is 3:1:1);
[0118] Step 3: Prepare a 0.5 mg / mL, pH=1.5 strongly acidic aqueous solution of octadecylamine hydrochloride using 2.5 M hydrochloric acid solution. Its chemical formula is CH3(CH2): 17 NH3·Cl;
[0119] Step 4, the strongly acidic aqueous solution of polystyrene sulfonic acid-polyvinyl sulfuric acid-polyvinyl sulfonic acid prepared in step 2 is mixed with the strongly acidic aqueous solution of octadecylamine hydrochloride prepared in step 3, and the two are subjected to electrostatic action for 7 hours, and then washed with a saturated sulfur dioxide aqueous solution to obtain an aqueous solution of three polymers with chemical structures shown in the following formula (x:y=0.5);
[0120]
[0121] Step 5, mixing the polymer aqueous solution obtained in step 4 with an acetone / acetonitrile / isopropanol organic solvent in a volume ratio of 2:1:3 to obtain a polymer coating solution with an organic solvent / water volume ratio of 0.2 and a polymer concentration of 10 mg / mL;
[0122] Step 6, inject the polymer coating solution prepared in step 5 at room temperature into an inkjet printer, and print on the clean silk surface obtained in step 1. The coating time is 45 minutes. After drying, the printing is repeated twice. After drying, a polymer coating containing strong acid groups having a chemical structure shown in the above formula formed based on electrostatic action is obtained.
[0123] Example 12
[0124] Step 1: Treat the polyester sheet in an oxygen environment of a plasma cleaning machine for 10 minutes to remove surface impurities and obtain a clean polyester surface;
[0125] Step 2, using 3M hydrochloric acid solution to prepare a 4 mg / mL, pH=1.3, strongly acidic aqueous solution of sodium polyvinyl sulfonate with a weight average molecular weight of 20 kDa and potassium polyvinyl sulfate with a weight average molecular weight of 15 kDa (the molar ratio of the two polymers is 4:1);
[0126] Step 3: Prepare a 6 mg / mL, pH=1.3 strongly acidic aqueous solution of dodecylamine hydrochloride using 1M sulfuric acid solution. Its chemical formula is CH3(CH2): 11 NH3·Cl;
[0127] Step 4: Mix the strongly acidic aqueous solution of sodium polysulfonate-potassium polysulfate prepared in step 2 with the strongly acidic aqueous solution of dodecylamine hydrochloride prepared in step 3, subject the two to electrostatic action for 9 hours, and wash with a saturated sulfur dioxide aqueous solution to obtain two polymer aqueous solutions with chemical structures shown in the following formula (x:y=0.6);
[0128]
[0129] Step 5, mixing the polymer aqueous solution obtained in step 4 with an organic solvent of dimethylformamide / acetonitrile / ethylene glycol in a volume ratio of 1:3:1 to obtain a polymer coating solution with an organic solvent / water volume ratio of 0.35 and a polymer concentration of 3 mg / mL;
[0130] Step 6, inject the polymer coating solution prepared in step 5 at 23°C into the syringe of the electrospinning device, and electrospin the polymer film on the clean polyester sheet obtained in step 1. The coating time is 25 minutes. After drying at 50°C, the coating is repeated 7 times. After drying, a polymer coating containing strong acid groups is obtained based on electrostatic action, and the chemical structure shown in the above formula is obtained.
[0131] Embodiment 13
[0132] Step 1: Treat the polyethylene tube in an oxygen environment of a plasma cleaning machine for 10 minutes to remove surface impurities and obtain a clean polyethylene surface;
[0133] Step 2, using 1M hydrochloric acid solution to prepare a 0.8 mg / mL, pH=1 strongly acidic aqueous solution of sodium polystyrene sulfonate with a weight average molecular weight of 1000 kDa, sodium polyvinyl sulfonate with a weight average molecular weight of 8 kDa, and lithium polyvinyl sulfate with a weight average molecular weight of 25 kDa (the molar ratio of the three polymers is 1:3:1);
[0134] Step 3, using 1M hydrochloric acid solution to prepare a 0.7 mg / mL, pH=1.4 strongly acidic aqueous solution of octylamine hydrochloride, whose chemical formula is CH3(CH2)7NH3·Cl;
[0135] Step 4, the strongly acidic aqueous solution of sodium polystyrene sulfonate-sodium polyvinyl sulfonate-lithium polyvinyl sulfate prepared in step 2 is mixed with the strongly acidic aqueous solution of octylamine hydrochloride prepared in step 3, and the two are subjected to electrostatic action for 5 hours, and washed with a saturated sulfur dioxide aqueous solution to obtain an aqueous solution of three polymers with the chemical structure shown in the following formula (x:y=0.4);
[0136]
[0137] Step 5, mixing the polymer aqueous solution obtained in step 4 with an organic solvent of dimethyl sulfoxide / acetone / ethanol in a volume ratio of 2:3:5 to obtain a polymer coating solution with an organic solvent / water volume ratio of 0.2 and a polymer concentration of 0.5 mg / mL;
[0138] Step 6, soak the clean polyethylene tube obtained in step 1 in the polymer coating solution obtained in step 5 at 35°C for 20 minutes, repeat the soaking 6 times after drying, and obtain a polymer coating containing strong acid groups having a chemical structure shown in the above formula formed based on electrostatic action after drying.
[0139] In order to prove the beneficial effects of the present invention, the present invention verifies the growth inhibition and bactericidal effect of the polymer coating containing strong acid groups with bactericidal function formed based on electrostatic action, and the specific test is as follows:
[0140] The present invention uses bacteria such as Escherichia coli, Staphylococcus aureus, Pseudomonas aeruginosa, Helicobacter pylori and fungi such as Candida to carry out verification tests.
[0141] Test 1
[0142] The inhibitory effect of the samples on the growth of E. coli was verified according to the following steps.
[0143] Step 1, prepare bacterial culture lysate broth (LB) solution: dissolve 25g LB powder in 1000ml water and stir thoroughly to dissolve, and sterilize the prepared culture solution in a high temperature sterilizer;
[0144] Step 2, prepare E. coli bacterial culture solution: dissolve 10 μL of bacterial culture in 10 mL of LB solution sterilized in step 1;
[0145] Step 3, placing the bacterial liquid treated in step 2 in a shaker at a temperature of 37°C and a shaking speed of 250 rpm for 24 hours;
[0146] Step 4: centrifuge the bacterial solution cultured in step 3 at a speed of 3000 rpm for 10 min;
[0147] Step 5: quantitatively dilute the bacteria centrifuged in step 4 with the LB solution sterilized in step 1, so that the absorption value at OD=600nm in the ultraviolet absorption test is 0.008-0.01, and the corresponding bacterial concentration is 10 8 CFU / mL, and then the bacterial concentration was 10 8 The bacterial solution was further diluted with LB solution to a bacterial concentration of 10 CFU / mL. 4 CFU / mL of bacterial solution is used for subsequent experimental operations;
[0148] Step 6: Place the sample obtained in Example 1 and the unmodified solid surface as a control sample on the solid surface with a bacterial concentration of 10 4 CFU / mL of bacterial solution, the culture temperature is 37°C, the shaker speed is 200rpm, the OD value is measured every 2h, and the culture time is 18h;
[0149] Step 7: Analyze the bacterial growth process of the samples of Example 1 and the blank control samples cultured separately in step 6.
[0150] The results of the verification of the inhibition of E. coli growth on the samples are as follows Figure 1 As shown in the figure: Since the sample of Example 1 releases hydrogen ions, the normal growth of bacteria in the bacterial solution in which it is immersed is inhibited (the OD value is close to 0.5 after 18 hours of bacterial culture); while the OD value of the bacteria in the bacterial solution immersed in the blank control sample is greater than 1.2 after 18 hours of bacterial culture. The number of bacteria in the bacterial solution immersed in the sample of Example 1 is much lower than the number of bacteria in the blank control sample, and the number of bacteria between the two shows an order of magnitude difference.
[0151] The inhibitory effect of the polymer coating containing strong acid groups with bactericidal function formed based on electrostatic effect on the growth of Escherichia coli was verified.
[0152] Test 2
[0153] The inhibitory effect of the samples on the growth of Staphylococcus aureus was verified according to the following steps.
[0154] The bacterial growth process was inhibited according to the standard described in Experiment 1, except that the Staphylococcus aureus seed solution was prepared for the experiment. The effect of Example 6 on inhibiting the growth of Staphylococcus aureus was verified, and the bacterial growth process of the sample of Example 6 and the corresponding blank control sample cultured separately was analyzed.
[0155] The results of the sample's inhibition of Staphylococcus aureus growth showed that the sample of Example 6 adsorbed a large amount of hydrogen ions, which inhibited the normal growth of bacteria in the bacterial solution in which it was immersed (the OD value was lower than 0.5 after 18 hours of bacterial culture); while the OD value of the bacteria in the bacterial solution immersed in the blank control sample was close to 1.5 after 18 hours of bacterial culture. The number of bacteria in the bacterial solution immersed in the sample of Example 6 was much lower than the number of bacteria in the blank control sample, and the number of bacteria between the two showed an order of magnitude difference.
[0156] The inhibitory effect of the polymer coating containing strong acid groups with bactericidal function formed based on electrostatic action on the growth of Staphylococcus aureus was verified.
[0157] Test 3
[0158] The inhibitory effect of the samples on the growth of Pseudomonas aeruginosa was verified according to the following steps.
[0159] The bacterial growth process was inhibited according to the standard described in Experiment 1, except that the Pseudomonas aeruginosa seed solution was prepared for the experiment. The effect of Example 7 on inhibiting the growth of Pseudomonas aeruginosa was verified, and the bacterial growth process of the sample of Example 7 and the corresponding blank control sample cultured separately was analyzed.
[0160] The results of the sample's inhibition of Pseudomonas aeruginosa growth showed that the sample of Example 7 was loaded with a large amount of hydrogen ions, which inhibited the normal growth of bacteria in the bacterial solution in which it was immersed (the OD value was lower than 0.4 after 18 hours of bacterial culture); while the OD value of the bacterial solution in which the blank control sample was immersed was close to 1.3 after 18 hours of bacterial culture. The number of bacteria in the bacterial solution in which the sample of Example 7 was immersed was much lower than the number of bacteria in the blank control sample, and the number of bacteria in the two showed an order of magnitude difference.
[0161] The inhibitory effect of the polymer coating containing strong acid groups with bactericidal function formed based on electrostatic action on the growth of Pseudomonas aeruginosa was verified.
[0162] Test 4
[0163] The inhibition of Candida growth of the samples was verified according to the following steps.
[0164] The bacterial growth inhibition process was performed according to the standard described in Experiment 1, except that the Candida species solution was prepared for the experiment. The effect of inhibiting the growth of Candida was verified for Example 2, and the fungal growth process of the sample of Example 2 and the corresponding blank control sample were analyzed by placing them separately.
[0165] The results of the verification of the inhibition of Candida growth on the samples are as follows Figure 2As shown in the figure, due to the large amount of hydrogen ions adsorbed on the sample of Example 2, the normal growth of fungi in the fungal solution in which it was immersed was inhibited (the OD value was lower than 0.4 after 18 hours of fungal culture); while the OD value of fungi in the fungal solution immersed in the blank control sample was close to 1.4 after 18 hours of fungal culture. The number of fungi in the fungal solution immersed in the sample of Example 2 was much lower than the number of bacteria in the blank control sample, and the number of fungi in the two samples showed an order of magnitude difference.
[0166] The inhibitory effect of the polymer coating containing strong acid groups with bactericidal function formed based on electrostatic effect on the growth of Candida albicans was verified.
[0167] Test 5
[0168] Follow the steps below to verify the bactericidal (bacterial) effect of the sample.
[0169] Step 1, culturing the bacterial solution according to steps 1-4 described in Experiment 1, except that [preparing the Staphylococcus aureus seed solution];
[0170] Step 2: quantitatively dilute the bacterial solution centrifuged in step 1 with phosphate buffered saline (PBS) so that its absorption value at OD=600nm under ultraviolet absorption test is 0.008-0.01, corresponding to a bacterial concentration of 10 8 CFU / mL, and then the bacterial concentration was 10 8 The bacterial solution was further diluted with PBS to a bacterial concentration of 10 CFU / mL. 7 CFU / mL of bacterial solution is used for subsequent experimental operations;
[0171] Step 3: The samples in Example 3 and the corresponding blank control samples were respectively mixed with the bacterial concentration of 10 obtained in Step 2. 7 The bacterial solution of CFU / mL was spread on the agar plate by a spreader;
[0172] Step 4: Place the agar plate coated in step 3 in a constant temperature incubator at 37° C. and humidity RH=10% for 24 hours, and observe the bactericidal effects of the sample of Example 3 and the corresponding blank control sample.
[0173] The results of the bactericidal effect verification of the samples are as follows Figure 3 As shown: the agar plate coated with the blank control sample is full of bacterial colonies, while the agar plate coated with the sample of Example 3 has obvious inhibition rings due to the release of a large number of hydrogen ions carried by it.
[0174] The bactericidal effect of the polymer coating containing strong acid groups with bactericidal function formed by electrostatic action on Staphylococcus aureus was verified.
[0175] Test 6
[0176] Follow the steps below to verify the bactericidal (bacterial) effect of the sample.
[0177] According to the standard sterilization process described in Experiment 5, except that the Helicobacter pylori seed solution was prepared, the bactericidal property of Example 8 against Helicobacter pylori was verified, and the bactericidal effect of the sample of Example 8 and the corresponding blank control sample were analyzed separately.
[0178] The results of the bactericidal effect verification of the samples showed that the agar plate coated with the blank control sample was full of bacterial colonies, while the agar plate coated with the sample of Example 8 had an obvious antibacterial ring due to the release of a large amount of hydrogen ions carried by it.
[0179] The bactericidal effect of the polymer coating containing strong acid groups with bactericidal function formed based on electrostatic effect on Helicobacter pylori was verified.
[0180] Test 7
[0181] Follow the steps below to verify the bactericidal (bacterial) effect of the sample.
[0182] According to the standard sterilization process described in Experiment 5, except that the Pseudomonas aeruginosa seed solution was prepared for the experiment, the bactericidal property of Example 9 against Pseudomonas aeruginosa was verified, and the bactericidal effect of the sample of Example 9 and the corresponding blank control sample placed separately was analyzed.
[0183] The results of the bactericidal effect verification of the samples showed that the agar plate coated with the blank control sample was full of bacterial colonies, while the agar plate coated with the sample of Example 9 had an obvious antibacterial ring due to the release of a large amount of hydrogen ions carried by it.
[0184] The bactericidal effect of the polymer coating containing strong acid groups with bactericidal function formed based on electrostatic action on Pseudomonas aeruginosa was verified.
[0185] Test 8
[0186] The bactericidal (fungal) effect of the samples was verified according to the following steps.
[0187] According to the standard sterilization process described in Experiment 5, except that the Candida species solution was prepared, the bactericidal property of Example 4 against Candida was verified, and the bactericidal effect of the sample of Example 4 and the corresponding blank control sample were analyzed separately.
[0188] The results of the bactericidal effect verification of the samples are as follows Figure 4 As shown: the agar plate coated with the blank control sample is full of fungal colonies, while the agar plate coated with the sample of Example 4 has obvious inhibition rings due to the release of a large number of hydrogen ions carried by it.
[0189] The bactericidal effect of the polymer coating containing strong acid groups with bactericidal function formed by electrostatic action on Candida albicans was verified.
[0190] In summary, the results of the above embodiments and test examples show that the present invention has achieved the following technical effects:
[0191] 1. The method for preparing the polymer coating and the method for coating the surface of a substance of the present invention are simple and easy to implement;
[0192] 2. The present invention can make the surface of the coated object inactive, such as Escherichia coli, Staphylococcus aureus, Pseudomonas aeruginosa, Helicobacter pylori bacteria and Candida albicans, thereby achieving the effect of inhibiting the growth of microorganisms and killing bacteria.
[0193] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing the disclosure disclosed herein. This application is intended to cover any modification, use or adaptation of the present disclosure, which follows the general principles of the present disclosure and includes common knowledge or customary techniques in the art that are not disclosed in the present disclosure. The specification and examples are intended to be exemplary only, and the true scope and spirit of the present disclosure are indicated by the claims of the present application.
Claims
1. A polymer coating containing strong acid groups with bactericidal function, It is characterized in that It has the chemical structure shown in Formula 1: Where R 1 Strong acid group: sulfonic acid group -SO 3 , sulfate group-OSO 3 or benzenesulfonic acid group R 2 C n H 2n group, n is an integer greater than or equal to 1; R 3 is a methyl group or a hydrogen atom; x and y are degrees of polymerization, each selected from an integer ranging from 30 to 2000, and the ratio of x:y ranges from 0.1 to 0.
95.
2. A method for coating the surface of an object using the polymer coating according to claim 1, It is characterized in that the steps include: Step 1, cleaning the solid surface to be coated to obtain a clean solid surface; Step 2, preparing a strongly acidic aqueous solution of a strong electrolyte anion polymer, wherein the strong electrolyte anion polymer is one of polyvinyl sulfonic acid or its salt, polyvinyl sulfuric acid or its salt, polystyrene sulfonic acid or its salt, and the pH range of the solution is 0.5 to 1.5; Step 3, prepare a strongly acidic aqueous solution of a quaternary ammonium salt compound, wherein the chemical structural formula of the quaternary ammonium salt compound is CH 3 (CH 2 ) n N(R 3 ) 3 ·X, where R 3 is a methyl group or a hydrogen atom, n is an integer greater than or equal to 1, and X is Cl - Br - or I - , the solution pH range is 0.5 to 1.5; Step 4, mixing the strongly acidic aqueous solution of the strong electrolyte anion polymer prepared in step 2 with the strongly acidic aqueous solution of the quaternary ammonium salt compound prepared in step 3, or directly mixing the quaternary ammonium salt compound powder described in step 3 with the strongly acidic aqueous solution of the strong electrolyte anion polymer prepared in step 2, and obtaining an aqueous solution of a polymer having a chemical structure as shown in Formula 1 through electrostatic action between the two; Step 5, mixing the polymer aqueous solution obtained in step 4 with an organic solvent to obtain a polymer coating solution containing an organic solvent; Step 6: coating the polymer coating solution prepared in step 5 on the clean solid surface obtained in step 1, so that a polymer coating containing strong acid groups having a chemical structure as shown in formula 1 is formed on the surface of the object.
3. The method according to claim 2, It is characterized in that In step 1, the solid material to be coated includes: inorganic non-metallic materials, metal products, wood materials, artificial synthetic or natural polymer materials.
4. The method according to claim 2, It is characterized in that In step 2, the weight average molecular weight of the strong electrolyte anion polymer is in the range of 5 to 1000 kDa, and the mass concentration of the strong acid aqueous solution of the strong electrolyte anion polymer is in the range of 0.2 to 20 mg / mL.
5. The method according to claim 2, It is characterized in that In step 3, the mass concentration of the strongly acidic aqueous solution of the quaternary ammonium salt compound is 0.2-20 mg / mL, or in step 4, the mass concentration of the quaternary ammonium salt compound in the strongly acidic aqueous solution of the strong electrolyte anion polymer is 0.1-20 mg / mL.
6. The method according to claim 2, It is characterized in that In step 2 and step 3, the strongly acidic aqueous solution is obtained by adjusting the pH of a hydrochloric acid solution or a sulfuric acid solution to 0.5 to 1.
5.
7. The method according to claim 2, It is characterized in that In step 5, the organic solvent is one or more of methanol, ethanol, isopropanol, propanol, ethylene glycol, dimethyl sulfoxide, dimethylformamide, acetonitrile, acetone, chloroform or ethyl acetate; The volume ratio of the organic solvent to the aqueous solution in the polymer coating solution is in the range of 0.1 to 0.
5.
8. The method according to claim 2, It is characterized in that In step 6, the coating method of the polymer coating solution includes: dipping, spin coating, spraying, electrostatic spinning or inkjet printing.
9. The method according to claim 8, It is characterized in that The coating time is 10 seconds to 80 minutes, the coating temperature is 10 to 50° C., and the coating times are more than 1 time.
10. An application of a method for coating the surface of an object using the polymer coating according to claim 1 or the polymer coating according to any one of claims 2 to 9 in inhibiting the growth of microorganisms on the surface of the object, preferably, the microorganisms include Escherichia coli, Staphylococcus aureus, Pseudomonas aeruginosa, Helicobacter pylori bacteria or Candida fungi.
Citation Information
Patent Citations
Elastomeric article with antimicrobial coating
CN101351163A
Antibacterial coating agent, preparation method thereof, and antibacterial coating
CN108276820A
Bionic polymer and method for preparing durable double-bionic polymer coating and application thereof
CN109796616A