Film-forming composition and application thereof
The hydrophobic coating formed by the film forming composition solves the problems of poor hydrophobicity and edge-angle effects of the circuit board protective material, achieves better waterproof and corrosion-proof effects, and ensures the electrical connection stability of the connector.
Patent Information
- Application Number
- CN202410428245.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-10
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-04-10
AI Technical Summary
The existing circuit board protective materials have poor hydrophobicity and severe edge-angle effects, resulting in too thin coating at corner positions, affecting the electrical connection and protection effect of the connector.
Using a film-forming composition, including hydrophobic polymer I and hydrophobic polymer II, a hydrophobic coating is formed by physical mixing to ensure that the water droplet angle is greater than or equal to 90 degrees, the viscosity is greater than or equal to 10,000 mPa·S, and a relatively small amount is formed at the corner position. Thick protective coating.
Improves the waterproof performance and corrosion resistance of the circuit board, avoids short circuits and corrosion failures, ensures that the electrical connection of the connector is not affected, and maintains good conductivity during multiple plug-ins and unplugs.
Smart Images

Figure BDA0004785547630000081 
Figure BDA0004785547630000082 
Figure HDA0004785547730000011
Abstract
Description
Technical Field
[0001] The invention relates to the field of electronic component packaging materials, and in particular to a film-forming composition and application thereof. Background Art
[0002] Electronic devices contain circuit boards, on which connectors, chips, chip resistors and capacitors, wing-shaped pin devices and other electronic components are assembled. For the overall protection structure design of electronic devices, it is usually impossible to completely prevent external liquids (such as water, rain, sweat, daily liquids, etc.) from entering the interior of the electronic devices. For example, when the waterproof level is below IPX4, in daily use scenarios, external liquids may enter the interior of the electronic devices through openings on the device shell, gaps between structural parts or breathable parts, and form droplets inside the device through diffusion, condensation and other processes. When the droplets contact the circuit board components, it is easy to cause corrosion failure and short circuit of the electronic components. For example, when there is a certain voltage difference between two adjacent pins of an electronic component, when there are water droplets or water films between the two adjacent pins, rapid short circuit failure is likely to occur (usually within a few hours, due to low insulation impedance or excessive leakage current caused by rapid electrochemical migration corrosion). Even if such rapid short circuit failure does not occur, the droplets continue to be in the electronic device, which will cause corrosion of the exposed metal on the electronic components, and then still cause the failure of the electronic device. Therefore, it is necessary to provide a protective coating on the circuit board and the components therein to prevent water and other components from entering the interior of the electronic device and causing corrosion to the components inside the electronic device.
[0003] However, existing circuit board protective materials generally have problems such as poor hydrophobicity, severe angular effect (which easily leads to too thin coating at corners), and being unfavorable for electrical connection between connectors on the circuit board and other connectors, which limits their application.
[0004] Specifically, the related art uses conformal coating materials (commonly known as three-proof paint) to enhance the protection of circuit board components. The coating materials for circuit boards mainly use systems such as polyacrylate, silicone, polyurethane, alkyd resin, and fluorine-containing materials. The conformal coating (usually a thin layer of insulating coating, the thickness of which is generally about 15um to 150um) can be applied to the circuit board components by spraying, brushing, dipping, etc., to play a protective role such as moisture-proof, salt spray-proof, and mildew-proof. However, for circuit boards equipped with connectors (such as BTB connectors, USB interfaces, radio frequency connectors, etc.), this type of conformal coating material is not applicable. Specifically, when the connector of the circuit board is assembled with another connector, the connecting terminals of the two connectors need to be connected together so that the two connectors are electrically connected (electrically conductive). When the conformal coating material is used to form an insulating coating on the surface of the connector of the circuit board, the insulating coating cannot be effectively pierced or displaced by the connecting terminals of the two connectors, thereby affecting the electrical conductivity of the two connectors, especially when the connector usually needs to be plugged in and out many times during the processing or use of the equipment, and the tolerance for the insulating coating existing in the cross section of the connecting contact is lower. Therefore, when using the above-mentioned conformal coating material to protect a circuit board with a connector installed, when applying the coating material on a single board, the connector usually needs to be shielded to prevent the surface of the connector contact from being covered by the insulating coating formed by the coating material, thereby avoiding affecting the effective electrical connection between the connectors. However, this will make the connector on the circuit board a weak point of the electronic device. Once external liquid enters the interior of the electronic device, it is easy for short circuits and corrosion failures to occur at the connector position on the circuit board.
[0005] The vacuum chemical vapor deposition method is used to deposit a nano-hydrophobic film (whose thickness is usually tens to hundreds of nanometers) on the surface of the substrate. It mainly cleans and activates the surface of the substrate through plasma discharge in a vacuum environment, and provides energy for opening the chemical bonds of the coating material molecules, promoting the polymerization reaction to continue, so that the substrate surface activated by plasma is combined with the coating material monomer molecules through chemical bonds. At the same time, the monomer molecules continue to polymerize and grow, and a nano-scale thick organic molecular protective layer (nano-hydrophobic film) is formed on the surface of the coated substrate. The process mainly involves placing the whole machine to be processed into a cavity, evacuating the vacuum, generating plasma gas, injecting hydrophobic reaction monomers, depositing a nano-hydrophobic film on the surface of the whole machine, breaking the vacuum, and taking out the whole machine. The coating material used is usually a fluorine-containing material with certain hydrophobic properties, usually a fluorocarbon compound. If a nano-hydrophobic film is deposited on the entire surface of a circuit board using vacuum chemical vapor deposition, the circuit board and devices such as connectors on its surface can be protected to a certain extent. However, if the thickness of the nano-hydrophobic film is large, it is not easy to be pierced by the connecting terminals of the connector, which will affect the electrical connection between the connector on the circuit board and other connectors. If the thickness of the nano-hydrophobic film is reduced so that it can be pierced by the connecting terminals of the connector, the nano-hydrophobic film is too thin and has a poor protective effect on the circuit board, which cannot meet the anti-corrosion requirements of circuit board components in electronic equipment. At the same time, the vacuum chemical vapor deposition method also has defects such as complex process and high cost. These factors restrict its application in circuit board protection.
[0006] Therefore, the protective materials in the prior art generally have problems such as being unfavorable for the electrical connection between the connector on the circuit board and other connectors.
[0007] In addition, devices on circuit boards usually have corner structures (for example, the edges / pointed corners of device housings or 3D shaped parts (such as 3D pins)), and existing protective materials generally have serious edge effects, which makes the protective film layer at the corners too thin. Specifically, when the protective material is applied to the surface of the circuit board and the components on the circuit board, the uncured protective material has a large fluidity, which causes the protective material at the corners of the circuit board components to flow easily, making the coating (protective film layer) formed at the corners too thin, which is prone to failure when exposed to water, making it difficult for the circuit board to meet the reliable power-on requirements in the single-board component immersion and water spray test scenarios.
[0008] In addition, the water contact angle of the coating formed by the existing protective materials is usually less than 90 degrees, which makes it difficult to achieve the hydrophobic properties required for the circuit board protective coating.
[0009] In summary, existing circuit board protective materials generally have problems such as poor hydrophobicity, serious angular effect (which easily leads to too thin coating at the corners), and the protective coating formed is not easily punctured, thereby affecting the electrical connection between the connector on the circuit board and other connectors, which need to be solved urgently. Summary of the invention
[0010] The present invention provides a film-forming composition and its application, so as to at least solve the problems existing in the prior art, such as poor hydrophobicity of circuit board protective materials, serious angular effect (which easily leads to too thin coating at corner positions), and the formed protective coating being not easily punctured, thereby affecting the electrical connection between a connector on the circuit board and other connectors.
[0011] In one aspect of the present invention, a film-forming composition is provided, comprising the following components A to C: A, a hydrophobic polymer I, wherein the hydrophobic polymer I is a solid polymer; B, a hydrophobic polymer II, wherein the hydrophobic polymer II is a film-forming polymer; and C, an organic solvent.
[0012] According to one embodiment of the present invention, the water drop angle of the hydrophobic polymer II is greater than or equal to 90 degrees.
[0013] According to one embodiment of the present invention, the viscosity of the hydrophobic polymer II is greater than or equal to 10000 mPa·S.
[0014] According to one embodiment of the present invention, the hydrophobic polymer II comprises a liquid polymer.
[0015] According to one embodiment of the present invention, the hydrophobic polymer II includes silicone oil and / or linear polyolefin.
[0016] According to one embodiment of the present invention, the water drop angle of the hydrophobic polymer I is greater than or equal to 90 degrees.
[0017] According to one embodiment of the present invention, the hydrophobic polymer I includes one or more of silicone resin, polyolefins, and fluorinated polymers.
[0018] According to one embodiment of the present invention, the hydrophobic polymer I and the hydrophobic polymer II are made of the same material.
[0019] According to one embodiment of the present invention, the hydrophobic polymer I and the hydrophobic polymer II belong to an organosilicon system, or the hydrophobic polymer I and the hydrophobic polymer II belong to a polyolefin system.
[0020] According to one embodiment of the present invention, based on the total mass of the film-forming composition, the sum of the mass fractions of the hydrophobic polymer I and the hydrophobic polymer II is greater than or equal to 20%.
[0021] According to one embodiment of the present invention, based on the total mass of the film-forming composition, the mass fraction of the hydrophobic polymer I is greater than the mass fraction of the hydrophobic polymer II.
[0022] According to one embodiment of the present invention, the film-forming composition satisfies the following conditions: after the organic solvent evaporates, a portion of the hydrophobic polymer I dissolves in the hydrophobic polymer II and is physically mixed with the hydrophobic polymer II to form a film matrix, and another portion of the hydrophobic polymer I precipitates to form particles during the volatilization of the organic solvent, and the particles are dispersed in the film matrix.
[0023] Another aspect of the present invention provides a structural part, comprising: a substrate; an electronic component disposed on the substrate; a hydrophobic coating located on a side of the substrate where the electronic component is disposed and existing on the surface of the electronic component; the hydrophobic coating is formed by the above-mentioned film-forming composition.
[0024] According to one embodiment of the present invention, the water drop angle of the hydrophobic coating is greater than or equal to 90 degrees.
[0025] According to an embodiment of the present invention, the electronic component has a corner structure, the hydrophobic coating covers the corner structure, and the thickness of the hydrophobic coating covering the corner structure is greater than 5 μm.
[0026] According to one embodiment of the present invention, the electronic component and / or the substrate has a planar area, the hydrophobic coating covers the planar area, and the thickness of the hydrophobic coating covering the planar area is 10 μm to 100 μm.
[0027] According to one embodiment of the present invention, the electronic component includes a pin, and the hydrophobic coating exists on the surface of the pin.
[0028] According to one embodiment of the present invention, the electronic component includes a connector, and the hydrophobic coating exists on the surface of the connector.
[0029] According to one embodiment of the present invention, a plurality of the electronic components are disposed on the substrate, and the hydrophobic coating is continuously distributed between at least two adjacent electronic components and covers the at least two adjacent electronic components.
[0030] Another aspect of the present invention provides a terminal product, comprising the above-mentioned structural component.
[0031] The implementation of the present invention has at least the following beneficial effects:
[0032] (1) The film-forming composition of the present invention has good hydrophobicity, and the formed hydrophobic coating has better waterproof effect, which can prevent the corrosion, short circuit failure and other problems of components such as circuit boards;
[0033] (2) The film-forming composition of the present invention can avoid the edge effect and form a thicker protective coating at the corner position (such as the surface of a 3D pin, etc.), thereby preventing the protective coating at the corner position from being too thin, thereby improving the protective effect on devices such as circuit boards.
[0034] (3) The protective coating formed by the film-forming composition of the present invention has good flexibility and other properties. The coating located on the surface of the connector contact can be easily punctured by the connecting terminals of the connector when squeezed by two matching connectors, thereby achieving electrical connection between the two connectors without affecting the electrical conduction during the plugging and unplugging of the connector.
[0035] Therefore, the film-forming composition provided by the present invention is a hydrophobic insulating material (insulating protective material) with good hydrophobicity and corrosion resistance. It is suitable for the protection of electronic components such as circuit boards, and is particularly suitable for the protection of circuit boards with connectors installed. It can form a protective coating on the surface of components such as circuit boards and their connectors to protect connectors and other devices on the circuit board as well as the entire circuit board. It will not affect the electrical connection between the connector on the circuit board and other connectors, and can ensure the thickness of the waterproof coating formed at the corners of the circuit board assembly to avoid problems such as corrosion and short circuit failure at the corners of the circuit board assembly. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a schematic structural diagram of a circuit board having a hydrophobic coating formed on the surface in one embodiment of the present invention;
[0037] Figure 2 FIG. 4 is a schematic structural diagram of a display module having a hydrophobic coating formed on the side surface in one embodiment of the present invention. DETAILED DESCRIPTION
[0038] In order to enable those skilled in the art to better understand the scheme of the present invention, the present invention is further described in detail below. The specific implementation methods listed below are only for describing the principles and features of the present invention. The examples are only used to explain the present invention and are not intended to limit the scope of the present invention. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.
[0039] An embodiment of the present invention provides a film-forming composition, comprising the following components A to C: A. hydrophobic polymer I (hereinafter referred to as polymer A), hydrophobic polymer I is a solid polymer; B. hydrophobic polymer II (hereinafter referred to as polymer B), hydrophobic polymer II is a film-forming polymer; C. an organic solvent (hereinafter referred to as solvent C).
[0040] In the embodiment of the present invention, the film-forming composition can form a film at room temperature, that is, when the above-mentioned film-forming composition is applied, the film-forming composition is coated on the device to be protected (such as the preset surface of a circuit board with a connector installed, etc.), and then the solvent C is volatilized at room temperature. After the solvent C is completely evaporated, a non-flowable film layer (or protective coating, protective layer, protective adhesive layer, or hydrophobic coating) is finally formed by the physical mixture of polymer A and polymer B.
[0041] In the film-forming process, polymer A and polymer B do not undergo chemical reaction, that is, in the physical blend of polymer A and polymer B, polymer A and polymer B are only physically mixed, there is no chemical bond between them, and no chemical cross-linking reaction occurs. Therefore, the film layer formed by polymer A and polymer B is easily punctured or pushed away when subjected to external force, so that the film-forming composition and the hydrophobic coating formed by the film-forming composition are suitable for circuit boards with connectors installed. When the hydrophobic coating is formed on the circuit board with the connector installed, the film layer can cover the connector to protect the connector and avoid problems such as short circuit and failure of the connector; at the same time, when the connector of the circuit board is connected to another connector, the hydrophobic coating present in the contact part (connection terminal) of the connector can be punctured or pushed away under the squeezing action of the connection terminals of the two connectors, thereby realizing the electrical connection of the connection terminals of the two connectors; at the same time, the hydrophobic coating has good flexibility and other properties, and the hydrophobic coating located in other parts of the connector surface (non-contact part) will not be damaged. Therefore, after the connector is plugged in and out, the hydrophobic coating (insulating protective material) still exists between different connector terminals, thereby maintaining the protection effect on the connector and the circuit board, and avoiding problems such as short circuit and corrosion failure when encountering water.
[0042] Generally, the above-mentioned physical blend (film layer) may include a film matrix and particulate matter present in the film matrix, wherein the film matrix mainly includes polymer A and polymer B, that is, it is mainly formed by a physical mixture of polymer A and polymer B, and the particulate matter mainly includes polymer A, that is, it is mainly formed by polymer A, and is randomly distributed in the film matrix, and the average size (particle size) of the particulate matter is in the micron level, for example, 2 to 100 μm, such as 2 μm, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm or a range consisting of any two of them.
[0043] Specifically, the above-mentioned film-forming composition can meet the following requirements: after the solvent C evaporates, part of the polymer A dissolves in the polymer B and physically mixes with the polymer B to form a film matrix, and another part of the polymer A precipitates to form particles during the volatilization of the solvent C, and the particles are dispersed in the film matrix (that is, this part of the polymer A precipitates in the form of particles and is dispersed in the film matrix).
[0044] Generally, during the volatilization process of solvent C, most of polymer A in the film-forming composition will dissolve in polymer B, thereby physically mixing with polymer B and forming a film matrix, while a small portion of polymer A will precipitate from the composition to form particulate matter, that is, after the volatilization of solvent C, most of polymer A will enter the film matrix, while a small portion of polymer A will exist in the film matrix in the form of particles, and the proportion of polymer A in the film matrix to the total mass of polymer A in the film-forming composition is greater than 50%, and the total mass of polymer A in the film-forming composition (also the total mass of polymer A in the hydrophobic coating) is substantially equal to the sum of the mass of polymer A in the film matrix and the mass of the particulate matter (i.e., the mass of polymer A forming the particulate matter).
[0045] During specific implementation, the hydrophobic coating can be sliced, and the area ratio of the particles in the preset area of the cross section (section) of the hydrophobic coating can be detected by a microscope. According to the detection results, there are particles in the preset area (the area observed by the microscope), and the area ratio of the particles (i.e., the ratio of the area occupied by the particles in the preset area to the total area of the preset area) is less than 50%, usually less than 25%, and specifically less than 10%. The hydrophobic coating is mainly formed by polymer A and polymer B, both of which are polymers with substantially the same density. Thus, the proportion of the polymer A forming the particles to the total mass of the polymer A in the film-forming composition is approximately the area ratio of the particles, that is, the proportion of the polymer A forming the particles to the total mass of the polymer A in the film-forming composition is less than 50%, and accordingly, the proportion of the polymer A in the film matrix to the total mass of the polymer A in the film-forming composition is greater than 50%. Among them, the microscope used can be a conventional high-power optical microscope in the art, and when the cross section of the hydrophobic coating is detected, the magnification of the high-power optical microscope can be 200 to 1000 times.
[0046] In the related art, in order to improve the properties of the film-forming composition such as viscosity, fluidity and hydrophobicity, it is usually necessary to add fillers (such as hydrophobic fillers) to the film-forming composition, but the filler and the organic substrate of the film-forming composition are not the same material system, and the compatibility between them is poor. After the protective coating is formed, phase separation is likely to occur. Specifically, there is a difference in the fluidity of the filler and the organic substrate under the action of external force, resulting in phase separation. For example, the filler will be enriched in a local position in the protective coating, and the dispersion uniformity in the protective coating is poor. In the embodiment of the present invention, the above-mentioned film-forming composition has suitable viscosity and fluidity, and the angular effect can be avoided. At the same time, in the hydrophobic coating formed by the above-mentioned film-forming composition, the particulate matter and the film matrix belong to the polymer material system, and the material of the particulate matter is mainly polymer A, and polymer A is also present in the film matrix, so that they have good compatibility, and thus the hydrophobic coating is not prone to phase separation (particulate matter and film matrix separation) and other problems.
[0047] Specifically, in the embodiment of the present invention, in the hydrophobic coating formed by the above-mentioned film-forming composition, the particulate matter is formed by the precipitation of polymer A in the film-forming composition, has good flexibility, and is in micron size. After the film-forming composition is used to form a hydrophobic coating on the surface of a circuit board with a connector installed, during multiple and long-term plugging and unplugging of the connector of the circuit board and other connectors, under the action of the matching force of the two connector terminals, the particulate matter in the hydrophobic coating can move with the film matrix without phase separation, thereby not affecting the plugging and unplugging performance of the connector, and not affecting the connection reliability of the two connectors under multiple plugging and unplugging.
[0048] In addition, polymer A is supersaturated relative to polymer B, that is, during the volatilization process of solvent C, there is polymer A that is not dissolved in polymer B. This part of polymer A precipitates in granular form, which can further increase the viscosity of the physical mixture formed by dissolving polymer A in polymer B, thereby improving the thixotropic properties of the physical mixture (thixotropic properties usually refer to shear stress, that is, the viscosity of the material decreases after encountering external stress, and the viscosity of the material recovers after the external force disappears), reducing the fluidity of the physical mixture, thereby avoiding the angular effect, and avoiding the problems of thin coating thickness and poor protection effect on the corner structure surface of the device (such as 3D pins).
[0049] Generally speaking, based on the total mass of the film-forming composition, the mass fraction of polymer A is greater than the mass fraction of polymer B, that is, the mass content of polymer A in the film-forming composition is greater than the mass content of polymer B. This is beneficial for part of polymer A to precipitate in granular form during the volatilization of solvent C, that is, to form particles dispersed in the film matrix.
[0050] For example, the mass ratio of polymer A to polymer B can be greater than or equal to 5:3, and the mass ratio of polymer A to polymer B can specifically be (5-30):3, for example, 5:3, 8:3, 10:3, 12:3, 15:3, 18:3, 20:3, 23:3, 25:3, 28:3, 30:3 or a range consisting of any two of them.
[0051] In the embodiment of the present invention, polymer A can be dissolved in polymer B, that is, after polymer A and polymer B are mixed in an appropriate ratio and sufficiently stirred, a uniform mixture without a suspended phase can be formed. The uniform state of the mixture can be a long-term state, for example, no suspended phase appears after standing for a long time at room temperature, and the uniformity of the system can be maintained. Alternatively, the uniform state of the mixture can also be a short-term state, for example, no suspended phase can be achieved under external effects such as stirring or heating.
[0052] Generally, the mixing ratio of polymer A in polymer B is lower than the solubility of polymer A in polymer B (i.e., the solubility of polymer A in polymer B is x%, i.e., on average, xg of polymer A can be dissolved in 100g of polymer B at most, then the mixing ratio of polymer A and polymer B is lower than x% (i.e., the amount of polymer A added in 100g of polymer B is lower than xg on average)), polymer A can be completely dissolved in polymer B to form a mixture in a uniformly dispersed state without suspension, and the mixture can be specifically transparent. When the mixing ratio of polymer A in polymer B is greater than the solubility of polymer A in polymer B, polymer A is usually partially dissolved in polymer B.
[0053] In some preferred embodiments, after polymer A is dissolved in polymer B, the uniform state of the resulting mixture is long-term. In specific implementations, the types and amounts of polymer A and polymer B can be adjusted to achieve a long-term uniform state of the mixture, and a film-forming composition can be formed according to such conditions.
[0054] According to further research by the inventors, during the volatilization of solvent C, non-flowable polymer A is dissolved in polymer B with good fluidity. By adjusting the solid content and other conditions of the film-forming composition, the fluidity of the physical blend formed by dissolving polymer A in polymer B during the volatilization of solvent C can be further improved, making it difficult to flow or basically non-flowable. In particular, supersaturation of polymer A relative to polymer B can be achieved, and part of polymer A can be precipitated to form particles dispersed in the physical blend, so as to further improve the thixotropic properties of the physical blend and avoid problems such as thin film thickness formed on the surface of the device corner structure. Generally, in order to achieve good anti-corrosion effect, the film thickness at the device corner position (such as the pin) is preferably greater than 5 μm, and more preferably greater than or equal to 10 μm.
[0055] Taking the above factors into consideration, the solid content of the film-forming composition (the sum of the mass fractions of polymer A and polymer B based on the total mass of the film-forming composition) is preferably greater than or equal to 20%, preferably greater than or equal to 25%.
[0056] Therefore, in the embodiment of the present invention, by adding components such as polymer A to the film-forming composition, the viscosity of the film-forming composition can be increased, specifically, the viscosity of the film-forming composition can be made to be more than 20%, so that when the film-forming composition is applied to the surface of a device such as a circuit board equipped with a connector, the problem of thin film layer thickness formed at the corner position due to excessive fluidity of the film-forming composition can be avoided. Specifically, the film layer thickness on the surface of the corner structure can be made to be more than 10μm.
[0057] In addition, solvent C is mainly used to dissolve and disperse polymer A and polymer B, reduce the viscosity of the film-forming composition, and enable it to be coated into a film through processes such as spot coating (spray spot coating), spray coating (atomized spray coating), curtain coating (curtain coating), dipping, and brushing (that is, the film-forming composition can be applied to the surface of devices such as connectors through these processes), and at the same time contribute to the film-forming properties of the film-forming composition, for example, a film layer of lower thickness can be formed as needed.
[0058] Specifically, in the film-forming composition, the mass percentage of the solvent C (ie, the ratio of the mass of the solvent C to the total mass of the film-forming composition) may be less than or equal to 80%, and further may be less than or equal to 75%.
[0059] In some embodiments, in the film-forming composition, the mass percentage of solvent C can be 15% to 80%, for example, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80% or any two thereof.
[0060] Specifically, in the film-forming composition, the mass percentage of polymer A (i.e., the ratio of the mass of polymer A to the total mass of the film-forming composition) may be greater than or equal to 10%, less than or equal to 80% (i.e., the mass percentage of polymer A may be 10% to 80%), for example, less than or equal to 50%.
[0061] Illustratively, in the film-forming composition, the mass percentage of polymer A can be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80% or a range consisting of any two thereof.
[0062] Specifically, in the film-forming composition, the mass percentage of polymer B (i.e., the ratio of the mass of polymer B to the total mass of the film-forming composition) may be less than or equal to 40%, for example, less than or equal to 20%, or less than or equal to 15%.
[0063] In some embodiments, in the film-forming composition, the mass percentage of polymer B can be 3% to 40%, for example, 3%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40% or any two thereof.
[0064] Specifically, polymer A or polymer B can be dissolved in solvent C, that is, polymer A or polymer B and polymer C can form a uniform, transparent, uniform mixed system without a suspended phase after mixing. This uniform state can exist for a long time, but is not limited to this.
[0065] In some preferred embodiments, in order to improve the application process performance of the film-forming composition, in the above-mentioned film-forming composition, solvent C can completely dissolve polymer A and polymer B, that is, polymer A and polymer B are completely dissolved in solvent C. At this time, the film-forming composition is a uniform, transparent mixed system without a suspended phase, which is beneficial for the film-forming composition to have a lower viscosity, and can further improve the processing performance of the film-forming composition. It is suitable for atomization spraying, spray coating, dispensing, curtain coating, dipping, brushing and other processes, that is, the film-forming composition can be applied to devices such as circuit boards through these processes to form a film.
[0066] Specifically, the viscosity of the film-forming composition may be less than or equal to 1000 mPa·S, so that the film-forming composition can be coated into a film by atomization spraying, jet coating, glue dispensing, curtain coating, dip coating, brush coating and other processes.
[0067] In some embodiments, when the viscosity of the film-forming composition is less than or equal to 1000 mPa·S, the mass percentage of solvent C in the film-forming composition may be greater than or equal to 30% (correspondingly, the solid content of the film-forming composition is less than 70%), at this time, the mass percentage of polymer A is less than 70%, and the mass percentage of polymer B may be less than 40%.
[0068] In some specific embodiments, the viscosity of the film-forming composition can be 3 to 1000 mPa·S, for example, 3 mPa·S, 5 mPa·S, 10 mPa·S, 30 mPa·S, 50 mPa·S, 80 mPa·S, 100 mPa·S, 120 mPa·S, 150 mPa·S, 180 mPa·S, 200 mPa·S, 300 mPa·S, 400 mPa·S, 500 mPa·S, 600 mPa·S, 700 mPa·S, 800 mPa·S, 900 mPa·S, 1000 mPa·S or a range consisting of any two of them.
[0069] However, the dissolution conditions of polymer A and polymer B in solvent C, and the viscosity of the film-forming composition are not limited to the above embodiments. For example, in some other embodiments, when the atomization spraying process is not required, the viscosity of the film-forming composition may also be greater than 1000 mPa·S. In this case, it is allowed that the solvent C does not completely dissolve polymer A and polymer B. The mass percentage of solvent C in the film-forming composition may be, for example, less than 30% (correspondingly, the solid content of the film-forming composition is greater than or equal to 70%), usually less than 20% (correspondingly, the solid content of the film-forming composition is greater than or equal to 80%). In this case, the mass percentage of polymer A is less than 80%, and the mass percentage of polymer B may be less than 40%.
[0070] In the embodiment of the present invention, the polymer is a solid polymer A, which has basically no fluidity, that is, when polymer A exists alone, it is usually in a non-flowable solid state under normal temperature conditions. When the molecular weight of polymer A is low, it can also yield and flow under a certain force.
[0071] In addition, polymer A is hydrophobic, and its water drop angle (water contact angle) can be greater than or equal to 90 degrees (°), and further can be greater than or equal to 100°, which is conducive to the formed film layer having good hydrophobicity.
[0072] In some specific embodiments, the water drop angle of polymer A may be 90° to 120°, for example, 90°, 92°, 95°, 98°, 100°, 102°, 104°, 105°, 108°, 110°, 115°, 120° or a range consisting of any two thereof.
[0073] In addition, in addition to cooperating with polymer B and other components to regulate the viscosity of the film-forming composition and achieve a non-flowable film layer, polymer A can also improve the mechanical properties of the film layer formed by the film-forming composition. For example, it can regulate the hardness of the film layer formed on the surface of devices such as connectors, increase the film layer thickness and mechanical properties on the surface of the device's corner structure (such as angular edges), and further improve the protective effect of the device.
[0074] Specifically, polymer A may include a polymer with a cross-linked molecular structure, that is, its molecular structure is a cross-linked network structure. Polymer A may include one or more organic polymers with a cross-linked molecular structure. In some embodiments, polymer A may include one or more of silicone resin (cross-linked silicone resin), polyolefins, and fluorinated polymers. Among them, silicone resin may specifically include functionalized silicone resin, such as methyl silicone resin and / or phenyl silicone resin. Methyl silicone resin (or dimethyl silicone resin) is a polydimethylsiloxane with a cross-linked molecular structure. The outer layer of the fluorinated polymer molecule generally has a layer of fluorine (F) functional groups, making the fluorinated polymer hydrophobic. The fluorinated polymer may include one or more of fluorinated polyester, fluorinated polyacrylate, fluorinated silicone resin, etc.
[0075] Specifically, polymer A may be in a plurality of molecular weight distribution states. For example, polymer A may include a plurality of organic polymers having the same chemical structural formula units, and these organic polymers have different molecular weights. For example, polymer A may include a silicone resin with a molecular weight distribution of M1 and a silicone resin with a molecular weight distribution of M2.
[0076] Specifically, polymer A may be a non-polar polymer, such as a non-polar silicone resin. The non-polar organic resin has good flexibility, which is conducive to the formed film layer having good flexibility.
[0077] In some embodiments, to improve the gas corrosion resistance (eg, anti-sulfurization performance) of the circuit board assembly, polymer A may include a silicone resin with a high cross-linking density, such as a phenyl silicone resin.
[0078] In the embodiment of the present invention, polymer B is hydrophobic, and its water drop angle may be greater than or equal to 90°, and may further be greater than or equal to 95°, or greater than or equal to 100°, which is beneficial for the formed film layer to have good hydrophobicity.
[0079] In some specific embodiments, the water drop angle of polymer B may be 90° to 120°, such as 90°, 95°, 100°, 105°, 110°, 115°, 120° or a range consisting of any two thereof.
[0080] In an embodiment of the present invention, polymer B is a film-forming material having good fluidity (i.e., it has good fluidity when existing alone). Polymer B may specifically include a liquid polymer that can be used for film formation. When the liquid polymer exists alone, it is liquid at room temperature. When it exists alone, it may be oily, so that it has good film-forming properties and can be used for film formation. At the same time, it can dissolve polymer A to form a physical blend with higher viscosity, thereby achieving film formation on the surface of a 3D complex shape.
[0081] Specifically, polymer B may include a linear polymer with a linear molecular structure (i.e., its molecular structure is a linear structure) and / or a cross-linked polymer with a low degree of cross-linking. For example, polymer B may include one or more organic polymers (linear polymers) with a linear molecular structure and / or one or more cross-linked polymers with a low degree of cross-linking.
[0082] In some embodiments, polymer B may include silicone oil and / or linear polyolefin, wherein the silicone oil may specifically include linear silicone oil and / or cross-linked silicone oil with a low degree of cross-linking (cross-linked polymer with a low degree of cross-linking).
[0083] Specifically, the silicone oil may include one or more of polysiloxane, and a copolymer of a first monomer and a second monomer, wherein the first monomer is a siloxane polymer, which may specifically include one or more of polysiloxane, polysiloxane methacrylate, etc., the polysiloxane may include polydimethylsiloxane, the polysiloxane methacrylate may include polytrimethylsiloxane methacrylate, and the second monomer may include one or more of methylsiloxane, diphenylsiloxane, phenylmethylsiloxane, trimethylsiloxysilicate, acrylic acid (ester), alkane, or a polymer formed by polymerization of at least two of these compounds.
[0084] The linear silicone oil may include linear polysiloxane (polysiloxane having a linear molecular structure), for example, linear polydimethylsiloxane (linear dimethylpolysiloxane).
[0085] The cross-linked silicone oil with a low cross-linking degree may include polysiloxane with a low cross-linking degree and / or a copolymer of the first monomer and the second monomer.
[0086] Exemplarily, the cross-linked polymer with a low degree of cross-linking may include one or more of polydimethylsiloxane / methylsiloxane, polydimethylsiloxane / methylsiloxane / diphenylsiloxane, polydimethylsiloxane / methylsiloxane / phenylmethylsiloxane, polydimethylsiloxane / phenylmethylsiloxane, polydimethylsiloxane / diphenylsiloxane, polydimethylsiloxane (and) trimethylsiloxysilicate, polydimethylsiloxane (and) acrylic acid (ester) type / polytrimethylsiloxane methacrylate copolymer, alkane (and) acrylic acid (ester) type / polytrimethylsiloxane methacrylate copolymer, etc.
[0087] In the embodiments of the present invention, "A / B" and "A (and) B" respectively represent copolymers of A and B. For example, "polydimethylsiloxane / methylsiloxane" refers to a copolymer of polydimethylsiloxane and methylsiloxane; "acrylic (ester)" refers to acrylic and / or acrylic esters.
[0088] Specifically, a cross-linked polymer (cross-linked silicone oil) with a low degree of cross-linking is usually prepared by chain addition reaction of two types of polysiloxanes, which are linear polysiloxane a (linear silicone oil) and linear polysiloxane b (linear silicone oil), respectively. Polysiloxane a is a linear silicone oil with the following molecular structure, and its schematic diagram is as follows:
[0089] Polysiloxane a
[0090] Among them, R1 can be selected from hydrogen groups, alkenyl groups (such as vinyl groups), etc.; R2 can be selected from alkyl groups, aryl groups, cycloalkyl groups, and other functional groups (such as ether, carboxyl, amine, sulfonic acid, hydroxyl, ester, thiol), etc.
[0091] Generally, the linear polysiloxane b contains m groups that can react with R1 in the polysiloxane a, where m is an integer greater than or equal to 1, specifically 1 or 2; and n is an integer representing the number of repeating segments.
[0092] In short, the above-mentioned cross-linked silicone oil (polymer B) is prepared by a chain addition reaction of two or more silicone oils (linear), and the number of reactive groups between the linear silicone oils is m, preferably not more than 2 (i.e. preferably 1≤m≤2).
[0093] In general, cross-linked silicone polymers usually contain R 2 SiO 2 / 2 , R 3 SiO 1 / 2 、RSiO 3 / 2 、SiO 4 / 2 Unit, where R 2 Represents R 2 SiO 2 / 2 There are two R connected to Si in the unit, R 3 Represents R 3 SiO 1 / 2 There are three Rs connected to the Si in the unit. The more Rs there are, the lower the crosslinking degree of the crosslinked silicone polymer. For crosslinked silicone oil, the units that constitute the repeating chain segments of the polymer are mainly composed of R2SiO 2 / 2、 R 3 / 2 Composition, does not contain SiO 4 / 2 Units, while for cross-linked silicone resins (organic silicone resins), the units that constitute the repeating polymer segments are mainly SiO 4 / 2 Unit (SiO 4 / 2 In the unit, one Si connects to four Os, the bond is short, and the cross-linking degree is high).
[0094] Generally, cross-linked silicone resin can be prepared from two or more silicone oils (linear) through a chain addition reaction, and the silicone oil acting as a cross-linking agent contains more than or equal to 3 reactive groups.
[0095] Specifically, polymer B may be in multiple molecular weight distribution states. For example, polymer B may include multiple organic polymers having the same chemical structural formula units, and these organic polymers have different molecular weights. For example, polymer B may include organic silicone oil with a molecular weight distribution of M3 and organic silicone oil with a molecular weight distribution of M4.
[0096] In the embodiments of the present invention, materials such as silicone resin, silicone oil, solvent, etc. can be obtained by commercial means or the like, and there is no particular limitation on this.
[0097] Specifically, the material of polymer A and polymer B can be the same, that is, polymer A and polymer B belong to the same material system. For example, polymer A and polymer B both belong to the silicone system (polymer A is silicone resin and polymer B is silicone oil), or both belong to the polyolefin system (polymer A is a polyolefin with a cross-linked molecular structure and polymer B is a linear polyolefin). In this case, it is beneficial to improve the solubility of polymer A in polymer B. At the same time, in the film layer formed by the above-mentioned film-forming composition, the particulate matter and the film matrix belong to the same material system, have better compatibility, and are less likely to have problems such as phase separation, which is beneficial to improve the protection effect on devices such as circuit boards.
[0098] Generally speaking, when polymer A and polymer B are made of the same material, the infrared spectrum of polymer A and the infrared spectrum of polymer B have a high degree of similarity.
[0099] Of course, in the implementation of the present invention, the materials of polymer A and polymer B may also be different, that is, polymer A and polymer B belong to different material systems, but both belong to the same polymer system. In the film layer formed by the film-forming composition, the particulate matter and the film matrix will still maintain good compatibility, and problems such as phase separation of the particulate matter and the film matrix are not likely to occur.
[0100] In general, non-polar organic polymers are hydrophobic. Examples of non-polar polymers are polyolefins (such as the above-mentioned cross-linked molecular structured polyolefins (polymer A) and linear polyolefins (polymer B)). Examples of polyolefins include polyethylene, polypropylene, polystyrene, and the like.
[0101] In addition, when the side chains on the main chain of the organic polymer molecule are symmetrical structures and the side chain groups are mainly non-polar functional groups, the surface of the organic polymer is hydrophobic (also called hydrophobic). Since silicone polymers (polysiloxanes) usually have a layer of non-polar organic groups on the outer layer of the molecule and based on the symmetry of their molecular structure, silicone polymers (such as the above-mentioned silicone resins and silicone oils) are hydrophobic.
[0102] Specifically, silicone polymers are common hydrophobic materials. Highly cross-linked polysiloxanes with a cross-linked / network structure are called silicone resins, and polysiloxanes with a linear molecular structure or a low degree of cross-linking are called silicone oils.
[0103] In some embodiments, the molecular structural unit of the silicone resin is as shown in Formula 1, in which R3 is a side chain group, and the side chain groups at different positions may be the same or different.
[0104] Specifically, R3 in Formula 1 can be a non-polar group such as an alkyl group (such as a methyl group) or a phenyl group, and R3 is preferably a non-reactive functional group, such as a -H group, -OH group, vinyl group, alkoxy group, etc., to avoid chemical reactions that may occur under comprehensive conditions such as moisture and high temperature, thereby causing the performance of the final protective coating to deteriorate. The side chain group R3 in a small amount can also be a polar functional group or a reactive functional group, such as a side chain containing -H group, -OH group, vinyl group, alkoxy group, epoxy group, F group, H group, OH group, ester group, ether group, etc.
[0105]
[0106] For example, the organosilicon resin is a methyl organosilicon resin, that is, R3 in Formula 1 is a methyl group.
[0107] In some embodiments, the molecular structure of the silicone oil is as shown in Formula 2 below, wherein R4, R5, R6, R7, R8, R9, R 10 , R 11 All are side chain groups, R4~R 11 They may be the same or different. These side chain groups may contain any one of the functional groups such as alkyl, phenyl, -H, -OH, vinyl, alkoxy, epoxy, F, H, OH, ester, ether, etc. The side chain groups are preferably non-polar groups with no reaction activity, such as alkyl (such as methyl, ethyl, propyl, etc.), phenyl, etc.
[0108]
[0109] For example, the above-mentioned silicone oil is linear polydimethylsiloxane, that is, R4, R5, R6, R7, R8, R9, R 10 , R 11 All are methyl.
[0110] In the above-mentioned organosilicon polymer, the number of R functional groups (the number of R3 in Formula 1, the number of R4 to R 11The ratio of the total number of Si to Si (R / Si value) has a great influence on the properties of the silicone polymer. Generally, the R / Si value of silicone oil is >2, and the R / Si value of silicone resin is <2. Preferably, the R / Si value of silicone resin is <1.6.
[0111] Generally, the viscosity of polymer B may be greater than or equal to 10,000 mPa·S (10,000 mPa·S), that is, the embodiment of the present invention may adopt a hydrophobic polymer II with a viscosity greater than or equal to 10,000 mPa·S, which is beneficial to increase the viscosity of the film-forming composition, so that the film-forming composition avoids the angular effect and avoids the film layer formed on the corner structure surface of the device from being too thin, and at the same time can improve the film-forming performance of the film-forming composition.
[0112] In some embodiments, the viscosity of polymer B can be 100,000 mPa·S to 600,000 mPa·S, for example, 100,000 mPa·S, 150,000 mPa·S, 200,000 mPa·S, 250,000 mPa·S, 300,000 mPa·S, 350,000 mPa·S, 400,000 mPa·S, 450,000 mPa·S, 500,000 mPa·S, 550,000 mPa·S, 600,000 mPa·S or a range consisting of any two of them.
[0113] Generally, when the viscosity of polymer B is relatively high (for example, exceeding 1,000,000 mPa·S), solvent C can be first added to polymer B to reduce its viscosity, and then the film-forming composition is prepared (that is, polymer A, polymer B added with solvent C, and solvent C are mixed to prepare a film-forming composition). This is more conducive to uniform mixing of the components and is less likely to cause stratification, opacity of the system, and emulsion-like system.
[0114] Specifically, the film-forming composition or the film layer formed by the film-forming composition can be subjected to separation treatments such as extraction to separate polymer A and polymer B, and placed under room temperature conditions. The separated polymer A is solid at room temperature (i.e., polymer A in the film-forming composition is a solid polymer), and the separated polymer B is liquid at room temperature (i.e., polymer B in the film-forming composition is a liquid polymer).
[0115] Generally, polymer A and polymer B can satisfy the following requirement: the viscosity of the mixture of polymer A and polymer B (excluding other components such as solvent C) is greater than 1,000,000 mPa·S, which is beneficial to further improve the film-forming properties of the film-forming composition.
[0116] As mentioned above, the film layer formed by the above-mentioned film-forming composition is mainly formed by a physical blend of polymer A and polymer B. Therefore, the viscosity of the film layer formed by curing the film-forming composition is substantially equal to the viscosity of the mixture formed by mixing the above-mentioned polymer A and polymer B. The viscosity of the film layer is generally also greater than 1,000,000 mPa·S.
[0117] In the embodiment of the present invention, during the process of applying the film-forming composition to the device surface and curing it to form a film, the solvent C evaporates, and the formed film layer is mainly formed by a physical blend of polymer A and polymer B (including a film matrix and particles formed by polymer A), wherein the solvent C may evaporate through at least one of the following processes: (1) evaporate after the film-forming composition is applied to the device; (2) evaporate during the process of applying the film-forming composition to the device surface, and a small amount of residual solvent C evaporates after the coating is completed, but is not limited to this.
[0118] Specifically, solvent C may include non-polar solvents and / or polar solvents, and may specifically include one or more of alcohols, hydrocarbons, ethers, ketones, halogenated hydrocarbons, aldehydes, and silicones. Among them, alcohols include, for example, one or more of methanol, ethanol, and propanol; hydrocarbons may include aliphatic hydrocarbons, and aliphatic hydrocarbons may include alkanes, and may specifically include chain alkanes and / or isochain alkanes, for example, one or more of hexane, isooctane, and decane (such as n-decane); ethers include, for example, furans (such as tetrahydrofuran) and / or dialkyl ethers (such as diethyl ether); halogenated hydrocarbons may include all halogenated hydrocarbons and / or partially halogenated hydrocarbons; silicones are generally low molecular weight silicone oils (i.e., silicone oil solvents, whose molecular weight is generally less than 1000), which may include linear silicones and / or cyclic silicones, for example, including decamethylcyclopentasiloxane (D5). Solvent C may be one of the solvents, or a mixed solvent containing multiple solvents, for example, solvent C may be a low molecular weight mineral oil mainly composed of alkanes and aromatic hydrocarbons.
[0119] In an embodiment of the present invention, in order to further improve the performance of the film-forming composition and the film layer formed by the above-mentioned film-forming composition, the film-forming composition may include one or more functional additives such as a leveling agent, a stabilizer, an anti-aging agent, a fluorescent indicator, etc. These functional additives can all be conventional materials in the field and are not particularly limited.
[0120] In an embodiment of the present invention, in order to further improve the hydrophobicity or oleophobicity of the film-forming composition, the film-forming composition may include a hydrophobic filler and / or an oleophobic filler. The hydrophobic filler includes, for example, insulating silica particles surface-treated with silane, and the oleophobic filler includes, for example, insulating silica particles surface-treated with fluorine-based materials, etc., but is not limited thereto.
[0121] In the embodiment of the present invention, the film layer formed by the film-forming composition has good hydrophobicity, and the water drop angle of the film layer can be greater than or equal to 90°, and further can be greater than or equal to 100°, which can achieve good protection effects on electronic components such as circuit boards. Studies have shown that when the film-forming composition of the embodiment of the present invention is used to form a film layer on the surface of a device such as a connector, even if there are defects of hundreds of microns on the surface or local positions inside the film layer (such as the film layer at the corner position of the device), the film layer has good hydrophobicity, which can still prevent water from contacting the device and prevent device corrosion, and is not prone to short circuit failure and other problems in water immersion scenarios.
[0122] The film-forming composition of the embodiment of the present invention is suitable for protecting structural parts such as circuit board assemblies, and is particularly suitable for application scenarios where connectors are assembled on circuit boards. The circuit board (PCB) is part of an electronic device. The electronic device can be a consumer electronic device, such as a smart phone, a smart watch, a smart door lock, a smart tablet, a PC, a home network terminal, etc., or a communication electronic device, such as a wireless communication base station, an access network device, etc., or an industrial electronic device, such as a power supply, a controller, etc. The circuit board can be a rigid PCB or a flexible PCB, etc.
[0123] An embodiment of the present invention also provides a structural member, including: a substrate; an electronic component disposed on the substrate; a hydrophobic coating located on a side of the substrate where the electronic component is disposed and existing on the surface of the electronic component; the hydrophobic coating is formed by the above-mentioned film-forming composition.
[0124] Specifically, the substrate may include a circuit board, but is not limited thereto.
[0125] Specifically, the electronic components may include one or more of connectors, wing-shaped pin devices, chip electronic components (such as chip resistors, chip capacitors), integrated circuit (IC) components, power chips, packaged devices (such as SOP packaged devices), display modules, etc. The connectors may include board-to-board connectors, BTB connectors, board-to-cable connectors, RF connectors, power connectors, IC socket connectors, video / USB / audio and other special interface connectors, etc.
[0126] Among them, when a connector is installed on the substrate, there is a hydrophobic coating on the surface of the connector, which can protect the connector without affecting the electrical connection between the connector and other connectors.
[0127] Specifically, the water drop angle of the hydrophobic coating can be greater than or equal to 90°, and further can be greater than or equal to 100°. It has good hydrophobicity and can improve the protection effect of devices such as connectors on structural parts.
[0128] In some embodiments, the water drop angle of the hydrophobic coating can be 90° to 120°, for example, 90°, 95°, 100°, 105°, 110°, 115°, 120°, or a range consisting of any two thereof.
[0129] In an embodiment of the present invention, a hydrophobic coating is present on the surface of a structural member and electronic components (electronic parts) arranged on the structural member. The electronic components include components that are sensitive to external pollution conditions such as grease, salt water, etc. The surfaces of these components are exposed to the air. By forming a hydrophobic coating on their surfaces, these components can be prevented from being corroded.
[0130] Specifically, the electronic component and / or substrate has a planar area (eg Figure 1 The hydrophobic coating covers the plane areas, and the thickness of the hydrophobic coating covering the plane areas (i.e., the hydrophobic coating located on the surface of the plane areas) can be 10 μm to 100 μm, for example, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm or a range consisting of any two of them.
[0131] In addition, electronic components have corner structures (such as Figure 1 The hydrophobic coating covers the corner structure. Due to factors such as the angular effect, the hydrophobic coating covering the corner structure (i.e., the hydrophobic coating located on the surface of the corner structure) is the thinnest part of the entire hydrophobic coating. The thickness of the hydrophobic coating covering the corner structure is less than the thickness of the hydrophobic coating covering the flat area (e.g., Figure 1 The thickness of the hydrophobic coating on the corner structure surface in regions Q1, Q2, Q3, Q4, etc. is less than the thickness of the hydrophobic coating on the plane area (such as the third plane area 10, the first plane area 210, the second plane area 220, etc.)
[0132] In the embodiment of the present invention, the thickness of the hydrophobic coating covering the corner structure may be greater than or equal to 5 μm, and may further be greater than or equal to 10 μm.
[0133] In some embodiments, the thickness of the hydrophobic coating covering the corner structure may be 5-20 μm, for example, 5 μm, 8 μm, 10 μm, 13 μm, 15 μm, 18 μm, 20 μm, or any two thereof.
[0134] Specifically, the electronic component includes a pin, a hydrophobic coating is present on the surface of the pin, the pin has a corner structure, and the thickness of the hydrophobic coating on the surface can be greater than or equal to 5 μm, and further can be greater than or equal to 10 μm.
[0135] Generally, the above-mentioned pins may be 3D pins, such as wing pins of wing pin devices, solder terminal pins of chip electronic components, SOP pins of SOP packaged devices, pins (terminals) of connectors, etc.
[0136] In the embodiment of the present invention, the thickness of the hydrophobic coating at any part refers to the distance (usually the minimum distance) from the side of the hydrophobic coating at the part in contact with the electronic component (or substrate) to the side of the hydrophobic coating at the part away from the electronic component (or substrate). For example, Figure 1 As shown, the thickness of the hydrophobic coating 3 on the third plane area 10 refers to the distance from the side of the hydrophobic coating 3 on the third plane area 10 that contacts the substrate to the side of the hydrophobic coating that is away from the base, and the thickness of the hydrophobic coating 3 on the corner structure in area 1 refers to the distance from the side of the hydrophobic coating 3 that is released from the solder terminal pin 211 to the side of the hydrophobic coating 3 that is away from the solder terminal pin 211.
[0137] Specifically, a plurality of electronic components are arranged on the substrate, and the hydrophobic coating is continuously distributed between at least two adjacent electronic components and covers at least two adjacent electronic components.
[0138] Generally speaking, when there are water droplets inside an electronic device, the water droplets will come into contact with the exposed contacts of electronic components such as connectors, thereby causing corrosion to the exposed contacts of the electronic components. Therefore, a hydrophobic coating needs to be provided on the exposed contact surfaces of the electronic components. Preferably, a hydrophobic coating is provided on the surface of the circuit board, and on the surfaces of electronic components such as chip electronic components, packaged devices, and connectors (including exposed contact surfaces) arranged on the circuit board. The hydrophobic coating is distributed in the form of a thin film on the surfaces of these devices.
[0139] Specifically, the embodiments of the present invention can coat the entire board of electronic components such as circuit boards installed with connectors, that is, form a hydrophobic coating on the entire surface of the circuit board (including the surface of the connector contacts). As mentioned above, the hydrophobic coating can be easily punctured or pushed away by the terminals of the connector, and will not affect the plug-in connection between the connector of the circuit board and other connectors, that is, it will not affect the electrical connection between the two connectors. At the same time, the hydrophobic coating has good flexibility, and during the plug-in and pull-out process of the two connectors, the hydrophobic coating on other parts will not be damaged, thereby maintaining the protective effect of the hydrophobic coating on connectors and other devices.
[0140] As mentioned above, the film-forming composition of the embodiment of the present invention can be applied to the device surface by spot coating (spray coating), spray coating (atomized spray coating), curtain coating (curtain coating), dipping, brushing and other processes, and cured to form a film on the device surface to form a protective coating. Among them, during the application process, it can be applied by a single coating process (i.e., one-time application), or by multiple coating processes. For example, the above-mentioned film-forming composition can be used to protect the entire circuit board assembly. Specifically, the film-forming composition can be sprayed on the entire circuit board assembly surface by an atomized spray process (atomized spray process), and a hydrophobic coating can be formed by multiple spraying and superposition to avoid problems such as local defects in the coating formed by a single coating process.
[0141] Among them, when applied through multiple coating processes, the thickness of the film layer formed after each coating (the coating thickness of a single coating) can be 5μm to 50μm. After multiple coatings, a hydrophobic coating with a thickness of 10μm to 100μm is finally formed. Relatively speaking, if the coating thickness of a single coating is too thin (<5μm), the probability of local defects (such as local coating is too thin, or even exposed (exposing the device surface)) is relatively high, and if the coating thickness of a single coating is too thick, the surface smoothness of the hydrophobic coating formed is poor (for example, it is easy to have uneven appearance phenomena such as orange peel). Although the coating surface will become smooth after being placed for a period of time, it will affect the processing efficiency.
[0142] Generally, due to factors such as the spraying angle and the fluidity of the film-forming composition during the spraying process, the coating thickness on the plane of the substrate surface will be higher than the coating thickness on the corner structure (such as 3D pins) of the electronic component disposed on the substrate. However, by using the film-forming composition of the embodiment of the present invention, a higher coating thickness covering the corner structure can be achieved at the same plane coating thickness.
[0143] In addition, for corner positions such as 3D pins of electronic components, the film-forming composition can be applied through a spot coating process, which is beneficial to further improve the coating thickness and consistency on the surface of the corner position, and avoid the local coating thickness being too thin due to factors such as the spraying angle.
[0144] In addition, when the thickness of the hydrophobic coating on the surface of the connector contact is too large, even if the electrical conduction of the connector is not substantially affected after a single word or a few plug-ins, the conduction resistance of the connector may fluctuate after multiple plug-ins. Therefore, in order to further avoid the influence on the electrical conductivity of the connector, the thickness of the hydrophobic coating is preferably not more than 100 μm. In specific implementation, after the hydrophobic coating is formed on components such as circuit boards, performance tests such as conventional long-term salt spray corrosion tests in the art (for example, a neutral sodium chloride aqueous solution with a concentration of 5% salt spray test for 500 to 1000 hours) can be performed to make the thickness of the hydrophobic coating and other parameters meet the test requirements (for example, the circuit board component is immersed in water and powered on for several days without functional abnormalities, and the circuit board is sprinkled with water and powered on for dozens of days without functional abnormalities, etc.). Thus, the coating thickness of the film-forming composition can be controlled in combination with the above factors to form a hydrophobic coating of a preset thickness.
[0145] In the embodiment of the present invention, the hydrophobic coating on the structural part can be redissolved when encountering solvent C (such as a non-polar solvent). Therefore, when the above structural part needs to be repaired, the solvent C (such as a non-polar solvent) can be used to dissolve the hydrophobic coating. Therefore, the embodiment of the present invention also has the advantages of easy removal of the hydrophobic coating and good reworkability of the structural part, which is conducive to practical application.
[0146] In the embodiment of the present invention, when the hydrophobic coating is scratched by a mechanical external force, if the scratched portion is damaged, the damaged portion can be repaired by spot coating with a film-forming composition.
[0147] In the embodiment of the present invention, the hydrophobic coating is mainly formed by physically blending polymer A and polymer B. At high temperatures (such as welding temperature (>200°C)), the hydrophobic coating can soften, and high-density molten solder can enter under the hydrophobic coating and weld with structures such as pads located under the hydrophobic coating. Therefore, even if such a hydrophobic coating is applied to the surface of the circuit board, it still has good reworkability.
[0148] In some embodiments, Figure 1 As shown, the structural member includes a substrate 1, and an electronic component arranged on the substrate, the electronic component is a chip electronic component (chip component) 21 and a wing-shaped pin device, the electronic component 21 and the wing-shaped pin device are arranged at intervals, and the side of the substrate 1 provided with the electronic component includes a third plane area 10, and the third plane area 10 is an area on the surface of the substrate 1 where no electronic components are arranged; two solder end pins (3D pins) 211 are arranged on the side of the chip electronic component 21 away from the substrate, and the solder end pins 211 have a corner structure (such as Figure 1The two soldering pins are arranged at intervals, and the side of the chip electronic component 21 facing away from the substrate includes a first plane area 210 located between the two soldering pins 211. The wing-shaped pin device includes a body 22 and a wing-shaped pin (3D pin) 221. The wing-shaped pin 221 is connected between the body 22 and the substrate 1. The body 22 and the wing-shaped pin 221 have corner structures at their bends (such as Figure 1 The side of the body 22 facing away from the substrate 1 includes a second plane area 220. The hydrophobic coating 3 is continuously formed on the entire surface of the side of the structure with electronic components (the hydrophobic coating is uninterrupted), that is, the hydrophobic coating 3 covers the surface of the substrate without electronic components (the third plane area 10), and covers the surface of the chip electronic components and the special-shaped lead devices. Figure 1 Area A in the figure only indicates the corner structure of a part of the structural member, and the corner structures of other areas of the structural member are not indicated.
[0149] In other embodiments, Figure 2 As shown, the structural member includes a substrate and an electronic component arranged on the substrate. The electronic component is a display screen module, which includes a polarizer 101, an optical adhesive layer (OCA adhesive layer) 102, a display panel (screen body) 103, and a cover glass 104 which are stacked in sequence.
[0150] Among them, optical film materials such as OCA adhesive layer 102 and polarizer 101 are sensitive to external pollution. For example, these optical materials are easily corroded when they encounter external polluting liquids such as sweat, which leads to the failure of the display module function. The hydrophobic coating 3 is arranged on the surface of these film materials, for example, Figure 2 As shown, a hydrophobic coating 3 is provided on the side edge of the screen (on the side of the film materials such as the polarizer 101, the optical adhesive layer 102 and the display panel 103 (the side is parallel to the thickness direction of the film materials)), which can protect the surface of these film materials and avoid problems such as functional abnormality and failure.
[0151] Specifically, in Figure 2 In the embodiment shown, a hydrophobic coating can be formed by a spraying process, and its thickness is, for example, 30 μm to 60 μm. Specifically, this thickness can be achieved by multiple spraying layers. During the spraying process, the screen display area can be shielded by a shielding tool to avoid spraying on the screen display area and affecting the screen display appearance.
[0152] An embodiment of the present invention further provides a terminal product, comprising the above-mentioned structural component.
[0153] Specifically, the above-mentioned terminal products can be electronic devices, and the electronic devices can be consumer electronic devices (consumer smart devices), such as smart phones, smart watches, smart door locks, smart tablets, PCs, home network terminals, IoT smart devices, etc., or communication electronic devices, such as access layer network equipment, wireless communication base stations, access network equipment, etc., or industrial electronic devices, such as power supplies, controllers, and transformers, etc., which involve high voltage operation.
[0154] In the embodiment of the present invention, the above-mentioned film-forming composition is used to form a hydrophobic coating on the surface of components such as circuit boards, which can improve the protection effect of components such as circuit boards in terminal products. When the terminal product encounters water ingress, etc., it is not easy to have problems such as rapid short circuit and corrosion failure of components such as circuit boards due to water contact, and corrosion failure of components such as circuit boards due to moisture. Therefore, the application reliability of the terminal product can be significantly improved.
[0155] The present invention is further described below through specific embodiments.
[0156] In the following examples and comparative examples, methyl silicone resin (polydimethylsiloxane with a cross-linked molecular structure) is a solid polymer with a water drop angle of about 102-104°; linear dimethylpolysiloxane is a liquid polymer with a water drop angle of about 100° and a viscosity of about 200,000 mPa·S.
[0157] In the following examples and comparative examples, unless otherwise specified, the coating thickness (hydrophobic coating thickness) refers to the average thickness.
[0158] Example 1
[0159] The film-forming composition of Example 1 is a mixture of dimethyl silicone resin (polymer A), linear dimethyl polysiloxane (polymer B) and n-decane (solvent C). The mass ratio of dimethyl silicone resin, linear dimethyl polysiloxane and n-decane is 20:5:75, and the viscosity of the film-forming composition is about 5 mPa·S.
[0160] The above-mentioned film-forming composition is used to spray the entire circuit board assembled with BTB connectors, 0402 chip resistors, 0201 chip capacitors, SOP packaged devices and other devices through an atomization spraying process. The coating thickness of the first spraying is 20 μm, and then a second spraying is performed on the coating formed by the first spraying. The coating thickness of the second spraying is 20 μm; wherein, spot coating is performed on the pins of the SOP packaged device (SOP pins) and the pin areas of the connector to ensure that the protective coating of the 3D pins of the device is well wrapped.
[0161] Example 2: The difference from Example 1 is that in the film-forming composition of Example 2, the mass ratio of dimethyl silicone resin, linear dimethyl polysiloxane and n-decane is 50:15:35, the viscosity of the film-forming composition is about 100 mPa·S, and the other conditions are the same as those of Example 1.
[0162] Example 3: The difference from Example 1 is that in the film-forming composition of Example 6, the mass ratio of dimethyl silicone resin, linear dimethyl polysiloxane and n-decane is 30:5:65, the viscosity of the film-forming composition is about 10 mPa·S, and the other conditions are the same as those of Example 1.
[0163] Comparative Example 1: No hydrophobic coating is provided on the structural member.
[0164] Comparative Example 2: The difference from Example 1 is that an alkyd resin-type conformal coating is used to replace the film-forming composition, that is, in Comparative Example 2, a conventional alkyd resin-type conformal coating is used to spray the entire circuit board assembled with devices such as BTB connectors, 0402 chip resistors, 0201 chip capacitors, and SOP packaged devices. During spraying, the BTB connector is shielded to avoid the formation of a hydrophobic coating on the surface of the BTB device; the other conditions are the same as in Example 1.
[0165] Comparative Example 3: The difference from Example 1 is that the film-forming composition of Comparative Example 3 is a mixture of linear dimethylpolysiloxane and n-decane solvent in a mass ratio of 20:80, and the other conditions are the same as those of Example 1.
[0166] The following tests were performed on the structural parts with hydrophobic coatings formed on the surfaces of the embodiments and comparative examples. The results are shown in Table 1.
[0167] 1. Hydrophobicity: Test the water drop angle of the hydrophobic coating.
[0168] 2. The hydrophobic coating was sliced and the cross-section was examined using a high-power microscope (magnification of approximately 200 times). It was found that the hydrophobic coating in Examples 1 to 3 included a film matrix and particles dispersed in the film matrix (the area of the particles accounted for less than 10%). The film matrix was formed by a physical mixture of polymer A and polymer B, and the particles were formed by polymer A. The average size of the particles was about 2-5 μm.
[0169] 3. Circuit board surface coating thickness H 平面 : Slice the coating on the surface of the circuit board (hydrophobic coating in the flat area) and measure its thickness to measure the thickness of the coating on the surface of the circuit board.
[0170] 4. SOP pin surface coating thickness H sop: Slice the coating on the surface of the SOP pin (the coating on the corner structure surface) and measure its thickness to measure the coating thickness on the surface of the SOP pin.
[0171] 5. The coating thickness H at the tip of the chip component 尖角 :Slice the coating at the sharp corner of the chip component solder end (the coating on the corner structure surface) and measure its thickness to measure the coating thickness H at the sharp corner of the chip component solder end 尖角 .
[0172] 6. Connector conductivity: Use the four-wire method to test the contact resistance R between the connector terminals.
[0173] 7. Circuit board protection performance: Immerse the entire structure (circuit board with a hydrophobic coating on the surface) in distilled water, observe the current changes during power-on operation, and record the time t when the current reaches 1mA.
[0174] Table 1
[0175] Test items Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Water drop angle 104° 102° 106° / 85° 99° <![CDATA[H 平面 ]]> 40μm 40μm 40μm / 40um 40μm <![CDATA[H sop ]]> 9μm 25μm 13μm / <1μm 2~4μm <![CDATA[H 尖角 ]]> 10μm 23μm 15μm / <1μm 3~5μm Resistor R <15mΩ <15mΩ <15mΩ / / <15mΩ Time t >60min >600min >120min <1min <1min <20min
[0176] It can be seen that, compared with Comparative Examples 1 to 3, Examples 1 to 3 have better hydrophobicity and better protective effect on the circuit board (the time t when the current reaches 1 mA is greater than 60 min).
[0177] In addition, compared with Comparative Examples 1 to 3, Examples 1 to 3 can significantly increase the thickness (H) of the hydrophobic coating at the corner positions (such as SOP pins, the sharp corners of the soldering ends of chip components, etc.) sop Not less than 9μm, H 尖角 Not less than 10 μm), indicating that the film-forming compositions of Examples 1 to 3 can avoid the angular effect and significantly improve the overall protective effect on structural parts such as circuit boards.
[0178] In addition, the hydrophobic coating in Examples 1 to 3 can be formed on the contact surface of the BTB connector without affecting the electrical connection between the connector and other connectors (resistance R < 15 mΩ).
[0179] This shows that the film-forming composition of the embodiment of the present invention has good hydrophobicity and can avoid the angular effect, effectively increasing the thickness of the hydrophobic coating formed at the corner position. At the same time, the hydrophobic coating formed by the film-forming composition has good flexibility and other properties, and can be formed on the surface of devices such as BTB connectors. The hydrophobic coating located on the surface of the connector contact is easily punctured or pushed away by the connecting terminals of the connector when squeezed by two matching connectors, thereby realizing the electrical connection between the two connectors. At the same time, during the plugging and unplugging process of the two connectors, the hydrophobic coating in other parts will not be damaged, thereby maintaining the protective effect of the hydrophobic coating on connectors and other devices.
[0180] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A film-forming composition, characterized in that It includes the following components A to C: A, a hydrophobic polymer I, wherein the hydrophobic polymer I is a solid polymer; B, a hydrophobic polymer II, wherein the hydrophobic polymer II is a film-forming polymer; C. Organic solvents.
2. The film-forming composition according to claim 1, characterized in that The water drop angle of the hydrophobic polymer II is greater than or equal to 90 degrees.
3. The film-forming composition according to claim 1 or 2, characterized in that The viscosity of the hydrophobic polymer II is greater than or equal to 10000 mPa·S.
4. The film-forming composition according to claim 1, characterized in that The hydrophobic polymer II includes a liquid polymer.
5. The film-forming composition according to claim 1 or 4, characterized in that The hydrophobic polymer II includes silicone oil and / or linear polyolefin.
6. The film-forming composition according to claim 1, characterized in that The water drop angle of the hydrophobic polymer I is greater than or equal to 90 degrees.
7. The film-forming composition according to claim 1 or 6, characterized in that The hydrophobic polymer I includes one or more of silicone resin, polyolefins, and fluorinated polymers.
8. The film-forming composition according to claim 1, characterized in that The hydrophobic polymer I and the hydrophobic polymer II are made of the same material.
9. The film-forming composition according to claim 8, characterized in that The hydrophobic polymer I and the hydrophobic polymer II belong to an organosilicon system, or the hydrophobic polymer I and the hydrophobic polymer II belong to a polyolefin system.
10. The film-forming composition according to claim 1, characterized in that Based on the total mass of the film-forming composition, the sum of the mass fractions of the hydrophobic polymer I and the hydrophobic polymer II is greater than or equal to 20%.
11. The film-forming composition according to claim 1 or 10, characterized in that: Based on the total mass of the film-forming composition, the mass fraction of the hydrophobic polymer I is greater than the mass fraction of the hydrophobic polymer II.
12. The film-forming composition according to claim 1, characterized in that The film-forming composition satisfies the following conditions: after the organic solvent evaporates, a portion of the hydrophobic polymer I dissolves in the hydrophobic polymer II and is physically mixed with the hydrophobic polymer II to form a film matrix, and another portion of the hydrophobic polymer I precipitates to form particles during the volatilization process of the organic solvent, and the particles are dispersed in the film matrix.
13. A structural member, characterized in that: include: substrate; An electronic component is disposed on the substrate; A hydrophobic coating is located on the side of the substrate where the electronic component is provided and exists on the surface of the electronic component; the hydrophobic coating is formed by the film-forming composition according to any one of claims 1 to 12.
14. The structural member according to claim 13, characterized in that The water drop angle of the hydrophobic coating is greater than or equal to 90 degrees.
15. The structural member according to claim 13, characterized in that: The electronic component has a corner structure, the hydrophobic coating covers the corner structure, and the thickness of the hydrophobic coating covering the corner structure is greater than 5 μm.
16. The structural member according to claim 13, characterized in that The electronic component and / or the substrate has a plane area, the hydrophobic coating covers the plane area, and the thickness of the hydrophobic coating covering the plane area is 10 μm to 100 μm.
17. The structural member according to claim 13, characterized in that The electronic component comprises a pin, and the hydrophobic coating is present on the surface of the pin.
18. The structural member according to any one of claims 13 to 17, characterized in that: The electronic component comprises a connector, and the hydrophobic coating is present on the surface of the connector.
19. The structural member according to any one of claims 13 to 17, characterized in that: A plurality of the electronic components are arranged on the substrate, and the hydrophobic coating is continuously distributed between at least two adjacent electronic components and covers the at least two adjacent electronic components.
20. A terminal product, characterized in that: A structural member comprising any one of claims 13 to 19.
Citation Information
Patent Citations
Low dielectric constant silicon coating, method for the preparation and application thereof to integrated circuits
CN101283066A
Multilayered wiring board and method for manufacturing multilayered wiring board
CN102474993A
Cosmetic compositions comprising organopolysilicones
CN105451708A
Circuit carrier having a silicone polymer coating
CN106232747A
Super-hydrophobic coating, super-hydrophobic coating layer, and preparation method thereof
CN106366907A
Cited By
Film-forming composition and use thereof
WO2025213883A1
Method for applying a protective coating, and protective coating system
WO2026125224A1