Production method for improving flaw detection qualification rate of ocean platform steel

By using a converter-LF furnace-RH furnace-slab casting machine process, combined with KR desulfurization, BOF smelting, LF refining and RH vacuum refining, the problem of low flaw detection pass rate of marine platform steel was solved, and high-performance DH36 marine platform steel was produced.

CN118895403APending Publication Date: 2024-11-05WUHAN IRON & STEEL GRP ECHENG IRON & STEEL CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411179432.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing marine platform steel has defects such as inclusions, cracks and segregation in ultrasonic testing, resulting in a low pass rate.

Method used

By employing a converter-LF furnace-RH furnace-slab casting machine process, combined with KR desulfurization, BOF smelting, LF refining, RH vacuum refining and slab continuous casting, the total amount of inclusions and harmful gas elements are controlled to produce fine-grained, ultra-clean DH36 marine platform steel.

Benefits of technology

It improved the flaw detection pass rate of marine platform steel to 99.85%, and has high tensile strength, impact toughness and good comprehensive performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to a production method for improving the flaw detection qualification rate of ocean platform steel. The production method comprises the steps of KR desulfurization, BOF smelting, LF refining, RH vacuum refining, slab continuous casting, casting blank heating, controlled rolling, controlled cooling, finishing and normalizing heat treatment. According to the steel plate, the total amount of inclusions is reduced through the LF refining function, the form of the inclusions is effectively controlled, then the content of harmful gas elements of H and N in molten steel is effectively reduced through RH vacuum circulation degassing, and the thickness of the produced finished steel plate for the DH36 ocean platform is 16-60 mm through reasonable technological parameter setting of slab continuous casting, casting blank heating, rolling and cooling subsequently; the yield strength is 355-375 MPa, the tensile strength is 490-620 MPa, the ductility A is 21-25%, the impact energy KV2 at the temperature of-40 DEG C is larger than or equal to 200 J, and the steel plate has the good comprehensive characteristics of fine grains, ultra-cleanliness and the like, the ultrasonic flaw detection qualification rate reaches 99.85% or above, A-type inclusions are 0.5-1.5 levels, and the inclusion macroscopic rating is as follows: center segregation is 0.5-1.0 level, center porosity is 0.5-1.0 level, middle cracks are 0 level, corner cracks are 0 level and pinholes are 0 level.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel materials, in particular to a production method for improving the flaw detection pass rate of offshore platform steel. Background Art

[0002] With the shortage of oil resources and the continuous rise in oil prices, the development of marine resources has become increasingly important, and the demand and performance requirements for offshore platform steel have become increasingly higher. Therefore, at present, offshore platform steel generally needs to pass ultrasonic testing before delivery.

[0003] Ultrasonic flaw detection is a non-destructive testing method that uses the acoustic impedance of ultrasound in different media and the differences in transmittance and reflectivity after passing through the steel plate to judge the internal quality of the steel plate through the waveform reflected on the flaw detector. Ultrasonic flaw detection can reflect the purity, density and uniformity of molten steel at a microscopic level. From the analysis of steel plates that failed the flaw detection, the main defects of such steel plates are as follows: (1) From the perspective of the plate surface, the defects on the plate surface are relatively serious and spread throughout the entire steel plate. (2) From the perspective of the plate thickness, the defects are mainly concentrated at the position of 1 / 2 of the thickness. Sampling and analysis of slabs that failed flaw detection on offshore platforms showed that the slabs generally had central segregation and looseness. The matrix structure of the steel plate was F+P, and the segregation band structure in the center was M+B mixed structure. The cracks in the segregation band were caused by the abnormal martensite and bainite structures in the center of the plate thickness. Scanning electron microscope observation and energy spectrum reanalysis of the cracked samples showed that there were more S, Nb, and Ti inclusions at the cracks. The analysis may be related to the slag roll and nitride precipitation during the molten steel pouring process. In summary, the failure of flaw detection in actual production manifests itself as casting quality defects such as inclusions, cracks, and segregation. The causes of these quality defects need to be analyzed from multiple aspects such as molten steel cleanliness, endogenous inclusions, foreign inclusions, and liquid level fluctuations during the pouring process.

[0004] Therefore, developing a new production method for offshore platform steel is of great significance to improving the flaw detection pass rate of offshore platform steel. Summary of the invention

[0005] The purpose of the present invention is to provide a production method for improving the flaw detection pass rate of offshore platform steel. The steel plate of the present invention is produced by a converter-LF furnace-RH furnace-slab caster process, and the LF refining function is used to reduce the total amount of inclusions and effectively control the morphology of inclusions, and then the RH vacuum cycle degassing is used to effectively reduce the harmful gas element content of H and N in molten steel. The DH36 offshore platform steel prepared by the present invention has good comprehensive characteristics such as fine grains and ultra-cleanliness, and has high tensile strength and impact toughness, and the ultrasonic flaw detection pass rate is ≥99.85%.

[0006] The present invention provides a production method for improving the qualified rate of flaw detection of offshore platform steel, comprising: KR desulfurization → BOF smelting → LF refining → RH vacuum refining → slab continuous casting → billet heating → controlled rolling → controlled cooling → finishing → normalizing heat treatment, wherein: (1) KR desulfurization: The incoming molten iron contains the following chemical components by mass percentage: C: 4.0-4.5%, Si: 0.30-0.85%, Mn≤0.40%, P≤0.150%, S≤0.050%, As≤0.010%, Cu≤0.03%, the remainder is Fe and unavoidable impurities, the slag layer thickness is ≤50mm, and the molten iron temperature is ≥1300℃; the molten iron deep desulfurization process is carried out, and the S content in the molten iron is controlled to be ≤0.002%, the molten iron temperature is ≥1220℃, and the exposed surface of the molten iron is required to be more than 3 / 4 after slagging; (2) BOF smelting: S in scrap steel is required to be ≤0.030%; composite blowing, nitrogen-argon switching, smelting end point C: 0.04-0.06%, P≤0.010%, S≤0.015%, slag basicity R: 3.5-4.0, oxygen lance blowing times ≤2 times; slag blocking method, slide plate blocking slag; steel tapping time ≤4 minutes; (3) LF refining: 3.5-4.0m / t steel of aluminum wire is fed into the station. After 5 minutes of power supply, 10-12kg / t steel of lime, 1.0-2.0kg / t steel of calcium carbide, 1.0-1.5kg / t steel of fluorite powder, and 0.5-1.2kg / t steel of aluminum particles are added. After the white slag is formed, slag samples are taken for testing. The basicity of the white slag is required to be 3-4, and the white slag retention time is ≥10min. The Als content out of the station is 0.030-0.045%. The total refining time is 40-44min. Soft argon blowing is required for more than 8 minutes before the LF bag is hung. (4) RH vacuum refining: RH ultimate vacuum holding time ≥18min; air sampling and testing, add alloy according to the composition of molten steel, and the circulation time of molten steel after addition is ≥5min; after the RH treatment, temperature measurement, sampling, oxygen and nitrogen determination are required, and [O]≤5PPm, [N]≤30PPm, and the RH outgoing composition is controlled according to the target value. The Ti content is 0.25-0.35%. After the RH treatment, calcium treatment must be carried out, and calcium iron wire is fed at 3.5-4.0m / t; after the calcium treatment, soft argon blowing must be carried out, and the soft blowing time for the open casting furnace is ≥10min, and the continuous casting furnace is ≥8min, and the argon blowing intensity is 30-80Nm 3 / min, requiring the slag surface to have obvious fluctuations but no exposed steel liquid surface; (5) Slab continuous casting: The tundish pouring can only be carried out when the weight of the molten steel in the tundish is controlled to be ≥25 tons. During the pouring process, the weight of the molten steel in the tundish shall not be less than 25 tons. The tundish overheating degree is 12-30℃. The tundish covering agent is 50-70kg / furnace of wollastonite and 30-50kg / furnace of vermiculite added at one time. After the tundish pouring is started, 0.3-0.4kg / t of mold protection slag is added to the molten steel in the crystallizer to protect the casting. The cooling water of the crystallizer is adjusted from 4400L / min to 4200L / min, the taper is adjusted from 1.1% to 1.15%, and the straightening temperature is increased to 915℃. Adjustment of the speed of the turret of the casting machine: adjust the turret speed from 76 seconds to 60 seconds. (6) Billet heating: the temperature on the surface of the first heating element is 600-1100℃, the heating time is 54-61min, the temperature on the surface of the second heating element is 1235±50℃, the heating time is 54-61min, the temperature on the surface of the third heating element is 1220±20℃, the heating time is 54-61min, the soaking section is 1220±20℃, the heating time is 38-42min, and the furnace temperature is 1170±20℃; the total heating time is 200-225min; (7) Rolling: The starting temperature of rough rolling is 1100-1120℃, the starting temperature of finishing rolling is 900-940℃, and the final rolling temperature is 780-860℃. The steel plate must be straightened after rolling. If the steel plate is not straightened once, multiple straightening processes are required. (8) Cooling: After rolling, water the machine in ACC for cooling, and the return temperature should be controlled at 650±50℃.

[0007] The offshore platform steel is DH36 offshore platform steel, which contains the following chemical components in percentage by mass: C: 0.12-0.15%, Si: 0.25-0.35%, Mn: 1.42-1.55%, P≤0.018%, S≤0.005%, Nb: 0.030-0.045%, V: 0.045-0.055%, Ti: 0.007-0.015%, Als: 0.020-0.040%, and the balance is Fe and other inevitable impurities.

[0008] The finished steel plate prepared by the method of the present invention has a thickness of 16-60 mm, a yield strength of 355-375 MPa, a tensile strength of 490-620 MPa, an elongation A of 21-25%, and an impact energy KV2 of ≥200 J at -40°C.

[0009] The qualified rate of flaw detection results of the finished steel plate obtained by the method of the present invention is ≥99.85%, w (TO) 10 -6 : 15-23ppm,w(S) 10 -6: 40-60ppm, Class A inclusions: 0.5-1.5 level, no dendritic MnS was found through metallographic structure observation; low-power inclusion rating: center segregation 0.5-1.0 level, center looseness 0.5-1.0 level, middle crack 0 level, corner crack 0 level, pinhole 0 level.

[0010] The crystallizer protection slag in the present invention contains the following components in percentage by mass: SiO2: 25-33%, CaO: 35-43%, MgO: 1-3%, Fe2O3: 0.5-2.0%, Al2O3: 2.5-4.5%, NaO: 3-6%, F: 7-11%, C: 6-10%, and the rest are impurities; melting point 1100-1150°C, melting speed: 21-25S, viscosity 0.27-0.34Pa.s.

[0011] The main process parameters of the steel of the present invention are set for the following reasons: (1) Composition design principles: adopt the chemical composition design concept of "low carbon, high manganese, micro-alloying", control requirements for the five elements (C and Mn are appropriate, Si is controlled below 0.35%, S and P are reduced to the maximum extent), control of harmful elements N, O, and H (remove N in the early stage of smelting, remove O from aluminum and perform RH vacuum degassing, O ≤ 5ppm); Alloy element control (finally determined that Nb is added to DH36 grade ship plate to achieve grain refinement, and Ti is added to improve its stability, corrosion resistance, high temperature oxidation resistance, and improve steel plate performance); Ca treatment (control w(Ca) / w(Al)>0.1 in molten steel to improve anisotropy.

[0012] Due to the above-mentioned composition design adjustment, the smelting process of the steel of the present invention adopts the low P smelting and low N smelting ideas, which are as follows: Low-P smelting: The converter adopts the double-link method to ensure good slag formation with appropriate oxygen supply intensity and gun position, inhibit carbon oxidation and control the molten pool heating rate. The low-temperature P removal efficiency is ≥85%, and the slag is quickly heated after the P removal is completed. The end point P can be controlled within 0.012%; Low-N smelting: Use low-N scrap steel and alloy, limit the tapping temperature to ≤1630℃, avoid terminal overoxidation and post-blowing, and the terminal N content can be controlled at ≤30ppm to achieve the control target of low-N smelting.

[0013] (2) The principles for adjusting the casting, rolling and cooling process parameters of the steel of the present invention are as follows: Continuous casting process: Reasonable distribution of primary cooling water, weak cooling of the corners of the slab before straightening, and adjustment of the taper of the crystallizer can reduce the occurrence of corner cracks in the slab. During the steel pouring process, the slow effect of the change in secondary cooling water distribution can lead to strong cooling of the slab when the casting speed is reduced, and the probability of corner cracks in the slab increases; the speed adjustment of the casting machine turntable can reduce the risk of slag rolling caused by the lowering of the liquid level in the tundish.

[0014] Controlled rolling and controlled cooling: Rough rolling adopts high temperature and large reduction rolling, the slab is rolled to 2.5-4 times the thickness of the final product, the start rolling temperature is controlled at 1100-1120℃, and the cumulative reduction rate is about 60%. The start rolling temperature of finishing rolling is ≤940℃, the cumulative reduction rate is about 40%, and the final cooling temperature is controlled at 780-860℃. After controlled cooling, a uniform fine grain structure can be obtained to ensure excellent mechanical properties.

[0015] The beneficial effects of the present invention are as follows: The finished steel plate prepared by the method of the present invention has a thickness of 16-60 mm, a yield strength of 355-375 MPa, a tensile strength of 490-620 MPa, an elongation A of 21-25%, an impact energy KV2 of ≥200 J at -40°C, a qualified rate of flaw detection results of ≥99.85%, and a w(TO) of 10 -6 : 15-23ppm,w(S) 10 -6 : 40-60ppm, Class A inclusions: 0.5-1.5 level, no dendritic MnS was found through metallographic structure observation; inclusion low-power rating: center segregation 0.5-1.0 level, center looseness 0.5-1.0 level, middle crack 0 level, corner crack 0 level, pinhole 0 level. The marine platform steel produced by the present invention can be used in the fields of marine platform steel that have high requirements for steel plate toughness, fatigue resistance, and seawater corrosion resistance. The present invention improves the flaw detection pass rate of marine platform steel by deeply exploring the main defect factors of existing marine platform steel and formulating targeted improvement processes. The present invention has the advantages of simple manufacturing process and can be implemented in various metallurgical enterprises. DETAILED DESCRIPTION

[0016] In order to better explain the technical solution of the present invention, the technical solution of the present invention is further described below in conjunction with specific embodiments. The following embodiments are merely exemplary of the technical solution of the present invention and do not limit the present invention in any form. The serial numbers of the following embodiments are only for description and do not represent the advantages and disadvantages of the embodiments.

[0017] Table 1 below is a list of chemical composition values ​​(wt, %) of steel grades in various embodiments of the present invention; Table 2 below is a list of the main process parameter values ​​of the steel grades of various embodiments of the present invention; Table 3 below is a list of composition values ​​(wt, %) of the mold powder of each embodiment of the present invention; Table 4 below is a list of mechanical property test results of steel grades in various embodiments of the present invention; Table 5 below is a list of flaw detection and low-magnification rating conditions of various embodiments of the present invention.

[0018] A production method for improving the flaw detection pass rate of offshore platform steel according to each embodiment of the present invention comprises: KR desulfurization → BOF smelting → LF refining → RH vacuum refining → slab continuous casting → ingot heating → controlled rolling → controlled cooling → finishing → normalizing heat treatment, wherein: (1) KR desulfurization: The incoming molten iron contains the following chemical components by mass percentage: C: 4.0-4.5%, Si: 0.30-0.85%, Mn≤0.40%, P≤0.150%, S≤0.050%, As≤0.010%, Cu≤0.03%, the remainder is Fe and unavoidable impurities, the slag layer thickness is ≤50mm, and the molten iron temperature is ≥1300℃; the molten iron deep desulfurization process is carried out, and the S content in the molten iron is controlled to be ≤0.002%, the molten iron temperature is ≥1220℃, and the exposed surface of the molten iron is required to be more than 3 / 4 after slagging; (2) BOF smelting: S in scrap steel is required to be ≤0.030%; composite blowing, nitrogen-argon switching, smelting end point C: 0.04-0.06%, P≤0.010%, S≤0.015%, slag basicity R: 3.5-4.0, oxygen lance blowing times ≤2 times; slag blocking method, slide plate blocking slag; steel tapping time ≤4 minutes; (3) LF refining: 3.5-4.0m / t steel of aluminum wire is fed into the station. After 5 minutes of power supply, 10-12kg / t steel of lime, 1.0-2.0kg / t steel of calcium carbide, 1.0-1.5kg / t steel of fluorite powder, and 0.5-1.2kg / t steel of aluminum particles are added. After the white slag is formed, slag samples are taken for testing. The basicity of the white slag is required to be 3-4, and the white slag retention time is ≥10min. The Als content out of the station is 0.030-0.045%. The total refining time is 40-44min. Soft argon blowing is required for more than 8 minutes before the LF bag is hung. (4) RH vacuum refining: RH ultimate vacuum holding time ≥18min; air sampling and testing, add alloy according to the composition of molten steel, and the circulation time of molten steel after addition is ≥5min; after the RH treatment, temperature measurement, sampling, oxygen and nitrogen determination are required, and [O]≤5PPm, [N]≤30PPm, and the RH outgoing composition is controlled according to the target value. The Ti content is 0.25-0.35%. After the RH treatment, calcium treatment must be carried out, and calcium iron wire is fed at 3.5-4.0m / t; after the calcium treatment, soft argon blowing must be carried out, and the soft blowing time for the open casting furnace is ≥10min, and the continuous casting furnace is ≥8min, and the argon blowing intensity is 30-80Nm 3 / min, requiring the slag surface to have obvious fluctuations but no exposed steel liquid surface; (5) Slab continuous casting: The tundish pouring can only be carried out when the weight of the molten steel in the tundish is controlled to be ≥25 tons. During the pouring process, the weight of the molten steel in the tundish shall not be less than 25 tons. The tundish overheating degree is 12-30℃. The tundish covering agent is 50-70kg / furnace of wollastonite and 30-50kg / furnace of vermiculite added at one time. After the tundish pouring is started, 0.3-0.4kg / t of mold protection slag is added to the molten steel in the crystallizer to protect the casting. The cooling water of the crystallizer is adjusted from 4400L / min to 4200L / min, the taper is adjusted from 1.1% to 1.15%, and the straightening temperature is increased to 915℃. Adjustment of the speed of the turret of the casting machine: adjust the turret speed from 76 seconds to 60 seconds. (6) Billet heating: the temperature on the surface of the first heating element is 600-1100℃, the heating time is 54-61min, the temperature on the surface of the second heating element is 1235±50℃, the heating time is 54-61min, the temperature on the surface of the third heating element is 1220±20℃, the heating time is 54-61min, the soaking section is 1220±20℃, the heating time is 38-42min, and the furnace temperature is 1170±20℃; the total heating time is 200-225min; (7) Rolling: The starting temperature of rough rolling is 1100-1120℃, the starting temperature of finishing rolling is 900-940℃, and the final rolling temperature is 780-860℃. The steel plate must be straightened after rolling. If the steel plate is not straightened once, multiple straightening processes are required. (8) Cooling: After rolling, water the machine in ACC for cooling, and the return temperature should be controlled at 650±50℃.

[0019] Table 1 List of chemical composition values ​​of steels in various embodiments of the present invention Table 2 List of main process parameter values ​​of steel in various embodiments of the present invention

[0020] Table 3 List of composition values ​​of mold protection slag in various embodiments of the present invention

[0021] Note: The melting point of the mold protection slag is 1100-1150℃, the melting speed is 21-25S, and the viscosity is 0.27-0.34Pa.s.

[0022] Table 4 List of mechanical properties test results of steel grades in various embodiments of the present invention

[0023] Table 5 List of flaw detection and low magnification rating of various embodiments of the present invention

[0024] As shown in Tables 4 and 5 above, the thickness of the finished steel plate obtained by the method of the present invention is 16-60 mm, the yield strength is 355-375 MPa, the tensile strength is 490-620 MPa, the elongation A is 21-25%, the impact energy KV2 at -40°C is ≥200 J; the flaw detection pass rate is ≥99.85%, w (TO) 10 -6 : 15-23ppm,w(S) 10 -6 : 40-60ppm, Class A inclusions: 0.5-1.5 level, no dendritic MnS was found through metallographic structure observation; inclusion low-power rating: center segregation 0.5-1.0 level, center looseness 0.5-1.0 level, middle crack 0 level, corner crack 0 level, pinhole 0 level. The marine platform steel produced by the present invention can be used in the fields of marine platform steel that have high requirements for steel plate toughness, fatigue resistance, and seawater corrosion resistance. The present invention improves the flaw detection pass rate of marine platform steel by deeply exploring the main defect factors of existing marine platform steel and formulating targeted improvement processes. The present invention has the advantages of simple manufacturing process and can be implemented in various metallurgical enterprises. .

[0025] The above embodiments are only specific examples for explaining the present invention and do not limit the present invention in any form. Any non-substantial changes made by anyone based on the above contents and forms without departing from the protection scope of the claims of the present invention shall be deemed to fall within the protection scope of the claims of the present invention. The present invention is not limited to the above specific implementation examples.

Claims

1. A production method for improving the qualified rate of flaw detection of offshore platform steel, include: KR desulfurization → BOF smelting → LF refining → RH vacuum refining → slab continuous casting → billet heating → controlled rolling → controlled cooling → finishing → normalizing heat treatment, characterized by: (1) KR desulfurization: The incoming molten iron contains the following chemical components by mass percentage: C: 4.0-4.5%, Si: 0.30-0.85%, Mn≤0.40%, P≤0.150%, S≤0.050%, As≤0.010%, Cu≤0.03%, the remainder is Fe and unavoidable impurities, the slag layer thickness is ≤50mm, and the molten iron temperature is ≥1300℃; the molten iron deep desulfurization process is carried out, and the S content in the molten iron is controlled to be ≤0.002%, the molten iron temperature is ≥1220℃, and the exposed surface of the molten iron is required to be more than 3 / 4 after slagging; (2) BOF smelting: S in scrap steel is required to be ≤0.030%; composite blowing, nitrogen-argon switching, smelting end point C: 0.04-0.06%, P≤0.010%, S≤0.015%, slag basicity R: 3.5-4.0, oxygen lance blowing times ≤2 times; slag blocking method, slide plate blocking slag; steel tapping time ≤4 minutes; (3) LF refining: 3.5-4.0m / t steel of aluminum wire is fed into the station. After 5 minutes of power supply, 10-12kg / t steel of lime, 1.0-2.0kg / t steel of calcium carbide, 1.0-1.5kg / t steel of fluorite powder, and 0.5-1.2kg / t steel of aluminum particles are added. After the white slag is formed, slag samples are taken for testing. The basicity of the white slag is required to be 3-4, and the white slag retention time is ≥10min. The Als content out of the station is 0.030-0.045%. The total refining time is 40-44min. Soft argon blowing is required for more than 8 minutes before the LF bag is hung. (4) RH vacuum refining: RH ultimate vacuum holding time ≥18min; air sampling and testing, add alloy according to the composition of molten steel, and the circulation time of molten steel after addition is ≥5min; after the RH treatment, temperature measurement, sampling, oxygen and nitrogen determination are required, and [O]≤5PPm, [N]≤30PPm, and the RH outgoing composition is controlled according to the target value. The Ti content is 0.25-0.35%. After the RH treatment, calcium treatment must be carried out, and calcium iron wire is fed at 3.5-4.0m / t; after the calcium treatment, soft argon blowing must be carried out, and the soft blowing time for the open casting furnace is ≥10min, and the continuous casting furnace is ≥8min, and the argon blowing intensity is 30-80Nm 3 / min, requiring the slag surface to have obvious fluctuations but no exposed steel liquid surface; (5) Slab continuous casting: The tundish pouring can only be carried out when the weight of the molten steel in the tundish is controlled to be ≥25 tons. During the pouring process, the weight of the molten steel in the tundish shall not be less than 25 tons. The tundish overheating degree is 12-30℃. The tundish covering agent is 50-70kg / furnace of wollastonite and 30-50kg / furnace of vermiculite added at one time. After the tundish pouring is started, 0.3-0.4kg / t of mold protection slag is added to the molten steel in the crystallizer to protect the casting. The cooling water of the crystallizer is adjusted from 4400L / min to 4200L / min, the taper is adjusted from 1.1% to 1.15%, and the straightening temperature is increased to 915℃. Adjustment of the speed of the turret of the casting machine: adjust the turret speed from 76 seconds to 60 seconds. (6) Billet heating: the temperature on the surface of the first heating element is 600-1100℃, the heating time is 54-61min, the temperature on the surface of the second heating element is 1235±50℃, the heating time is 54-61min, the temperature on the surface of the third heating element is 1220±20℃, the heating time is 54-61min, the soaking section is 1220±20℃, the heating time is 38-42min, and the furnace temperature is 1170±20℃; the total heating time is 200-225min; (7) Rolling: The starting temperature of rough rolling is 1100-1120℃, the starting temperature of finishing rolling is 900-940℃, and the final rolling temperature is 780-860℃. The steel plate must be straightened after rolling. If the steel plate is not straightened once, multiple straightening processes are required. (8) Cooling: After rolling, water the steel plate in ACC for cooling, and the return temperature should be controlled at 650±50℃.

2. A production method for improving the qualified rate of flaw detection of offshore platform steel according to claim 1, Features: The offshore platform steel is DH36 offshore platform steel, which contains the following chemical components in percentage by mass: C: 0.12-0.15%, Si: 0.25-0.35%, Mn: 1.42-1.55%, P≤0.018%, S≤0.005%, Nb: 0.030-0.045%, V: 0.045-0.055%, Ti: 0.007-0.015%, Als: 0.020-0.040%, and the balance is Fe and other inevitable impurities.

3. A production method for improving the qualified rate of flaw detection of offshore platform steel according to claim 1 or 2, Features: The finished steel plate has a thickness of 16-60mm, a yield strength of 355-375MPa, a tensile strength of 490-620MPa, an elongation A of 21-25%, and an impact energy KV at -40℃. 2 ≥200J.

4. A production method for improving the qualified rate of flaw detection of offshore platform steel according to claim 1 or 2, Features: The qualified rate of flaw detection results of the finished steel plate is ≥99.85%, w (TO) 10 -6 : 15-23ppm,w(S) 10 -6 : 40-60ppm, type A inclusions: 0.5-1.5 level, no dendritic MnS was found through metallographic structure observation; low-power inclusion rating: central segregation 0.5-1.0 level, central porosity 0.5-1.0 level, middle crack 0 level, corner crack 0 level, pinhole 0 level.

5. A production method for improving the qualified rate of flaw detection of offshore platform steel according to claim 1, Features: The mold protection slag contains the following components by mass percentage: SiO 2 :25-33%, CaO: 35-43%, MgO: 1-3%, Fe 2 O 3 :0.5-2.0%,Al 2 O 3 : 2.5-4.5%, NaO: 3-6%, F: 7-11%, C: 6-10%, the rest are impurities; melting point 1100-1150℃, melting speed: 21-25S, viscosity 0.27-0.34Pa.s.

Citation Information

Cited By

  • Multi-stage controlled rolling and controlled cooling process for improving impact toughness of DH36 steel thick plate

    CN120249617A