40kg-grade high-strength toughness corrosion-resistant ship plate steel and production method thereof
By optimizing processes such as molten iron pretreatment and converter smelting, controlling chemical composition and process parameters, the existing 40kg class shipboard steel production process is solved, and 40kg with low cost, high strength and good corrosion resistance is achieved. Grade high-strength toughness steel for ship construction and high-strength structural parts.
Patent Information
- Application Number
- CN202411179485.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-05
AI Technical Summary
The existing 40kg-class shipboard steel has complex production processes and high costs, making it difficult to meet the needs of low-cost and simple processes.
Using processes such as water-molten iron pretreatment, converter smelting, argon blowing, LF furnace refining, RH furnace vacuum treatment, slab casting, slow cooling and cleaning of casting, heating of casting, controlled rolling, straightening and slow cooling, etc., to control chemistry Components and process parameters, including carbon, silicon, manganese, phosphorus, sulfur, vanadium, chromium, copper and nitrogen content, ensure high strength and toughness of the steel plate under light pressure and optimization of electromagnetic stirring, heating time and rolling temperature. Corrosion resistance.
Achieve low-cost, high-strength, good corrosion resistance and simple process of 40kg grade high-strength toughness ship plate steel, with yield strength of 390MPa, tensile strength ≥520MPa, elongation ≥20%, impact work ≥190J in -40℃, performance Stable, suitable for ship construction and high-strength structural parts.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel materials, in particular to a 40kg-grade high-strength and toughness corrosion-resistant ship plate steel and a production method thereof. Background Art
[0002] In recent years, due to the rapid development of the shipping industry and the emphasis on transportation safety, the scrapping speed of old ship types has accelerated, and the demand for new ships has increased. The high demand in the ship market has provided a good opportunity for the development of ship steel, and the large-scale and specialized ships have greatly increased the demand for low-alloy high-strength ship plates in the industry. Because ordinary shipbuilding steel has low strength, it is necessary to increase the thickness of the ship plate when building large ships. This not only increases the difficulty and cost of processing and welding during the manufacturing process, but also increases the deadweight of the hull and reduces the load capacity. Nowadays, 32-36kg grade high-strength ship plates are widely used. The development of higher-strength 40kg grade high-strength corrosion-resistant ship plates to replace ship plates with strength levels of 36kg and below is more conducive to improving ship safety, reducing deadweight, and increasing load capacity.
[0003] After searching: Chinese patent CN103205640A discloses an E40 high-strength ship plate and its preparation method. Its chemical composition by mass percentage is: C: 0.13-0.16%, Si: 0.2-0.4%, Mn: 1.5-1.6%, P≤0.03%, S≤0.005%, Ni: 0.3-0.35%, V: 0.055-0.065%, Nb: 0.035-0.045%, Ti: 0.010-0.020%, Als: 0.015-0.035%, and the balance is Fe. Its preparation method includes hot metal pretreatment process, converter smelting process, argon blowing process, LF refining process, VD refining process, continuous casting process, heating process, controlled rolling and controlled cooling, pile cooling process, and heat treatment process. The developed high-strength E40 steel has a yield strength of 430-450MPa, a tensile strength of 550-580MPa, an elongation of 22%-24%, and an impact energy of 210-280J at -40℃. The advantage is that the steel plate has good strength and toughness, which fully meets the standards and customer requirements. The disadvantage is that the production process is long, more alloys are added, and the production cost is high.
[0004] Chinese patent CN107287508A discloses a method for producing a 40kg-class ship plate for high-energy-input welding. Chemical composition: C: 0.07-0.11%, Si: 0.15-0.35%, Mn: 1.45-1.60%, Nb: 0.015-0.035%, Ti: 0.012-0.018%, Ni: 0.15-0.30%, Cu: 0.20-0.35%, Als: 0.015-0.04%, P≤0.020%, S≤0.005%, Ceq: 0.36-0.40%. The production method is as follows: steel is tapped from the converter with slag blocking, and the thickness of the slag layer is less than 100mm; vacuum treatment pressure holding or RH molten steel circulation time is ≥10min; the target superheat of the tundish is less than 25℃; the continuous casting billet is stacked and slowly cooled for 45 to 48h; the billet heating temperature is 1180 to 1220℃, and the time is 9 to 10min / cm; the second stage rolling temperature is 760 to 800℃, the total reduction in the second stage is greater than 60%, and the final rolling temperature is 740 to 780℃; the ACC water entry temperature is 710 to 750℃, the cooling rate is 4 to 8℃ / s, and the red return temperature is 550 to 620℃; the stacking slow cooling temperature is 250 to 350℃, and the time is ≥24 hours. The advantages are that the yield strength of the ship plate reaches 445MPa, the tensile strength is 577MPa, the elongation is 25.1%, and the -40℃ impact average is 159J, which meets the standard requirements. The disadvantage is that more strengthening elements need to be added when the carbon content is low, and the cost is relatively high.
[0005] Therefore, it is very necessary to develop a new high-strength and toughness corrosion-resistant ship plate steel with low cost and simple production process to solve the above problems. Summary of the invention
[0006] The purpose of the present invention is to provide a 40kg-grade high-strength, toughness and corrosion-resistant ship plate steel and a production method thereof in view of the problems that the current 40kg-grade ship plate steel has high cost and complicated production process. The ship plate steel provided by the present invention has almost no high-cost alloy components, and the production process is simple and the overall cost is low. The product has good strength, toughness and corrosion resistance and has strong market competitiveness.
[0007] The invention discloses a 40kg-grade high-strength and toughness corrosion-resistant ship plate steel, which comprises the following chemical components in percentage by mass: C: 0.13-0.15%, Si: 0.20-0.30%, Mn: 1.25-1.35%, P≤0.020%, S≤0.005%, Alt: 0.030-0.040%, V: 0.050-0.060%, Cr: 0.45-0.55%, Cu: 0.25-0.30%, N≤0.0050%, and the rest are Fe and unavoidable impurities.
[0008] The ship plate steel of the present invention has a maximum thickness of 40 mm, a yield strength ReH≥390 MPa, a tensile strength Rm≥520 MPa, an elongation A≥20%, and an impact energy KV2≥190 J at -40°C.
[0009] The present invention provides a production method of 40kg-grade high-strength and toughness corrosion-resistant ship plate steel, comprising: molten iron pretreatment → converter smelting → argon blowing in an argon station → LF furnace refining → RH furnace vacuum treatment → slab casting → slow cooling and cleaning of the ingot → heating of the ingot → controlled rolling → straightening → slow cooling → finishing; wherein: (1) According to the chemical composition requirements of ship plate steel, qualified molten steel is smelted, and slabs with a thickness of 200 mm are cast. During the casting process, the pulling speed is controlled to stabilize the casting, the superheat is controlled at 15-30°C, the pulling speed is 1.2-1.25 m / min, and light pressure reduction and electromagnetic stirring are used during the casting process. The light pressure reduction is 6 mm, the electromagnetic stirring frequency and current are 6 Hz and 430-450 A respectively, and the immersion nozzle insertion depth is 120-150 mm; after the slab is off the line, it is stacked and slowly cooled for ≥36 hours, and the surface defects of the slab are inspected and cleaned after slow cooling; (2) Billet heating process: furnace time 4-5 hours, furnace temperature 1100-1150°C, soaking time 40-50 minutes; (3) Controlled rolling process: After the slab is taken out of the furnace, it is descaled by high-pressure water to remove the iron oxide scale, and then enters the rough rolling mill for rolling. The starting temperature of the rough rolling is 1050-1080°C, and high-temperature and large-volume rolling is adopted. The intermediate waiting thickness is H+ (30-40) mm, where H is the thickness of the finished steel plate in mm; the starting temperature of the finishing rolling is ≤980°C, and the final rolling temperature is 810-870°C; (4) Cooling: After rolling, the steel plate shall not be cooled by water. After being leveled by the straightening machine, the steel plate ≤20mm shall be air-cooled to room temperature. The steel plate 20-40mm shall be stacked and slowly cooled for 48 hours off the production line.
[0010] The reasons for limiting the amounts of the main chemical components of the steel of the present invention are as follows: C: Carbon is one of the main elements that affect the strength of steel plates. It can significantly improve the strength of steel through interstitial solid solution strengthening. When the carbon content is low, it will seriously affect the strength of the controlled rolled steel plate. When the carbon content is too high, the toughness and weldability of the steel plate will deteriorate. Therefore, the carbon content of the steel of the present invention is controlled to 0.13-0.15%.
[0011] Si: Silicon is a necessary deoxidizing element for steelmaking and has a certain solid solution strengthening effect on steel plates. However, if the Si content is too high, it will make it difficult to remove the iron oxide scale on the surface of the steel billet, affecting the surface quality of the steel plate and reducing the low temperature toughness of the steel. Therefore, the Si content of the steel of the present invention is controlled to be 0.20-0.30%.
[0012] Mn: Manganese has the function of refining grains and improving the strength of steel plates. It is one of the main elements that affect the strength of steel plates and can also improve the low-temperature toughness of steel plates. However, if the content is too high, it will increase the segregation of the ingot and cause the grains of the steel to coarsen at high temperatures. Therefore, the Mn content of the steel of the present invention is controlled to be 1.25-1.35%.
[0013] P and S are unavoidable harmful impurity elements in steel. Phosphorus is prone to serious segregation in parts of steel, reducing the plasticity and toughness of steel, and is extremely harmful to low-temperature toughness. Sulfur is easy to segregate and enrich in steel, and sulfide inclusions in steel will significantly reduce the elongation and toughness of steel. Therefore, the steel of the present invention strictly controls P≤0.020% and S≤0.005%.
[0014] Al: Aluminum is an important deoxidizing element. Adding a small amount of aluminum to steel can effectively reduce the inclusion content. Al in steel can form AlN with N, which can hinder the growth of high-temperature austenite and play a role in refining grains. However, too high Al content can easily lead to surface cracks in the casting. Therefore, the Alt content of the steel of the present invention is controlled to 0.030-0.040%.
[0015] V: Vanadium can refine the grain structure and improve the strength and toughness of the steel plate. The effect is not obvious when added in small amounts. When the vanadium content exceeds 0.06%, the toughness and weldability of the steel decrease. Therefore, the V content of the present invention is controlled at 0.050-0.060%.
[0016] Cu: can improve the strength of steel through solid solution strengthening. Cu element can improve the corrosion resistance and weldability of steel and improve the low temperature toughness of steel, but it is easy to produce cracks when the Cu content is high. Therefore, the Cu content of the steel of the present invention is designed to be 0.25-0.30%.
[0017] Cr: Chromium and Cu elements can work together to improve the corrosion resistance of steel plates. Cr can reduce the phase transition point of steel, refine the structure, improve the strength of steel, and also improve oxidation resistance and high temperature corrosion resistance. However, if the Cr content is too high, the iron oxide scale on the surface of the ingot is difficult to remove, which affects the surface quality of the steel plate. Therefore, the Cr content of the steel of the present invention is in the range of 0.45-0.55%.
[0018] N: Nitrogen has a solid solution strengthening effect, but it is not significant. Since nitrides precipitate on the grain boundaries, they can increase the high-temperature strength of the grain boundaries and increase the creep strength of the steel. Through infiltration, it can form compounds with Cr and Al elements on the steel surface, increasing the surface strength and corrosion resistance of the steel. However, N also has a disadvantage in steel. It can cause aging and blue brittleness. When the content exceeds a certain limit, it is easy to form bubbles and looseness in the steel, and form angular and brittle inclusion groups with elements such as Ti and Al in the steel. Therefore, the steel of the present invention has N≤0.0050%.
[0019] The reasons for setting the main production process parameters of the steel of the present invention are as follows: Since the steel of the present invention contains more Cu, Cr, V and other alloys, in order to prevent cracks during the casting process, the superheat is controlled at 15-30°C, the pulling speed is controlled at 1.2-1.25m / min, and in order to improve the center segregation and prevent slag rolling, light pressure reduction and electromagnetic stirring are used during the casting process, the light pressure reduction is 6mm, the electromagnetic stirring frequency and current are 6Hz and 430-450A respectively, and the immersion nozzle insertion depth is 120-150mm. In order to avoid cracks in the slab during the cooling process, the slab is stacked and slowly cooled for ≥36 hours after it comes off the line. After slow cooling, the surface defects of the slab are checked and cleaned to prevent defective slabs from being sent down.
[0020] In order to improve the plasticity of steel, reduce deformation resistance, and improve the internal structure and performance of the slab, it is necessary to heat the slab to the temperature range of the austenite single-phase solid solution structure, so that it has enough time to homogenize the structure and dissolve carbides at a higher temperature, including the dissolution of micro-alloy elements. In order to fully dissolve the V micro-alloy element, diffuse the segregation elements, and prevent high temperature from destroying the grain boundary and avoiding the coarsening of the original grains, the heating process of the steel of the present invention is controlled as follows: the furnace time is 4 to 5 hours, the furnace temperature is 1100 to 1150°C, and the soaking time is 40 to 50 minutes.
[0021] The present invention adopts a controlled rolling process, which can give full play to the fine grain strengthening, precipitation strengthening, solid solution strengthening, and phase transformation strengthening effects of V microalloying elements and alloying elements such as Mn, Cu, and Cr during rolling and cooling, and obtain the required structure and steel plate performance. In order to ensure that the rough rolling stage is always in the austenite recrystallization zone and has sufficient deformation, the present invention controls the rough rolling start temperature to 1050-1080°C and adopts high temperature and large reduction rolling. The finishing rolling stage is rolled in the austenite non-recrystallization zone. In order to obtain fine and uniform ferrite grains, the total reduction rate of the non-recrystallization zone needs to be greater than a certain value, generally greater than 45%, so the intermediate waiting temperature thickness is controlled to be H+ (30-40) mm. At the same time, according to the characteristics and composition of the steel containing V microalloying elements of the present invention, the finishing rolling start temperature is ≤980°C, and the final rolling temperature is 810-870°C.
[0022] Since the steel of the present invention contains alloy elements such as Cu and Cr, in order to prevent cracks on the steel plate surface or micro cracks on the grain boundaries, the steel plate of the present invention shall not be cooled by water after rolling. After being leveled by a straightening machine, the steel plate ≤20mm is air-cooled to room temperature, and the steel plate 20-40mm is stacked and slowly cooled for 48 hours off the production line.
[0023] The beneficial effects of the present invention are as follows: The maximum thickness of the steel plate of the present invention is 40mm, the yield strength ReH≥390MPa, the tensile strength Rm≥520MPa, the elongation A≥20%, and the -40℃ impact energy KV2≥190J. The steel plate has stable performance, high strength, good plasticity and impact toughness. Since the ship plate steel of the present invention adds appropriate amounts of Cu and Cr elements, it has been verified in practice that the corrosion resistance and weldability of the steel plate are significantly improved.
[0024] The steel of the invention is a production method of a 40kg-grade high-strength and toughness corrosion-resistant ship plate steel, which can be used for shipbuilding or other structural parts with high strength and toughness requirements.
[0025] The invention has the advantages of simple manufacturing process and the like, and can be implemented in various metallurgical enterprises. DETAILED DESCRIPTION
[0026] In order to better explain the technical solution of the present invention, the technical solution of the present invention is further described below in conjunction with specific embodiments. The following embodiments are merely exemplary of the technical solution of the present invention and do not limit the present invention in any form. The serial numbers of the following embodiments are only for description and do not represent the advantages and disadvantages of the embodiments.
[0027] Table 1 below is a list of chemical composition values (wt, %) of steels of various embodiments of the present invention and comparative examples; Table 2 below is a list of main process parameter values of various example steels and comparative example steels of the present invention; Table 3 below is a list of the main mechanical properties test results of the steels of various embodiments of the present invention and the comparative example steels.
[0028] A production method of a 40kg-grade high-toughness corrosion-resistant ship plate steel according to each embodiment of the present invention comprises: molten iron pretreatment → converter smelting → argon blowing in an argon station → LF furnace refining → RH furnace vacuum treatment → slab casting → slow cooling and cleaning of the ingot → heating of the ingot → controlled rolling → straightening → slow cooling → finishing; wherein: (1) According to the chemical composition requirements of ship plate steel, qualified molten steel is smelted, and slabs with a thickness of 200 mm are cast. During the casting process, the pulling speed is controlled to stabilize the casting, the superheat is controlled at 15-30°C, the pulling speed is 1.2-1.25 m / min, and light pressure reduction and electromagnetic stirring are used during the casting process. The light pressure reduction is 6 mm, the electromagnetic stirring frequency and current are 6 Hz and 430-450 A respectively, and the immersion nozzle insertion depth is 120-150 mm; after the slab is off the line, it is stacked and slowly cooled for ≥36 hours, and the surface defects of the slab are inspected and cleaned after slow cooling; (2) Billet heating process: furnace time 4-5 hours, furnace temperature 1100-1150°C, soaking time 40-50 minutes; (3) Controlled rolling process: After the slab is taken out of the furnace, it is descaled by high-pressure water to remove the iron oxide scale, and then enters the rough rolling mill for rolling. The starting temperature of the rough rolling is 1050-1080°C, and high-temperature and large-volume rolling is adopted. The intermediate waiting thickness is H+ (30-40) mm, where H is the thickness of the finished steel plate in mm; the starting temperature of the finishing rolling is ≤980°C, and the final rolling temperature is 810-870°C; (4) Cooling: After rolling, the steel plate shall not be cooled by water. After being leveled by the straightening machine, the steel plate ≤20mm shall be air-cooled to room temperature. The steel plate 20-40mm shall be stacked and slowly cooled for 48 hours off the production line.
[0029] Table 1 List of chemical composition values of various examples of steel and comparative example steel of the present invention
[0030] Table 2 List of main process parameter values of various example steels and comparative example steels of the present invention
[0031] Table 3 List of test results of main mechanical properties of steels of various embodiments of the present invention and comparative examples
[0032] As shown in Table 3 above, the ship plate steel produced in Examples 1 to 5 of the present invention has a yield strength ReH of more than 397MPa, a tensile strength Rm of more than 538MPa, an elongation A of more than 20.5%, and an impact energy KV2 of more than 191J at -40°C. The steel plate has stable performance, high strength, good plasticity and impact toughness, and can have certain corrosion resistance through elements such as Cu and Cr. On the other hand, the steel plate of Comparative Example 1 has the problems of small yield strength margin, low elongation, and low impact; the steel plate of Comparative Example 2 has the problems of low elongation, large impact fluctuation, and low impact single value; the steel plate of Comparative Example 3 has the problem of low strength.
[0033] The above embodiments are only specific examples for explaining the present invention and do not limit the present invention in any form. Any non-substantial changes made by anyone based on the above contents and forms without departing from the protection scope of the claims of the present invention shall be deemed to fall within the protection scope of the claims of the present invention. The present invention is not limited to the above specific implementation examples.
Claims
1. A 40kg grade high strength and toughness corrosion resistant ship plate steel, characterized in that Contains the following chemical components in mass percentage: C: 0.13-0.15%, Si: 0.20-0.30%, Mn: 1.25-1.35%, P≤0.020%, S≤0.005%, Alt: 0.030-0.040%, V: 0.050-0.060%, Cr: 0.45-0.55%, Cu: 0.25-0.30%, N≤0.0050%, and the rest are Fe and unavoidable impurities.
2. The 40kg-grade high-strength and toughness corrosion-resistant ship plate steel according to claim 1, characterized in that: The ship plate steel has a maximum finished plate thickness of 40 mm, a yield strength ReH ≥ 390 MPa, a tensile strength Rm ≥ 520 MPa, an elongation A ≥ 20%, and an impact energy KV2 ≥ 190 J at -40°C.
3. A method for producing a 40kg-grade high-toughness corrosion-resistant ship plate steel as claimed in claim 1 or 2, comprising: Hot metal pretreatment → converter smelting → argon blowing at argon station → LF furnace refining → RH furnace vacuum treatment → slab pouring → slow cooling and cleaning of ingot → ingot heating → controlled rolling → straightening → slow cooling → finishing; its characteristics are: (1) According to the chemical composition requirements of ship plate steel, qualified molten steel is smelted, and slabs with a thickness of 200 mm are cast. During the casting process, the pulling speed is controlled to stabilize the casting, the superheat is controlled at 15-30°C, the pulling speed is 1.2-1.25 m / min, and light pressure reduction and electromagnetic stirring are used during the casting process. The light pressure reduction is 6 mm, the electromagnetic stirring frequency and current are 6 Hz and 430-450 A respectively, and the immersion nozzle insertion depth is 120-150 mm; after the slab is off the line, it is stacked and slowly cooled for ≥36 hours, and the surface defects of the slab are inspected and cleaned after slow cooling; (2) Billet heating process: furnace time 4-5 hours, furnace temperature 1100-1150°C, soaking time 40-50 minutes; (3) Controlled rolling process: After the slab is taken out of the furnace, it is descaled by high-pressure water to remove the iron oxide scale, and then enters the rough rolling mill for rolling. The starting temperature of the rough rolling is 1050-1080°C, and high-temperature and large-volume rolling is adopted. The intermediate waiting thickness is H+ (30-40) mm, where H is the thickness of the finished steel plate in mm; the starting temperature of the finishing rolling is ≤980°C, and the final rolling temperature is 810-870°C; (4) Cooling: After rolling, the steel plate shall not be cooled by water. After being leveled by the straightening machine, the steel plate ≤20mm shall be air-cooled to room temperature. The steel plate 20-40mm shall be stacked and slowly cooled for 48 hours off the production line.
Citation Information
Cited By
Low-brittle-transition-temperature low-temperature steel with excellent corrosion resistance and manufacturing method
CN122358052A