Wafer-level single-layer MX2 film and preparation and application thereof
By performing chemical vapor deposition on an unpolarized lithium niobate substrate, combined with temperature and time control, the controllability and uniformity of wafer-level single-layer MoS2 film is solved, and efficient preparation and application to electrical devices is achieved. Effect.
Patent Information
- Application Number
- CN202410944761.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-05
AI Technical Summary
The prior art has problems of poor controllability, poor uniformity and stability in preparing wafer-level uniformity and application in integrated circuits, making it difficult to achieve large-scale mass production and application in integrated circuits.
The deposition of MX2 films is carried out on an unpolarized lithium niobate substrate by chemical vapor deposition method. By controlling the deposition temperature and time, combining the deposition additives and carrier gas flow, the wafer-level single layer MX2 is efficient and controllable. film.
It has achieved high-quality and good thickness uniformity in single-layer MX2 film preparation, suitable for the application of electrical devices, and has the advantages of good reproducibility, simple operation and simple equipment.
Smart Images

Figure CN118895487A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of nanomaterials, and in particular relates to the field of preparation of wafer-level uniform single-layer two-dimensional material films. Technical Background
[0002] Chemical vapor deposition (CVD) is a promising and scalable method for preparing 2D-TMDs 1-3 MoS2 is the most representative and widely studied 2D-TMD material. It has an adjustable band gap, high carrier mobility, high on / off ratio and ideal power consumption. It is expected to become an ideal channel material for the next generation of new low-dimensional semiconductor devices. 4-8 The preparation of high-quality wafer-level uniform single-layer MoS2 thin films is the key to realizing the high-end industrial application of MoS2. In recent years, the work of preparing wafer-level MoS2 thin films by using the interaction between the sapphire substrate surface, the steps and the material has achieved unprecedented success. 9-14 . However, there are still two huge challenges in the process of preparing wafer-level MoS2 films by CVD. One is that it is difficult to accurately control the CVD synthesis process. Slight changes in the growth parameters will affect the repeatability of the experimental results, making it difficult to achieve large-scale batch production of wafer-level MoS2 films. Another challenge is the control of the thickness uniformity of the MoS2 film. The spatial concentration gradient of the gaseous precursor source inevitably leads to uneven thickness of the MoS2 film, which greatly limits its application in large-scale integrated circuits. The stable and efficient preparation of wafer-level uniform MoS2 films remains a major challenge.
[0003] References
[0004] 1. Q. Ji, C. Li, J. Wang, J. Niu, Y. Gong, Z. Zhang, Q. Fang, Y. Zhang, J. Shi, L. Liao, X. Wu, L. Gu, Z. Liu, Y. Zhang, Nano Lett. 2017, 17, 4908.
[0005] 2. Z. Zhang, J. Niu, P. Yang, Y. Gong, Q. Ji, J. Shi, Q. Fang, S. Jiang, H. Li, X. Zhou, L. Gu, X. Wu, Y. Zhang, Adv. Mater. 2017, 29, 1702359.
[0006] 3. H. Wang, X. Huang, J. Lin, J. Cui, Y. Chen, C. Zhu, F. Liu, Q. Zeng, J. Zhou, P. Yu, X. Wang, H. He, S. H. Tsang, W. Gao, K. Suenaga, F. Ma, C. Yang, L. Lu, T. Yu, E. H. T. Teo, G. Liu, Z. Liu, Nat. Commun. 2017, 8, 394.
[0007] 4.H.Wang,K.Kalantar-Zadeh,A.Kis,N.Coleman,S.Strano,Nat.Nanotech.2012,7,699.
[0008] 5.H.Yu,Y.Ong,L.Li,B.Xu,G.Zhang,W.Zhang,Y.Shi,R.Wang,Adv.Func.Mater.2017,27,104093.
[0009] 6. Z. Wang, R. Ma, J. Zhu, H. Wan, Y. Yue, L. Ma, R. Ma, L. Yang, H. Wang, Q. Li, X. Qian, Y. Yue, H. Wang, T. Zhong, Y. Zhou, P. Gao, S. Ruan, Y. Hu, Y. Liang, J. Dai, Adv. Mater. 2018, 30, 1800106.
[0010] 7. N. Li, Q. Wang, C. Shen, Z. Wei, H. Yu, J. Zhao, B. Lu, L. Wang, L. He, L. Xie, Q. Zhu, J. Du, R. Yang, X. Shi, Y. Zhang, Nat. Electro. 2020, 3, 711.
[0011] 8. Q. Zeng, Y. Xiao, X. Liu, N. Yang, L. Fu, Chem. Rev. 2018, 118, 6236.
[0012] 9. H. Yu, Z. Liao, J. Zhao, D. Liu, J. Zhou, Z. Wei, Z. Xu, H. Liu, H. Hu, K. Deng, Y. Zhou, A. Shi, L. Gu, C. Shen, T. Zhang, J. Du, L. Xie, Q. Zhu, W. Chen, R. Yang, X. Shi, Y. Zhang, ACS. Nano, 2017, 11, 12001.
[0013] 10. Q. Wang, N. Li, J. Tang, Q. Zhu, H. Zhang, Q. Jia, Y. Lu, Z. Wei, H. Yu, C. Zhao, T. Guo, L. Gu, G. Sun, W. Yang, R. Yang, X. Shi, Y. Zhang, Nano Lett. 2020, 20, 7193.
[0014] 11. L. Li, Q. Wang, F. Wu, L. Xu, P. Tian, H. Huang, H. Wang, X. Zhao, H. Zhang, K. Fan, Z. Li, L. Peng, K. Zhang, S. Ji, M. Zhi, C. Sun, T. Zhu, D. Zhu, P. Lu, Y. Lu, P. Wang, D. Bai, Y. Xu, W. Yang, N. Li, X. Shi, D. Xian, H. Liu, J. Du, Y. Zhang, Nat. Commun. 2024, 15, 1825.
[0015] 12. T. Li, W. Guo, L. Ma, S. Li, H. Yu, Z. Han, S. Gao, L. Liu, X. Fan, X. Wang, Y. Yang, Y. Lin, Z. Luo, Q. Chen, X. Dai, C. Tu, F. Pan, G. Yao, P. Wang, F. Nie, L. Wang, Y. Shi, R. Wang, Nat. Nanotech. 2021, 16, 1201.
[0016] 13.H.Fu,C.Min,K.Chang,C.Tseng,X.Wang,H.Sugisaki,Y.Li,M.Chang,I.Alnami,R.Syong,C.Lin,F.Fang,L.Zhao ,H.Luo,S.Lai,S.Chiu,S.Jian,H.Chang,J.Lu,K.Shih,J.Li,Y.Wan,M.Shi,V.Tung,Nat.Nanotech.2023,18,1289.
[0017] 14. G. Zuo, C. Liu, P. Ding, X. Qiao, P. Tian, C. Liu, H. Wang, D. Xue, L. You, L. Guo, H. Wang, Y. Fu, H. Liu, X. Zhou, H. Hong, H. Wu, B. Lu, R. Yang, Y. Zhang, P. Yu, G. Wang, D. Bai, F. Ding, H. Liu, Nat. Commun. 2024, 13, 1007. Summary of the invention
[0018] In view of the problems of poor controllability, uniformity and stability in the existing single-layer MX2 film preparation methods, the first purpose of the present invention is to provide a method for preparing a wafer-level single-layer MX2 film, aiming to controllably and efficiently synthesize a wafer-level single-layer MX2 film with good uniformity.
[0019] The second object of the present invention is to provide a wafer-level single-layer MX2 film prepared by the preparation method.
[0020] The third object of the present invention is to provide an application of the wafer-level single-layer MX2 film in the preparation of electrical devices.
[0021] A method for preparing a wafer-level single-layer MX2 film, wherein an M source and an X source are volatilized and chemically vapor deposited on the surface of a material A to form a wafer-level single-layer MX2 film on the surface of the material A;
[0022] The M in the M source is a transition metal element; the X source is at least one of sulfur and selenium;
[0023] The material A is an unpolarized self-polarizing material;
[0024] The temperature of the chemical vapor deposition stage is 450-900°C; the time of the chemical vapor deposition is more than 9 minutes.
[0025] The present invention shows that the innovative chemical vapor deposition of the MX2 on the surface of the unpolarized material A, combined with the combined control of the deposition temperature and time, can unexpectedly obtain a single-layer MX2 film with good wafer-level uniformity and stability. In addition, the preparation method of the present invention is easy to implement and has the advantage of a wide temperature range, especially the low-temperature preparation of the single-layer MX2 film.
[0026] In the present invention, in the M source, the M is at least one of Mo and W;
[0027] In the present invention, the M source is at least one of a simple substance and an oxide of M;
[0028] In the present invention, the volatilization temperature of the M source and the X source can be reasonably regulated according to the conventional CVD preparation principle. For example, the M source is a single substance of molybdenum, and its volatilization temperature is 650-800°C; or, the M source is a molybdenum oxide, and its volatilization temperature is 500-700°C. Or, the M source is a tungsten oxide, and its volatilization temperature is 850-950°C;
[0029] Preferably, the volatilization temperature of MoO3 is 530-600°C, and the volatilization temperature of WO3 is 850-950°C.
[0030] In the present invention, the X source is sulfur, and its volatilization temperature is 150°C to 240°C; or, the X source is selenium, and its volatilization temperature is 280°C to 400°C;
[0031] In the present invention, the weight ratio of the M source to the X source is 0.015-0.03:2-4;
[0032] In the present invention, a deposition aid is further added during the vapor deposition stage, wherein the deposition aid is an alkali metal salt raw material, preferably at least one of sodium chloride, potassium chloride, ammonium chloride and potassium iodide;
[0033] Preferably, the deposition aid and the M source are mixed and are in the same temperature zone;
[0034] Preferably, the weight ratio of the deposition aid to the M source is 1:1-50; further 1:3-35.
[0035] In the present invention, the material A is a material that is not artificially polarized but has self-polarization capability. For example, the material A is at least one of unpolarized lithium niobate, strontium titanate, and lanthanum aluminate;
[0036] Preferably, the material A is at least one of unpolarized Z-cut lithium niobate and X-cut lithium niobate.
[0037] In the present invention, the material A has a flat surface, and its surface size has no special requirements and can be adjusted according to the preparation scale. For example, it can be 0.1 cm 2 Above, for example, 0.5 to 100 cm 2 , and further can be 1 to 10 cm 2 .
[0038] In the present invention, the carrier gas for chemical vapor deposition is a protective gas; further, it is at least one of nitrogen and an inert gas;
[0039] Preferably, the flow rate of the protective atmosphere is 70 to 500 sccm;
[0040] Preferably, the carrier is also allowed to contain oxygen, wherein the flow rate of oxygen is below 10 sccm.
[0041] In the present invention, chemical vapor deposition is carried out in an improved CVD device, which includes a reaction tube and a sealing device A and a sealing device B for sealing both ends of the reaction tube; wherein the sealing device A is provided with an inlet pipe for supplying gas to the reaction tube; the sealing device B is provided with an exhaust pipe for outputting the gas in the reaction tube; the inlet pipe includes a carrier gas pipe and a raw material gas control pipe;
[0042] The CVD equipment also includes a temperature control device (such as a heating furnace) for controlling the temperature of the raw material and the substrate;
[0043] In the chemical vapor deposition stage, the X source is arranged in advance in the carrier gas upstream region of the reaction tube (close to the sealing device A side), the material A is arranged in the carrier gas downstream region (close to the sealing device B side), and the M source is arranged between the X source and the material A substrate and arranged in the raw material gas control pipe; then the carrier gas is introduced into the reaction tube chamber through the carrier gas pipe and the raw material gas control pipe, and the temperatures of the temperature zones where the X source, the M source and the material A substrate are located are controlled respectively, so that the X source and the M source are volatilized and deposited on the surface of the material A.
[0044] In the present invention, the specific positions of the X source, the M source and the material A are conventionally adjusted according to the required setting temperature.
[0045] The research of the present invention shows that the use of the equipment further in conjunction with the process of the present invention can further facilitate the coordinated preparation of the wafer-level single-layer MX2 film.
[0046] In the present invention, the flow rate of the atmosphere in the carrier gas tube is 100 to 400 sccm;
[0047] Preferably, the flow rate of the atmosphere in the raw material control gas pipe is 50 to 300 sccm, and further preferably 70 to 250 sccm.
[0048] In the present invention, the temperature of chemical vapor deposition is 450-850°C;
[0049] Preferably, the chemical vapor deposition time is 10 to 60 minutes, further 10 to 20 minutes.
[0050] The present invention also provides a wafer-level single-layer MX2 film prepared by the preparation method.
[0051] The present invention also provides an application of the wafer-level single-layer MX2 film, which is applied to the preparation of electrical devices;
[0052] In the present invention, the field effect transistor can be prepared based on conventional means, for example, the steps are:
[0053] The wafer-level single-layer MX2 film is transferred to a silicon wafer substrate using a thermal release adhesive; an electrode pattern is prepared by exposing on a sacrificial substrate using a UV photolithography machine, and then a metal is deposited on the surface of the sacrificial substrate to obtain an electrode, and the electrode is transferred to the sample surface on the silicon wafer substrate through a transfer platform to obtain a field effect transistor;
[0054] Preferably, the sacrificial substrate is a silicon wafer substrate, and the oxide layer thickness is 285nm;
[0055] Preferably, the metal is Au;
[0056] Preferably, the thickness of the metal Au is 100 nm.
[0057] The present invention also provides an electrical device, comprising the wafer-level single-layer MX2 film described in the present invention, or made from the wafer-level single-layer MX2 film described in the present invention.
[0058] Beneficial Effects
[0059] The present invention adopts the material A as the CVD substrate of MX2, and unexpectedly can grow the single-layer MX2 film efficiently, controllably and with high uniformity.
[0060] Taking the MX2 film as MoS2 as an example, its thickness is as thin as 0.8nm, the size is 1 to 10μm, and the morphology is good and quasi-circular. The single-layer MoS2 film material has good crystallinity, high quality, high thickness uniformity, and the film size is 1 to 3cm. MoS2 field effect transistors can be prepared using this method. The present invention can quickly prepare ultra-thin and ultra-uniform wafer-level single-layer MoS2 films, which is crucial for basic research and potential technical applications of wafer-level uniform high-quality two-dimensional material films. The preparation process of the present invention does not require complicated operating steps and the use of expensive raw materials. The equipment is simple, and the operation is simple and easy with good reproducibility. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] Figure 1 Schematic diagram of a low-pressure chemical vapor deposition device for preparing a uniform single-layer MoS2 thin film material;
[0062] Figure 2 Photos of a Z-cut lithium niobate substrate (left) and a wafer-level uniform single-layer MoS2 film prepared on a Z-cut lithium niobate substrate in Example 1-1 (right);
[0063] Figure 3 Schematic diagram of the optical performance of a single-layer MoS2 film prepared on a Z-cut lithium niobate substrate in Example 1-1;
[0064] Figure 4 Schematic diagram of the optical performance of a single-layer MoS2 film prepared on a Z-cut lithium niobate substrate in Example 1-2;
[0065] Figure 5 Schematic diagram of the optical performance of a single-layer MoS2 film prepared on a Z-cut lithium niobate substrate in Example 1-3;
[0066] Figure 6 Schematic diagram of the optical performance of a single-layer MoS2 film prepared on a Z-cut lithium niobate substrate in Example 1-4;
[0067] Figure 7A picture of a single-layer MoS2 film prepared on a Z-cut lithium niobate substrate in Example 1-5;
[0068] Figure 8 Schematic diagram of the optical performance of a single-layer MoS2 film prepared on a Z-cut lithium niobate substrate in Example 1-5;
[0069] Fig. 9 A picture of a single-layer MoS2 film prepared on a Z-cut lithium niobate substrate in Example 1-6;
[0070] Fig.10 Schematic diagram of the optical performance of a single-layer MoS2 film prepared on a Z-cut lithium niobate substrate in Example 1-6;
[0071] Fig.11 A picture of a single-layer MoS2 film prepared on a Z-cut lithium niobate substrate in Example 1-7;
[0072] Fig.12 Schematic diagram of the optical performance of a single-layer MoS2 film prepared on a Z-cut lithium niobate substrate in Example 1-7;
[0073] Fig.13 A picture of a single-layer MoS2 film prepared on a Z-cut lithium niobate substrate in Example 1-8;
[0074] Fig.14 Schematic diagram of the optical performance of a single-layer MoS2 film prepared on a Z-cut lithium niobate substrate in Example 1-8;
[0075] Fig.15 A picture of a single-layer MoS2 film prepared on a Z-cut lithium niobate substrate in Example 1-9;
[0076] Fig.16 Schematic diagram of the optical performance of a single-layer MoS2 film prepared on a Z-cut lithium niobate substrate in Example 1-9;
[0077] Fig.17 A picture of a single-layer MoS2 film prepared on a Z-cut lithium niobate substrate according to Example 1-10;
[0078] Fig.18 Schematic diagram of the optical performance of a single-layer MoS2 film prepared on a Z-cut lithium niobate substrate in Example 1-10;
[0079] Fig.19 A picture of a single-layer MoS2 film prepared on a Z-cut lithium niobate substrate in Example 1-11;
[0080] Fig. 20 Schematic diagram of the optical performance of a single-layer MoS2 film prepared on a Z-cut lithium niobate substrate in Example 1-11;
[0081] Fig.21 A picture of a single-layer MoS2 film prepared on a Z-cut lithium niobate substrate according to Example 1-12;
[0082] Fig. 22 Schematic diagram of the optical performance of a single-layer MoS2 film prepared on a Z-cut lithium niobate substrate in Example 1-12;
[0083] Fig.23 This is a picture of multiple single-layer MoS2 films obtained by repeated reaction on a Z-cut lithium niobate substrate in Example 1-1;
[0084] Fig.24 Pictures of an X-cut lithium niobate substrate (left) and a single-layer MoS2 film prepared on an X-cut lithium niobate substrate in Example 1-13 (right);
[0085] Fig.25 Schematic diagram of the optical performance of a single-layer MoS2 film prepared on an X-cut lithium niobate substrate in Example 1-13;
[0086] Fig.26 Schematic diagram of the optical structure of the WSe2 film prepared on the Z-cut lithium niobate substrate in Example 1-14;
[0087] Fig. 27 Atomic force microscope images of WSe2 thin films prepared on Z-cut lithium niobate substrates according to Examples 1-14;
[0088] Fig.28 This is an optical schematic diagram of the MoS2 thin film prepared on the c-plane sapphire substrate in Comparative Example 1-1;
[0089] Fig.29 Schematic diagram of the optical performance of the MoS2 thin film prepared on the SiO2 / Si substrate in Comparative Example 1-2;
[0090] Fig.30 This is a picture of the MoS2 field effect transistor prepared on the SiO2 / Si substrate in Example 2-1;
[0091] Fig.31 This is the electrical transfer characteristic curve of the MoS2 field effect transistor in implementation case 2-1.
[0092] Fig.32 The electrical output characteristic curve of the MoS2 field effect transistor in Example 2-1;
[0093] Fig.33 Statistics of electrical transfer characteristic curves of 20 MoS2 field effect transistors in Example 2-1;
[0094] Fig.34 Statistics of electrical output characteristic curves of 20 MoS2 field effect transistors in Example 2-1;
[0095] Fig.35 The carrier mobility curve statistics of 20 MoS2 field effect transistors in Example 2-1; DETAILED DESCRIPTION
[0096] The present invention is further described below through implementation cases, but the content of the present invention is not limited to the following content.
[0097] In the present invention, as an implementable solution, the Figure 1 The CVD equipment is used to carry out the CVD deposition preparation, which includes a reaction tube and a sealing device A and a sealing device B for sealing both ends of the reaction tube; wherein the sealing device A is provided with an inlet pipe for supplying gas to the reaction tube; the sealing device B is provided with an exhaust pipe for outputting the gas in the reaction tube; the inlet pipe includes a carrier gas pipe and a raw material gas control pipe; the inlet pipe is connected to the gas source, and the outlet is arranged in the CVD chamber, wherein the outlet of the carrier gas pipe is arranged near the sealing device A side, and the raw material gas control pipe is arranged in the chamber area where the temperature can be controlled.
[0098] The CVD equipment also includes a temperature control device for controlling the temperature of the raw material and the substrate;
[0099] During the CVD deposition process, the X source is pre-arranged in the carrier gas upstream region of the reaction tube, the material A is pre-arranged in the carrier gas downstream region, and the M source is pre-arranged between the X source and the material A substrate and in the raw material gas control pipe. Subsequently, the carrier gas is introduced into the reaction tube chamber through the carrier gas pipe and the raw material gas control pipe, and the temperatures of the temperature zones where the X source, the M source and the material A substrate are located are respectively controlled, so that the X source and the M source are volatilized and deposited on the surface of the material A.
[0100] In the present invention, as an exemplified scheme, the material A is taken as a non-polarized lithium niobate substrate, and the MX2 is taken as MoS2. The exemplified preparation process is, for example: volatilizing a mixed raw material of a transition metal raw material and an alkali metal salt and a chalcogen raw material and depositing them on the surface of the lithium niobate substrate; controlling the carrier gas flow rate of the deposition process to be 70-510 sccm; and the deposition temperature to be 450-850°C;
[0101] In the mixed raw materials, the transition metal raw material is MoO3, the alkali metal salt is NaCl; the volatilization temperature thereof is 500-700°C; the chalcogen raw material is S powder, and the volatilization temperature thereof is 150-240°C; the carrier gas component is a mixed gas of protective gas Ar and reactive gas O2; the flow rate of protective gas Ar is 70-500sccm, and the flow rate of reactive gas O2 is 0-10sccm.
[0102] The substrate is a lithium niobate substrate; the lithium niobate substrate is a Z-cut lithium niobate substrate and an X-cut lithium niobate substrate.
[0103] The present invention innovatively discovered that by reacting and growing a mixture of a transition metal oxide raw material MoO3 and an alkali metal salt NaCl and an S raw material on the surface of a lithium niobate substrate, a wafer-level ultra-uniform single-layer MoS2 thin film material can be quickly obtained through van der Waals epitaxy. On this basis, the carrier gas flow rate, deposition temperature, and raw material volatilization temperature are further changed, and a uniform single-layer MoS2 thin film material can still be obtained on the lithium niobate substrate in a controllable manner. On this basis, multiple repeated experiments are carried out, and a uniform single-layer MoS2 thin film material can be stably and repeatedly obtained on the lithium niobate substrate.
[0104] Preferably, the lithium niobate substrate is a Z-cut lithium niobate substrate and an X-cut lithium niobate substrate; preferably a Z-cut lithium niobate substrate. Studies have found that by using a lithium niobate substrate as a growth substrate, an ultra-uniform single-layer MoS2 thin film material can be quickly, stably and controllably obtained within an ultra-wide growth window. The lithium niobate substrate is not pre-polarized but has spontaneous polarization, and the polarization direction of the Z-cut lithium niobate substrate is along the c-axis direction, forming a strongly polarized surface. Compared with sapphire and SiO2 / Si substrates, the adsorption energy and diffusion energy of a single MoS2 domain on a lithium niobate substrate are lower, which is conducive to the migration and aggregation of MoS2 precursor molecules on the lithium niobate substrate, making it easy to nucleate on the lithium niobate substrate, and the growth of the MoS2 nucleus is also changed from conventional thermodynamically controlled diffusion growth to kinetically controlled isotropic growth. In addition, the lithium niobate substrate has an atomically flat surface, which has better lattice matching with the two-dimensional material MoS2. The strongly polarized surface of lithium niobate can regulate the electrical and optical properties of the MoS2 material grown thereon. These characteristics ensure the advantages of lithium niobate substrate in the growth of single-layer uniform MoS2 thin film materials.
[0105] The following are more specific typical solutions:
[0106] 1. Preparation of single-layer MoS2 film on Z-cut lithium niobate substrate:
[0107] Example 1-1
[0108] The experimental setup of single-layer MoS2 film is shown in the figure. Figure 1As shown. The independent source tube (inlet tube) of the device includes a raw material gas control tube and a carrier gas tube, and a heating belt is added to the gas inlet end of the quartz tube. A porcelain boat containing a mixed powder of MoO3 and NaCl with a mass ratio of 30:1 is placed in the constant temperature zone 1 of the raw material gas control tube, and sulfur powder is placed in the heating belt area outside the quartz tube (upstream of the carrier gas). A Z-cut lithium niobate substrate with a thickness of 500μm is used as a growth substrate for a single-layer MoS2 film. It is placed on another porcelain boat and placed in the constant temperature zone 2 (downstream of the carrier gas) of the tube furnace to obtain an appropriate crystal growth temperature. The weight ratio of molybdenum oxide to sulfur is 0.02:3; before heating, a large flow of argon gas is used and a vacuum pump is used to exhaust the air in the reaction chamber. Then, the heating zone outside the quartz tube and the constant temperature zones 1 and 2 are heated to 220°C (sulfur volatilization temperature), 530°C (molybdenum oxide volatilization temperature) and 850°C (deposition temperature), respectively. The argon flow rate in the raw material control gas pipe is 75sccm, the oxygen flow rate is 3sccm, the flow rate in the carrier gas pipe is 200sccm, the constant temperature deposition time is 10min (deposition time), and a certain vacuum degree is maintained for reaction. Wafer-level uniform single-layer MoS2 film can be prepared on the Z-cut lithium niobate substrate. The photo of the prepared wafer-level single-layer MoS2 film is shown in the figure. Figure 2 As shown, the optical photograph of wafer-level single-layer MoS2 film is as follows Figure 3 shown.
[0109] Figure 2 This is a photo of the single-layer MoS2 film prepared in this case. The left picture shows the Z-cut lithium niobate substrate before growth, and the right picture shows the Z-cut lithium niobate substrate with a single-layer MoS2 film deposited on it. The film size is 3*3cm. Figure 3 This is an optical schematic diagram of the single-layer MoS2 film prepared in this case. 1 in the figure represents the Z-cut lithium niobate substrate, and 2 in the figure represents the grown MoS2 film. The single-layer MoS2 film obtained under this condition has good crystallinity, a clean and pollution-free surface, and highly uniform thickness. Figure 3 The scale bar in the figure is 20 μm.
[0110] Example 1-2
[0111] Compared with Example 1-1, the only difference is that the constant temperature deposition time is 5 minutes, and other operations and parameters are the same as Example 1-1. Figure 4 This is an optical schematic diagram of MoS2 nanosheets prepared on a Z-cut lithium niobate substrate. 1 in the figure represents the Z-cut lithium niobate substrate, and 2 in the figure represents a single-layer MoS2 nanosheet. The circular single-layer MoS2 nanosheets obtained under this condition have good crystallinity, a domain size of 1-3μm, and uniform thickness. Figure 4 The scale bar in the figure is 20 μm.
[0112] Examples 1-3
[0113] Compared with Example 1-1, the only difference is that the constant temperature deposition time is 8 minutes, and other operations and parameters are the same as Example 1-1. Figure 5 This is an optical schematic diagram of MoS2 nanosheets prepared on a Z-cut lithium niobate substrate. 1 in the figure represents the Z-cut lithium niobate substrate, and 2 in the figure represents a single-layer MoS2 nanosheet. The circular single-layer MoS2 nanosheets obtained under this condition have good crystallinity, the domain size increases to 5-10μm, and the thickness is uniform. Figure 5 The scale bar in the figure is 20 μm.
[0114] Examples 1-4
[0115] Compared with Example 1-1, the only difference is that the constant temperature deposition time is 15 minutes, and other operations and parameters are the same as Example 1-1. Figure 6 This is an optical schematic diagram of MoS2 nanosheets prepared on a Z-cut lithium niobate substrate. 1 in the figure represents the Z-cut lithium niobate substrate, and 2 in the figure represents a single-layer MoS2 film. The circular single-layer MoS2 nanosheets obtained under this condition have good crystallinity, the domain size increases to 5-10μm, and the thickness is uniform. Figure 6 The scale bar in the figure is 20 μm.
[0116] Examples 1-5
[0117] Compared with Example 1-1, the only difference is that the deposition temperature is 750°C, and other operations and parameters are the same as Example 1-1. Figure 7 This is a photo of a single-layer MoS2 film prepared on Z-cut lithium niobate in this case. The film size is 1*1cm. Figure 8 This is an optical schematic diagram of a single-layer MoS2 film prepared on Z-cut lithium niobate in this case. The single-layer MoS2 film obtained under this condition has good crystallinity, a clean and pollution-free surface, and highly uniform thickness. Figure 8 The scale bar in the figure is 20 μm.
[0118] Examples 1-6
[0119] Compared with Example 1-1, the only difference is that the deposition temperature is 650°C, and other operations and parameters are the same as Example 1-1.
[0120] Fig. 9 This is a photo of a single-layer MoS2 film prepared on Z-cut lithium niobate in this case. The film size is 1*1cm. Fig.10 This is an optical schematic diagram of a single-layer MoS2 film prepared on Z-cut lithium niobate in this case. The single-layer MoS2 film obtained under this condition has good crystallinity, a clean and pollution-free surface, and highly uniform thickness. Fig.10 The scale bar in the figure is 20 μm.
[0121] Examples 1-7
[0122] Compared with Example 1-1, the only difference is that the deposition temperature is 550° C., and other operations and parameters are the same as Example 1-1.
[0123] Fig.11 This is a photo of a single-layer MoS2 film prepared on Z-cut lithium niobate in this case. The film size is 1*1cm. Fig.12 This is an optical schematic diagram of a single-layer MoS2 film prepared on Z-cut lithium niobate in this case. The single-layer MoS2 film obtained under this condition has good crystallinity, a clean and pollution-free surface, and highly uniform thickness. Fig.12 The scale bar in the figure is 20 μm.
[0124] Examples 1-8
[0125] Compared with Example 1-1, the only difference is that the deposition temperature is 450°C, and other operations and parameters are the same as Example 1-1.
[0126] Fig.13 This is a photo of a single-layer MoS2 film prepared on Z-cut lithium niobate in this case. The film size is 1*1cm. Fig.14 This is an optical schematic diagram of a single-layer MoS2 film prepared on Z-cut lithium niobate in this case. The single-layer MoS2 film obtained under this condition has good crystallinity, a clean and pollution-free surface, and highly uniform thickness. Fig.14 The scale bar in the figure is 20 μm.
[0127] Examples 1-9
[0128] Compared with Example 1-1, the only difference is that the flow rate in the carrier gas tube is 125 sccm, and other operations and parameters are the same as Example 1-1.
[0129] Fig.15 This is a photo of a single-layer MoS2 film prepared on Z-cut lithium niobate in this case. The film size is 1*1cm. Fig.16 This is an optical schematic diagram of a single-layer MoS2 film prepared on Z-cut lithium niobate in this case. The single-layer MoS2 film obtained under this condition has good crystallinity, a clean and pollution-free surface, and highly uniform thickness. Fig.16 The scale bar in the figure is 20 μm.
[0130] Examples 1-10
[0131] Compared with Example 1-1, the only difference is that the carrier gas in the raw material control gas pipe is Ar, and its flow rate is 100 sccm, and the carrier gas in the carrier gas pipe is Ar, and its flow rate is 300 sccm. Other operations and parameters are the same as Example 1-1.
[0132] Fig.17 This is a photo of a single-layer MoS2 film prepared on Z-cut lithium niobate in this case. The film size is 1*1cm. Fig.18This is an optical schematic diagram of a single-layer MoS2 film prepared on Z-cut lithium niobate in this case. The single-layer MoS2 film obtained under this condition has good crystallinity, a clean and pollution-free surface, and highly uniform thickness. Fig.18 The scale bar in the figure is 20 μm.
[0133] Embodiment 1-11
[0134] Compared with Example 1-1, the only difference is that the argon flow rate in the raw material control gas pipe is 200 sccm, and the flow rate in the carrier gas pipe is 300 sccm. Other operations and parameters are the same as Example 1-1.
[0135] Fig.19 This is a photo of a single layer of MoS2 prepared on Z-cut lithium niobate in this case, with a domain size of approximately 1-3μm. Fig. 20 This is an optical schematic diagram of a single-layer MoS2 film prepared on Z-cut lithium niobate in this case. Under this condition, the single-layer MoS2 domain obtained has reduced crystallinity, a smaller domain size, and a low film-forming rate. Fig. 20 The scale bar in the figure is 20 μm.
[0136] Examples 1-12
[0137] Compared with Example 1-1, the only difference is that the volatilization temperature of MoO3 powder is 540°C, and the other operations and parameters are the same as Example 1-1. Fig.21 This is a photo of a single-layer MoS2 film prepared on Z-cut lithium niobate in this case. The film size is 1*1cm. Fig. 22 This is an optical schematic diagram of a single-layer MoS2 film prepared on Z-cut lithium niobate in this case. The single-layer MoS2 film obtained under this condition has good crystallinity, a clean and pollution-free surface, and highly uniform thickness. Fig. 22 The scale bar in the figure is 20 μm.
[0138] Examples 1-13
[0139] Compared with Example 1-1, the only difference is that an X-cut lithium niobate substrate is used instead, and other operations and parameters are the same as Example 1-1. Fig.24 This is a photo of a single-layer MoS2 film prepared on X-cut lithium niobate in this case. The film size is 1*1cm. Fig.25 This is an optical schematic diagram of a single-layer MoS2 film prepared on X-cut lithium niobate in this case. 1 in the figure represents the X-cut lithium niobate substrate, and 2 in the figure represents the single-layer MoS2 film. The single-layer MoS2 film obtained under this condition has good crystallinity, a clean and pollution-free surface, and highly uniform thickness. Fig.25 The scale bar in the figure is 20 μm.
[0140] Examples 1-14
[0141] Place a porcelain boat containing a 3:1 WO3 and NaCl mixed powder in constant temperature zone 1 of the raw material gas control tube, place selenium powder in the heating zone outside the quartz tube, and place a 500 μm thick Z-cut lithium niobate substrate as the growth substrate of the WSe2 film on another porcelain boat and place it in constant temperature zone 2 of the tube furnace to obtain an appropriate crystal growth temperature. The weight ratio of WO3 and Se is 0.03:4;
[0142] Before heating, use a large flow of argon gas and a vacuum pump to exhaust the air in the reaction chamber. Then heat the heating zone and constant temperature zones 1 and 2 to 350°C (selenium volatilization temperature), 880°C (tungsten oxide volatilization temperature), and 850°C (deposition temperature), respectively. The argon flow rate in the raw material control gas pipe is 100 sccm, the flow rate in the carrier gas pipe is 200 sccm, the constant temperature deposition time is 15 minutes (deposition time), and a certain vacuum degree is maintained for the reaction. A large-area uniform WSe2 film with a thickness of ~4nm can be prepared on a Z-cut lithium niobate substrate. The optical photograph of the prepared large-area WSe2 film is shown in Figure 2. Fig.26 As shown, the atomic force microscopy image of large-area WSe2 film is as follows Fig. 27 shown.
[0143] Comparative Example 1-1
[0144] Compared with Example 1-1, the only difference is that the growth substrate is replaced with a sapphire substrate, and other operations and parameters are the same as Example 1-1.
[0145] Fig.28 This is an optical schematic diagram of the single-layer MoS2 film prepared on c-plane sapphire in this case. The single-layer MoS2 film obtained under this condition has nuclei and multi-layer MoS2 deposition on the surface, and the thickness is uneven. Fig.28 The scale bar in the figure is 20 μm.
[0146] Comparative Example 1-2
[0147] Compared with Example 1-1, the only difference is that the growth substrate is replaced with a SiO2 / Si substrate, and the other operations and parameters are the same as Example 1-1.
[0148] Fig.29 This is an optical schematic diagram of the single-layer MoS2 film prepared on the SiO2 / Si substrate in this case. Under this condition, the single-layer MoS2 film obtained has nuclei and multi-layer MoS2 deposition on the surface, with low film formation rate and uneven thickness. Fig.29 The scale bar in the figure is 20 μm.
[0149] 2. Field Effect Transistor Preparation
[0150] Example 2-1
[0151] The preparation method of MoS2 field effect transistor is to transfer the MoS2 film prepared by CVD on Z-cut lithium niobate substrate to SiO2 / Si substrate (material prepared in Example 1-1), and use a transfer platform to transfer 100nm Au electrode to the MoS2 film on SiO2 / Si substrate to obtain MoS2 field effect transistor. The picture of the prepared MoS2 field effect transistor is shown in Fig.30 As shown, the scale bar in the figure is 200μm.
[0152] Fig.31 is the transfer characteristic curve of MoS2 field effect transistor; Fig.32 is the output characteristic curve of MoS2 field effect transistor; Fig.33 Statistics of transfer characteristic curves of 20 MoS2 field effect transistors; Fig.34 Statistics of output characteristic curves of 20 MoS2 field effect transistors; Fig.35 The carrier mobility statistics of 20 MoS2 field effect transistors prove that the single-layer MoS2 film prepared by the present invention has n-type semiconductor behavior and has good electrical properties and electrical uniformity.
[0153] In summary, the research found that the rapid and successful preparation of epitaxial wafer-level uniform single-layer MoS2 film on lithium niobate substrate is highly controllable and repeatable. On this basis, by further adjusting the volatilization temperature, deposition temperature, carrier gas flow rate, deposition time and other parameters of the raw materials, a single-layer uniform MoS2 film material can still be quickly and stably obtained on the lithium niobate substrate. For example, the deposition temperature of MoS2 is further changed, the mixed raw materials of MoO3 and NaCl are volatilized at a volatilization temperature of 530-700℃, and the S powder is volatilized at a volatilization temperature of 200-240℃; the volatilized raw materials react and grow on the surface of the lithium niobate substrate at a carrier gas flow rate of 70-510sccm and a deposition temperature of 450-850℃, which is helpful to successfully prepare a single-layer uniform MoS2 film material on the lithium niobate substrate; further research found that in multiple experiments, a uniform single-layer MoS2 film material can be repeatedly obtained, and the experimental repeatability is high.
Claims
1. A wafer-level single-layer MX 2 Method for preparing thin film, Features: The M source and the X source are volatilized and chemically vapor deposited on the surface of material A to form a wafer-level single-layer MX on the surface of material A. 2 film; The M in the M source is a transition metal element; the X source is at least one of sulfur and selenium; The material A is an unpolarized self-polarizing material; The temperature of the chemical vapor deposition stage is 450-900°C; the time of the chemical vapor deposition is more than 9 minutes.
2. The wafer-level single-layer MX 2 Method for preparing thin film, Features: In the M source, the M is at least one of Mo and W; Preferably, the M source is at least one of a simple substance and an oxide of M; Preferably, the M source is a single substance of molybdenum, and its volatilization temperature is 650-800°C; or, the M source is a molybdenum oxide, and its volatilization temperature is 500-700°C; Or, the M source is tungsten oxide, and its volatilization temperature is 850-950°C; Preferably, the X source is sulfur, whose volatilization temperature is 150°C to 240°C; or, the X source is selenium, whose volatilization temperature is 280°C to 400°C; Preferably, the weight ratio of the M source to the X source is 0.015-0.03:2-4; Preferably, a deposition aid is also added during the vapor deposition stage, wherein the deposition aid is an alkali metal salt raw material, preferably at least one of sodium chloride, potassium chloride, ammonium chloride and potassium iodide; Preferably, the deposition aid and the M source are mixed and are in the same temperature zone; Preferably, the weight ratio of the deposition aid to the M source is 1:1-50; further 1:3-35.
3. The wafer-level single-layer MX 2 Method for preparing thin film, Features: The material A is at least one of unpolarized lithium niobate, strontium titanate, and lanthanum aluminate; Preferably, the material A is at least one of unpolarized Z-cut lithium niobate and X-cut lithium niobate.
4. The wafer-level single-layer MX 2 Method for preparing thin film, Features: The carrier gas for chemical vapor deposition is a protective gas; further, it is at least one of nitrogen and an inert gas; Preferably, the flow rate of the protective atmosphere is 70 to 500 sccm; Preferably, the carrier is also allowed to contain oxygen, wherein the flow rate of oxygen is below 10 sccm.
5. The wafer-level single-layer MX 2 Method for preparing thin film, Features: Chemical vapor deposition is carried out in an improved CVD device, which includes a reaction tube and a sealing device A and a sealing device B for sealing both ends of the reaction tube; wherein the sealing device A is provided with an inlet pipe for supplying gas to the reaction tube; the sealing device B is provided with an exhaust pipe for outputting gas in the reaction tube; the inlet pipe includes a carrier gas pipe and a raw material gas control pipe; The CVD equipment also includes a temperature control device for controlling the temperature of the raw material and the substrate; In the chemical vapor deposition stage, the X source is arranged in advance in the carrier gas upstream region of the reaction tube, the material A is arranged in the carrier gas downstream region, and the M source is arranged between the X source and the material A substrate and in the raw material gas control pipe; then the carrier gas is introduced into the reaction tube chamber through the carrier gas pipe and the raw material gas control pipe, and the temperatures of the temperature zones where the X source, the M source and the material A substrate are located are controlled respectively, so that the X source and the M source are volatilized and deposited on the surface of the material A.
6. The wafer-level single-layer MX 2 Method for preparing thin film, Features: The flow rate of the atmosphere in the carrier gas tube is 100 to 400 sccm; Preferably, the flow rate of the atmosphere in the raw material control gas pipe is 50 to 300 sccm, and further preferably 70 to 250 sccm.
7. The wafer-level single-layer MX 2 Method for preparing thin film, Features: The temperature of chemical vapor deposition is 450-850°C; Preferably, the chemical vapor deposition time is 10 to 60 minutes, further 10 to 20 minutes.
8. A wafer-level single-layer MX 2 film.
9. A wafer-level single-layer MX 2 Application of thin films, Features: Applied to the preparation of electrical devices; Preferably used for the preparation of a field effect transistor, the steps are: The wafer-level single-layer MX 2 The film is transferred to a silicon wafer substrate; An ultraviolet lithography machine is used to expose and prepare an electrode pattern on a sacrificial substrate, and then a metal is deposited on the surface of the sacrificial substrate to obtain an electrode. The electrode is transferred to the sample surface on the silicon wafer substrate through a transfer platform to obtain a field effect transistor; Preferably, the sacrificial substrate is a silicon wafer substrate, and the oxide layer thickness is 285nm; Preferably, the metal is Au; Preferably, the thickness of the metal Au is 100 nm.
10. An electrical device, It is characterized in that The wafer-level single-layer MX 2 thin film, or a wafer-level single-layer MX 2 Film obtained.