Processing method of magnesium alloy outer part

By carrying out oxidation-resistant treatment and forming porous oxide layers on the magnesium alloy exterior parts, combined with electric pore sealing treatment, the problem of corrosion of the magnesium alloy exterior parts after mechanical processing is solved, and long-term maintenance of its corrosion resistance and gloss is achieved .

CN118895545APending Publication Date: 2024-11-05CATCHER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311775969.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-02
Filing Date
2023-12-21
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Magnesium alloy exterior parts are prone to corrosion after machining, resulting in the inability to maintain the metallic gloss texture for a long time, and the prior art is difficult to take into account its light and thin functions and corrosion resistance.

Method used

The machining is performed using water-free cutting oil, and the pore sealing layer is formed by antioxidant treatment on the magnesium alloy substrate, and the pore sealing layer is formed, using alkaline antioxidant solution and pulse current anodizing treatment, combined with electrical pore sealing Treatment to reduce the chance of contact between the magnesium alloy substrate and air.

Benefits of technology

Effectively improve the corrosion resistance and gloss of magnesium alloy appearance parts, so that they maintain high gloss during long-term use, and verify their salt spray resistance through salt spray test.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895545A_ABST
    Figure CN118895545A_ABST
Patent Text Reader

Abstract

The invention discloses a processing method of a magnesium alloy outer part. The processing method of the magnesium alloy exterior part comprises at least the following steps. A magnesium alloy base material is provided, and the magnesium alloy base material is machined to form a drilling and cutting surface on the magnesium alloy base material. And carrying out antioxidant treatment on the machined magnesium alloy base material. And carrying out electrolytic treatment on the magnesium alloy base material subjected to the anti-oxidation treatment so as to form a porous oxide layer on the magnesium alloy base material. And forming a hole sealing layer on the porous oxide layer to obtain the magnesium alloy exterior part. The drilling and cutting surface of the magnesium alloy outer part has the glossiness ranging from 250 GU to 450 GU.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a processing method, in particular to a processing method for a magnesium alloy appearance part. Background Art

[0002] Today's portable electronic devices require a thin and light structure. Magnesium alloy has become a popular material for the housing and parts of portable electronic devices due to its excellent mechanical properties and light weight. In addition, after mechanical processing (such as drilling, polishing, laser engraving, etc.), magnesium alloy materials can present a metallic luster in appearance, giving the product a sense of quality.

[0003] Since magnesium alloys are susceptible to corrosion, their surfaces are usually anodized to form an anodized film to prevent them from being directly exposed to the air. However, after users have repeatedly touched the product, electrochemical corrosion can still easily occur on its surface, causing the product to be unable to maintain its metallic luster for a long time.

[0004] Therefore, how to improve the corrosion resistance of magnesium alloy objects by improving the processing steps and methods, so that they have both light and thin functionality and long-term corrosion resistance with metallic gloss, to overcome the above-mentioned defects, has become one of the important issues. Summary of the invention

[0005] The object of the present invention is to provide a method for processing a magnesium alloy appearance part in view of the deficiencies in the prior art, which can make the drilled surface of the magnesium alloy appearance part have a corrosion-resistant effect and maintain a certain glossiness for a long time.

[0006] The technical concept of the present invention is to immerse the machined magnesium alloy substrate in an antioxidant treatment liquid to reduce the contact of the machined surface of the magnesium alloy with air and avoid the risk of oxidation. In addition, no acidic reagents or solutions are used in the processing method of the present invention, which is conducive to maintaining high gloss and corrosion resistance.

[0007] Specifically, one of the technical solutions adopted by the present invention is to provide a method for processing a magnesium alloy appearance part, comprising at least the following steps: providing a magnesium alloy substrate; mechanically processing the magnesium alloy substrate to form a drilled surface on the magnesium alloy substrate; performing an anti-oxidation treatment on the magnesium alloy substrate after the mechanical processing; performing an electrolytic treatment on the magnesium alloy substrate after the anti-oxidation treatment to form a porous oxide layer on the magnesium alloy substrate; and performing an electric sealing treatment on the magnesium alloy substrate after the electrolytic treatment to form a sealing layer on the porous oxide layer to obtain a magnesium alloy appearance part. The drilled surface of the magnesium alloy appearance part after processing has a glossiness between 250GU and 450GU.

[0008] Furthermore, the machining includes applying cutting oil to the magnesium alloy substrate, and the cutting oil does not contain water.

[0009] Furthermore, the anti-oxidation treatment includes immersing the magnesium alloy substrate in an alkaline anti-oxidation solution.

[0010] Furthermore, the alkaline antioxidant solution contains 1 wt % to 50 wt % of sodium hydroxide or potassium hydroxide.

[0011] Furthermore, the electrolyte used in the electrolytic treatment comprises 5wt% to 15wt% of an aqueous potassium hydroxide solution, and the conditions of the electrolytic treatment include: an operating voltage of 40V to 80V, a temperature of 25°C to 40°C, and a treatment time of 20 minutes to 60 minutes.

[0012] Furthermore, the electrolytic treatment is a pulse current anodizing treatment; wherein the pulse voltage of the pulse current anodizing treatment is 40V to 80V, the temperature is 25°C to 35°C, the treatment time is 20 to 60 minutes, the duty cycle is 40% to 90%, and the frequency is 5,000Hz to 100,000Hz.

[0013] Furthermore, before the magnesium alloy substrate after the anti-oxidation treatment is subjected to the electrolytic treatment to form the porous oxide layer on the magnesium alloy substrate, the magnesium alloy substrate is also subjected to a pretreatment, which includes alkaline degreasing, decarburization and hot alkaline washing.

[0014] Furthermore, before the magnesium alloy substrate after the electrolysis treatment is subjected to the electric sealing treatment to form the sealing layer on the porous oxide layer, the magnesium alloy substrate is further subjected to dyeing treatment. The dyeing treatment includes filling a plurality of pores of the porous oxide layer with an alkaline reactive dye.

[0015] Furthermore, the solid content of the resin composition used in the electrosealing treatment is between 5wt% and 20wt%, and the conditions of the electrosealing treatment include: an operating voltage of 10V to 100V, a temperature of 25°C to 35°C, and a treatment time of 1 minute to 5 minutes.

[0016] Furthermore, the resin composition comprises epoxy resin or acrylic resin.

[0017] One of the beneficial effects of the present invention is that the processing method of the magnesium alloy appearance part provided by the present invention can reduce the chance of the drilled surface of the magnesium alloy substrate contacting the air during the processing through the technical scheme of "performing an anti-oxidation treatment on the magnesium alloy substrate after the mechanical processing" and "forming a porous oxide layer on the magnesium alloy substrate and forming a sealing layer on the porous oxide layer", so that the drilled surface of the magnesium alloy appearance part has a corrosion-resistant effect and can maintain a certain glossiness for a long time.

[0018] In order to further understand the features and technical contents of the present invention, please refer to the following detailed description and drawings of the present invention. However, the drawings provided are only for reference and description and are not intended to limit the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The figure is a flow chart of a method for processing a magnesium alloy appearance part according to an embodiment of the present invention.

[0020] Figure 2 Another flow chart of the method for processing a magnesium alloy appearance part according to an embodiment of the present invention.

[0021] Figure 3 Schematic diagram of the structure of a magnesium alloy appearance part according to an embodiment of the present invention.

[0022] Figure 4 for Figure 3 A partial enlarged view of part IV of the embodiment of the present invention shows that the magnesium alloy appearance part of the embodiment of the present invention does not have any dye.

[0023] Figure 5 for Figure 4 , which shows that the magnesium alloy appearance part of the embodiment of the present invention is coated with dye. DETAILED DESCRIPTION

[0024] The following is an explanation of the implementation method of the "processing method of magnesium alloy appearance parts" disclosed in the present invention through specific embodiments. Those skilled in the art can understand the advantages and effects of the present invention from the contents disclosed in this specification. The present invention can be implemented or applied through other different specific embodiments, and the details in this specification can also be modified and changed in various ways based on different viewpoints and applications without departing from the concept of the present invention. In addition, the drawings of the present invention are only simple schematic illustrations and are not depicted according to actual dimensions. It is stated in advance. The following embodiments will further explain the relevant technical contents of the present invention in detail, but the disclosed contents are not intended to limit the scope of protection of the present invention. In addition, the term "or" used in this article may include any one or more combinations of the associated listed items depending on the actual situation.

[0025] Unless otherwise defined, the terms used herein have the same meanings as those generally understood by those skilled in the art. The materials involved in each embodiment are commercially available or prepared according to the prior art unless otherwise specified. The process methods involved in each embodiment are the process methods commonly used in the art unless otherwise specified.

[0026] It should be understood that although the steps in the method flow chart are described in a specific order in this article, this does not require or imply that the steps must be performed in this specific order, or that all steps must be performed to achieve the desired result. Optionally, multiple steps can be combined into one step for execution, or one step can be decomposed into multiple steps for execution.

[0027] See also Figure 1 As shown, the present invention provides a method for processing a magnesium alloy appearance part, which includes at least the following main steps: step S100, providing a magnesium alloy substrate; step S102, performing mechanical processing; step S104, performing antioxidant treatment; step S106, performing electrolytic treatment; and step S108, performing electric sealing treatment.

[0028] See also Figure 1 And cooperate Figure 3 As shown, each step of the method for processing the magnesium alloy appearance part of the present invention will be described in detail later.

[0029] First, in step S100, the magnesium alloy substrate 1 provided may be a metal containing magnesium or a combination thereof, such as a magnesium alloy and a magnesium-aluminum alloy. In order to make the magnesium alloy appearance part into a desired appearance (for example, a housing, a shield, and a back plate of an electronic device, etc.), the magnesium alloy substrate 1 may be first formed into a rough shape required for practical application by extrusion, die casting, forging, or cutting. However, the present invention is not limited to the above examples.

[0030] In step S102, the magnesium alloy substrate 1 is mechanically processed in order to form a drilled surface 11 on the magnesium alloy substrate 1, so that the drilled surface 11 can present a metallic texture (glossiness greater than 250GU). The drilled surface 11 can be formed by using a diamond tool to process the surface of the magnesium alloy substrate 1 under high speed and low feed conditions, but it is not limited to this. In the present embodiment, the magnesium alloy substrate 1 is die-cast and sprayed for surface treatment, and then the drilled surface 11 is formed by drilling. In some other embodiments, the mechanical processing can also be computer numerical control (CNC) cutting. Alternatively, in order to obtain a special surface effect, the magnesium alloy substrate 1 can also be polished, sandblasted, or a combination of the two. However, the present invention is not limited to the above examples.

[0031] Generally speaking, metal cutting oil is applied to metal parts during mechanical processing, which has the effects of cooling, lubricating and improving the processing precision. Metal cutting oil can be divided into oily cutting oil, water-based cutting oil and synthetic cutting oil. Among them, water-based cutting oil is an emulsion obtained by diluting concentrated mineral oil with water in proportion, while synthetic cutting fluid is a mixture of polymers, organic matter, inorganic matter and water. Since magnesium alloys have the characteristic of being easily oxidized, whether it is in contact with air or aqueous solution, it is possible that an oxide film will form on the surface of the magnesium alloy, resulting in a decrease in the glossiness of its surface. Therefore, in step S102, mechanical processing includes applying cutting oil to the magnesium alloy substrate 1, which does not contain water. That is, in order to maintain the high gloss of the drilled surface 11, the processing method of the magnesium alloy appearance part of the present invention uses 100% crude oil (such as mineral oil), which can have a higher anti-oxidation effect than water-containing water-based cutting oil and synthetic cutting oil.

[0032] In step S104, the anti-oxidation treatment is to immerse the magnesium alloy substrate 1 after mechanical processing in an alkaline anti-oxidation solution to reduce the risk of oxidation by reducing the contact between the drilled surface 11 of the magnesium alloy substrate 1 and the air. Specifically, the alkaline anti-oxidation solution may contain 1wt% to 50wt% of sodium hydroxide or potassium hydroxide. Preferably, the alkaline anti-oxidation solution may be a 5wt% sodium hydroxide aqueous solution or a potassium hydroxide aqueous solution.

[0033] In step S106, the electrolytic treatment of the magnesium alloy substrate 1 after the antioxidant treatment is carried out in an electrolytic cell (not shown) to form a porous oxide layer 2 on the magnesium alloy substrate 1. In the present embodiment, the electrolytic treatment is an anodic oxidation treatment, and during the treatment process, the magnesium alloy substrate 1 is used as an anode and electrically connected to the positive electrode of the high-voltage power supply, and the cathode of the electrolytic cell (e.g., a stainless steel electrode) is electrically connected to the negative electrode of the high-voltage power supply. The conditions of the electrolytic treatment may include an operating voltage of 40V to 80V, a temperature of 25°C to 40°C, and a treatment time of 20 minutes to 60 minutes. The electrolyte may contain 5wt% to 15wt% of potassium hydroxide. However, the present invention is not limited to the above examples.

[0034] In some other embodiments, the electrolytic treatment may be a pulse current anodizing treatment, so that the porous oxide layer 2 may have a relatively flat surface, and the surface of the magnesium alloy substrate may maintain high gloss and uniform appearance. Further, the conditions of the pulse current anodizing treatment include: the pulse voltage of the pulse current anodizing treatment is preferably 60V, the temperature is 30±5°C (i.e., 25°C to 35°C, preferably 30°C), the treatment time is 40 minutes (may be 20 minutes to 60 minutes), the duty cycle is 40% to 90%, and the frequency is 5,000Hz to 100,000Hz.

[0035] In an embodiment of the present invention, in the pulse current anodizing treatment, the pulse voltage may be 40V, 45V, 50V, 55V or 60V; the pulse frequency may be 5,000Hz, 5,500Hz, 6,000Hz, 6,500Hz, 7,000Hz, 7,500Hz, 8,000Hz, 8,500Hz, 9,000Hz, 9,500Hz or 100,000Hz; the duty cycle may be 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85% or 90%.

[0036] Also, see Figure 2 And cooperate Figure 3 As shown, the processing method of the magnesium alloy appearance part of the present invention further includes step S105, pretreatment; that is, pretreatment of the magnesium alloy substrate 1 before electrolysis treatment to remove dirt, impurities, natural oxide film, etc. on the surface of the magnesium alloy substrate 1. The means of pretreatment vary with different purposes and may include alkaline degreasing, decarburization, and hot alkaline washing or any combination thereof. It is worth noting that in the processing steps of the processing method of the magnesium alloy appearance part of the present invention, the use of a treatment method requiring an acidic solution is avoided, so the pretreatment does not include acid degreasing or pickling.

[0037] See also Figure 1 And cooperate Figure 3 and Figure 4 As shown, in step S108, the electro-deposition coating treatment is to cover the surface of the porous oxide layer 2 with a sealing layer 3 to seal the pores 21 of the porous oxide layer 2, wherein a portion of the sealing layer 3 will be filled in the pores 21. The solid content of the resin composition used for electro-sealing is between 5wt% and 20wt% to meet the requirements of gloss, hardness, corrosion resistance, etc. The conditions for the electro-sealing treatment include: an operating voltage of 10V to 100V, a temperature of 25°C to 35°C, and a treatment time of 1 minute to 5 minutes. The resin composition may include an epoxy resin or an acrylic resin. Moreover, the formed coating can be hardened by baking to form a sealing layer 3, and the baking conditions include: a baking temperature of 120°C to 160°C, and a baking time of 30 minutes to 180 minutes. After the sealing layer is formed, a magnesium alloy appearance part is obtained.

[0038] See also Figure 2 And cooperate Figure 5As shown, the processing method of the magnesium alloy appearance part of the present invention further includes step S107, dyeing treatment; that is, dyeing treatment is performed on the magnesium alloy substrate 1 before the electric sealing treatment to change the appearance color effect of the outer surface of the magnesium alloy substrate 1. The dyeing treatment can be performed by immersion dyeing (immersing the magnesium alloy substrate 1 in the alkaline dye 4), so that the alkaline dye 4 is attached to the magnesium alloy substrate and at least partially penetrates into the multiple holes 21 of the porous oxide layer 2. After the immersion dyeing is completed, cleaning can be performed as needed to remove the alkaline dye 4 that is not adsorbed on the magnesium alloy substrate 1.

[0039] In an embodiment of the present invention, the glossiness of the drilled surface 11 of the magnesium alloy appearance part 1 may be 250GU, 275GU, 300GU, 325GU, 350GU, 375GU, 400GU, 410GU, 420GU, 430GU, 440GU or 450GU. After machining, the drilled surface 11 of the magnesium alloy substrate 1 has glossiness, and after the above steps S100 to S108, the drilled surface 11 of the magnesium alloy appearance part still maintains the glossiness.

[0040] The processing method of the magnesium alloy appearance part of the present invention will be further described in the following specific examples, but the specific examples are only used as examples and should not be construed as limiting the embodiments of the present invention.

[0041] Specific example 1

[0042] The die-cast AZ91D magnesium alloy object was CNC drilled under the condition of applying 100% oily cutting oil, and a drilled surface with a glossiness of 420GU was obtained on the magnesium alloy object. The magnesium alloy object was transferred and immersed in a 5wt% sodium hydroxide aqueous solution, and then the magnesium alloy object was cleaned (first alkaline degreasing at 50°C for 1 minute, then decarbonizing at room temperature for 2 minutes, and hot alkaline washing at 70°C for 2 minutes). After cleaning, the magnesium alloy object was immersed in an electrolyte containing 5wt% potassium hydroxide. A pulse anodizing treatment was performed with the magnesium alloy object as the anode and the carbon plate or stainless steel plate as the cathode: the pulse voltage was 40V, the frequency was 9,000Hz, the duty cycle was 90%, and the treatment time was 20 minutes. The magnesium alloy object was then dried at 100°C for 15 minutes. With the magnesium alloy object as the cathode and the stainless steel as the anode, a resin composition containing a cationic epoxy resin (solid content of 10%) was used for electric sealing under the following conditions: the operating voltage was 60V and the duration was 1 minute. Then, the coating was hardened by baking at a temperature of 120°C for 3 hours. After completion, the magnesium alloy object can obtain a transparent and high-gloss diamond cut surface with corrosion resistance.

[0043] Specific example 2

[0044] The die-cast magnesium alloy object is CNC drilled under the condition of applying 100% oily cutting oil, and a drilled surface with a glossiness of 450GU is obtained on the magnesium alloy object. The magnesium alloy object is transferred and immersed in a 15wt% potassium hydroxide aqueous solution, and then the magnesium alloy object is cleaned (first alkaline degreasing at 50°C for 1 minute, then decarbonizing at room temperature for 2 minutes, and hot alkaline washing at 70°C for 2 minutes). After cleaning, the magnesium alloy object is immersed in an electrolyte containing 10wt% potassium hydroxide. The magnesium alloy object is configured as an anode and a carbon plate or a stainless steel plate as a cathode, and pulse anodizing treatment is performed under the following conditions: pulse voltage is 60V, frequency is 4500Hz, duty cycle is 95%, and treatment time is 25 minutes. The magnesium alloy object is then immersed in a commercial reactive dye (pH value controlled at 9) for dyeing, and then the magnesium alloy object is used as the cathode and the stainless steel is used as the anode. A resin composition containing a cationic epoxy resin (solid content of 10%) is used for electric sealing under the following conditions: the operating voltage is 65V and the duration is 1 minute. Then, the coating is hardened by baking at a temperature of 120°C for 3 hours. After completion, the magnesium alloy object can obtain a high-gloss diamond cut surface with a corrosion-resistant effect and a blue appearance.

[0045] Specific example 3

[0046] The die-cast AZ91D magnesium alloy object was CNC drilled under the condition of applying 100% oily cutting oil, and a drilled surface with a glossiness of 440GU was obtained on the magnesium alloy object. The magnesium alloy object was transferred and immersed in a 20wt% sodium hydroxide aqueous solution, and then the magnesium alloy object was cleaned (first alkaline degreasing at 50°C for 1 minute, then decarbonizing at room temperature for 2 minutes, and hot alkaline washing at 70°C for 2 minutes). After cleaning, the magnesium alloy object was immersed in an electrolyte containing 12wt% potassium hydroxide. A pulse anodizing treatment was performed with the magnesium alloy object as the anode and the carbon plate or stainless steel plate as the cathode: the pulse voltage was 80V, the frequency was 5,000Hz, the duty cycle was 50%, and the treatment time was 20 minutes. The magnesium alloy object was then dried at 100°C for 15 minutes. With the magnesium alloy object as the anode and the stainless steel as the cathode, the resin composition containing anionic acrylic resin (solid content of 14%) was used for electric sealing under the following conditions: the operating voltage was 20V and the duration was 2 minutes. Then, the coating was hardened by baking at a temperature of 120°C for 3 hours. After completion, the magnesium alloy object can obtain a transparent and high-gloss diamond cut surface with corrosion resistance.

[0047] Specific example 4

[0048] The die-cast AZ91D magnesium alloy object was CNC drilled under the condition of applying 100% oily cutting oil, and a drilled surface with a glossiness of 450GU was obtained on the magnesium alloy object. The magnesium alloy object was transferred and immersed in a 5wt% sodium hydroxide aqueous solution, and then the magnesium alloy object was cleaned (first alkaline degreasing at 50°C for 1 minute, then decarbonizing at room temperature for 2 minutes, and hot alkaline washing at 70°C for 2 minutes). After cleaning, the magnesium alloy object was immersed in an electrolyte containing 20wt% potassium hydroxide. The magnesium alloy object was configured as an anode and a carbon plate or a stainless steel plate as a cathode, and pulse anodizing treatment was performed under the following conditions: a pulse voltage of 40V, a frequency of 8,000Hz, a duty cycle of 80%, and a treatment time of 40 minutes. The anodized magnesium alloy object is then immersed in a commercial reactive dye (pH value controlled at 10) for dyeing, and then the magnesium alloy object is used as the anode and the stainless steel is used as the cathode. A resin composition containing anionic acrylic resin (solid content of 10%) is used to perform electric sealing under the following conditions: the operating voltage is 20V and the duration is 2 minutes. Then, the coating is hardened by baking at a temperature of 120°C for 3 hours. After completion, the magnesium alloy object can obtain a high-gloss diamond cut surface with a corrosion-resistant effect and a yellow-red appearance.

[0049] Salt spray test

[0050] The salt spray test is an artificial accelerated salt spray corrosion test method. In this test, the parameters of MIL-STD-810F are used as the test conditions to test Examples 1 to 4. First, the test object (magnesium alloy appearance parts of Examples 1 to 3) is placed at 35±2℃ for at least 2 hours, and then 5±1wt% salt spray (sedimentation rate 1mL / 80cm 3 / h to 4mL / 80cm 3 / h) so that the object to be tested is surrounded by salt mist. According to the provisions of the test plan, the test is carried out with a test cycle of 24 hours of salt mist spraying / 24 hours of drying / 24 hours of salt mist spraying / 24 hours of drying. The salt spray test is converted to the actual number of days, and a 24-hour salt spray test is approximately equal to 120 days in the coastal environment, or equal to a year (365 days) of natural exposure to the environment. Salt spray test results: Specific Examples 1 to Specific Examples 4 do not have any corrosion in appearance, which proves that the magnesium alloy appearance parts obtained by the processing method of the magnesium alloy appearance parts of the present invention can have a high salt spray resistance (corrosion resistance) effect.

[0051] Advantageous Effects of Embodiments

[0052] One of the beneficial effects of the present invention is that the processing method of the magnesium alloy appearance part provided by the present invention can reduce the chance of the drilled surface of the magnesium alloy substrate contacting the air during the processing through the technical scheme of "performing an anti-oxidation treatment on the magnesium alloy substrate after the mechanical processing" and "forming a porous oxide layer on the magnesium alloy substrate and forming a sealing layer on the porous oxide layer", so that the drilled surface of the magnesium alloy appearance part has the effect of salt spray resistance and can maintain a certain glossiness for a long time.

[0053] Furthermore, the present invention applies a non-aqueous cutting oil to perform machining, which can keep the drilled surface of the magnesium alloy substrate from being easily oxidized.

[0054] Furthermore, the processing method of the magnesium alloy appearance part of the present invention does not use acidic reagents in each step of the processing, so it can effectively reduce the surface of the magnesium alloy appearance part from becoming oxidized, fogged and dull due to the step processing.

[0055] The contents disclosed above are only preferred feasible embodiments of the present invention, and are not intended to limit the protection scope of the claims of the present invention. Therefore, all equivalent technical changes made using the contents of the present invention description and drawings are included in the protection scope of the claims of the present invention.

Claims

1. A method for processing magnesium alloy appearance parts, It is characterized in that The processing method of the magnesium alloy appearance part comprises: Provide magnesium alloy substrate; Mechanically processing the magnesium alloy substrate to form a drilled surface on the magnesium alloy substrate; performing an anti-oxidation treatment on the magnesium alloy substrate after the mechanical processing; performing electrolytic treatment on the magnesium alloy substrate after the anti-oxidation treatment to form a porous oxide layer on the magnesium alloy substrate; and Performing an electric sealing treatment on the magnesium alloy substrate after the electrolysis treatment to form a sealing layer on the porous oxide layer to obtain a magnesium alloy appearance part; Wherein, the drilled surface of the magnesium alloy appearance part has a glossiness between 250GU and 450GU.

2. The method for processing a magnesium alloy appearance part according to claim 1, It is characterized in that The machining includes applying cutting oil to the magnesium alloy substrate, the cutting oil not containing water.

3. The method for processing a magnesium alloy appearance part according to claim 1, It is characterized in that The anti-oxidation treatment includes immersing the magnesium alloy substrate in an alkaline anti-oxidation solution.

4. The method for processing a magnesium alloy appearance part according to claim 3, It is characterized in that The alkaline antioxidant solution contains 1 wt % to 50 wt % of sodium hydroxide or potassium hydroxide.

5. The method for processing a magnesium alloy appearance part according to claim 1, It is characterized in that The electrolyte used in the electrolytic treatment contains 5wt% to 15wt% potassium hydroxide, and the conditions of the electrolytic treatment include: an operating voltage of 40V to 80V, a temperature of 25°C to 40°C, and a treatment time of 20 minutes to 60 minutes.

6. The method for processing a magnesium alloy appearance part according to claim 5, It is characterized in that The electrolytic treatment is an anodic oxidation treatment using a pulse current; wherein the pulse voltage is 40V to 80V, the frequency is 5,000Hz to 100,000Hz, the duty cycle is 40% to 90%, and the treatment time is 20 minutes to 60 minutes.

7. The method for processing a magnesium alloy appearance part according to claim 1, It is characterized in that Before the magnesium alloy substrate after the anti-oxidation treatment is subjected to the electrolytic treatment to form the porous oxide layer on the magnesium alloy substrate, the magnesium alloy substrate is also subjected to pretreatment; wherein the pretreatment includes alkaline degreasing, decarburization, hot alkaline washing or a combination thereof.

8. The method for processing a magnesium alloy appearance part according to claim 1, It is characterized in that Before forming the sealing layer on the porous oxide layer, the method further includes dyeing the magnesium alloy substrate; wherein the dyeing includes filling a plurality of pores of the porous oxide layer with an alkaline reactive dye.

9. The method for processing a magnesium alloy appearance part according to claim 1, It is characterized in that The solid content of the resin composition used in the electric sealing treatment is between 5wt% and 20wt%, and the conditions of the electric sealing treatment include: an operating voltage of 10V to 100V, a temperature of 25°C to 35°C, and a treatment time of 1 minute to 5 minutes.

10. The method for processing a magnesium alloy appearance part according to claim 9, It is characterized in that The resin composition comprises epoxy resin or acrylic resin.