MXene organic solvent dispersion liquid, three-dimensional conductive MXene composite film as well as preparation and application of MXene organic solvent dispersion liquid and three-dimensional conductive MXene composite film
Through the MXene technology of centrifugal expansion in water and dispersing in polar organic solvents, the problem of low dispersion in MXene in organic solvents is solved, and efficient flexible sensor preparation is achieved, which improves conductivity and stability, and is suitable for commercial production. .
Patent Information
- Application Number
- CN202310489327.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-04
- Publication Date
- 2024-11-05
AI Technical Summary
MXene has low dispersion in organic solvents, resulting in a decrease in conductivity and stability of flexible sensors. The existing preparation methods are complex and wasteful of organic solvents, making it difficult to meet commercial needs.
Multiple sheets of MXene expanded in water are separated by multiple centrifugation and added to polar organic solvents to ensure that MXene exists in a single sheet, improves its dispersion in the organic solvent, and is mixed with the thermoplastic polymer , prepare three-dimensional conductive composite films.
It significantly improves the dispersion of MXene in organic solvents, realizes its uniform distribution in polymer matrix, extends the stability of the material, improves the conductivity, sensitivity and service life of the flexible sensor, simplifies the preparation process, and is suitable for Commercial production.
Smart Images

Figure CN118896710A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of composite materials, and specifically relates to a MXene organic solvent dispersion, a three-dimensional conductive MXene composite film, and a preparation method and application thereof. Background Art
[0002] Flexible sensors mainly identify the movement status of the object by detecting the changes in electrical signals caused by strain / pressure stimulation during the movement of the object. In order to meet the performance requirements of flexible sensors, the method of combining conductive materials with polymer matrices is usually adopted. There are currently two major types of combining methods: one is to spray conductive materials on the surface of the polymer, and the other is to fill the conductive materials in the polymer matrix. In the former, the conductive material is in direct contact with the outside world, which may cause the device to be oxidized or contaminated, thereby affecting the service life of the sensor; in the latter, the conductive material is wrapped by the polymer, which can effectively prevent the denaturation of the conductive material. However, since a large amount of organic solvents are usually involved in the processing, the conductive material has poor dispersion in the organic solvent and is prone to agglomeration, which leads to a higher percolation threshold and stress concentration, affecting the sensing performance and mechanical properties of the conductive network.
[0003] As a new type of two-dimensional conductive material, MXene is considered to be an ideal choice for constructing flexible sensors because of its excellent conductivity, high specific surface area, and rich surface functional groups. Currently, the most widely used method for preparing MXene is to selectively etch away the A layer in the ternary layered precursor MAX ceramic phase, and then obtain a single layer of MXene by ultrasound. Limited by the hydrophilicity of MXene, it is difficult for MXene to achieve high dispersibility in organic solvents. It is easy to form agglomerates during blending with non-aqueous polymers, which reduces device performance. Moreover, MXene is prone to oxidation and precipitation in aqueous solutions, which brings problems to the processing of flexible sensors. How to improve the dispersibility of MXene in organic solvents and expand the scope of use of MXene has become an urgent problem to be solved.
[0004] The dispersion of MXene in organic solvents reported in the literature is less than 0.5 mg / mL. Existing preparation methods either add intercalating agents or coupling agents, which may lead to degradation and loss of MXene surface functional groups, affecting its performance; or use solvent exchange methods to transfer materials, which will cause a large amount of organic solvent waste, and the processing method is complicated and difficult to implement. Therefore, there is an urgent need for a simple and effective MXene preparation method to improve the dispersion of MXene in organic solvents, achieve uniform distribution in the polymer matrix, reduce the stability loss caused by oxidation, and thus synergistically improve the conductivity, sensitivity, and service life of flexible sensors. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a method for preparing a MXene organic solvent dispersion, and the obtained MXene organic solvent dispersion has high concentration and good stability, so as to solve the technical problem that the MXene organic solvent dispersion produced by the existing process has low concentration and cannot meet the commercialization needs. At the same time, the dispersion is used to prepare a three-dimensional conductive sensor, and the sensor has good flexibility and excellent sensing performance.
[0006] One of the purposes of the present invention is to provide a method for preparing a MXene organic solvent dispersion, comprising: dispersing MXene in water, performing multiple centrifugal separations, removing a lower precipitate, adding an organic solvent S1 and mixing evenly, and then centrifuging and collecting the liquid to obtain the MXene organic solvent dispersion.
[0007] In the preparation method of the above-mentioned MXene organic solvent dispersion, the MXene is a multi-layer MXene, which can be obtained by a common preparation method, and can be prepared specifically by the following method: lithium fluoride is added to an inorganic acid and stirred evenly, and then Ti3AlC2 is added and stirred to obtain an acidic solution, which is washed and dried to obtain the desired multi-layer MXene powder. Among them, the mass ratio of lithium fluoride, inorganic acid, and Ti3AlC2 is 1: (2-8): (1-2); the inorganic acid is selected from at least one of hydrochloric acid and hydrofluoric acid; the stirring conditions are 30-40°C and 3-24h; the washing conditions are washing with deionized water until the solution pH is 6-7; and the drying is freeze-drying at -50--20°C.
[0008] In the preparation method of the above MXene organic solvent dispersion:
[0009] The mass ratio of the MXene to water is (0.0001-0.01):1, preferably (0.001-0.01):1;
[0010] The centrifugal separation is performed at least twice, preferably 3 to 5 times; after multiple centrifugation processes, the distance between the multi-layer MXene layers increases, and the volume of the MXene expands. When the volume of the MXene expands to more than twice the original volume, the lower precipitate is removed. Preferably, the volume of the MXene expands to 2 to 3 times the volume of the MXene before centrifugation;
[0011] The organic solvent S1 is selected from polar organic solvents, preferably at least one selected from N,N-dimethylformamide, N,N-dimethylacetamide, methanol, ethanol, dimethyl sulfoxide, N-methylpyrrolidone, acetone, and ethylene carbonate.
[0012] The concentration of the obtained MXene organic solvent dispersion in the preparation method of the above MXene organic solvent dispersion is 0.1 to 100 mg / mL, preferably 1 to 20 mg / mL.
[0013] According to an embodiment of the present invention, the method for preparing the MXene organic solvent dispersion may specifically adopt the following steps:
[0014] Step 1: Place multiple layers of MXene in a centrifuge tube, add an appropriate amount of water to mix the two evenly, centrifuge, and retain the lower layer of sediment;
[0015] Step 2: Add water to the lower sediment and mix evenly, repeat step 1 until the volume of the lower sediment is significantly expanded;
[0016] Step 3: Mix the organic solvent and the lower layer of sediment evenly, put them into a centrifuge for centrifugation, and collect the upper black liquid to obtain the MXene organic solvent dispersion.
[0017] A second object of the present invention is to provide a MXene organic solvent dispersion prepared by the above-mentioned preparation method.
[0018] A third object of the present invention is to provide a three-dimensional conductive MXene composite film prepared from a thermoplastic polymer material and the above-mentioned MXene organic solvent dispersion.
[0019] In the three-dimensional conductive MXene composite film, the thermoplastic polymer is selected from at least one of polyurethane, polycaprolactone, polylactic acid, polyvinyl alcohol, polyimide, polymethyl methacrylate, polyamide, and polyacrylonitrile; the weight average molecular weight of the thermoplastic polymer is 2000 to 200000, preferably 5000 to 150000.
[0020] The thickness of the three-dimensional conductive MXene composite film is 0.1 to 3 mm, preferably 0.1 to 1 mm.
[0021] The fourth object of the present invention is to provide a method for preparing the above-mentioned three-dimensional conductive MXene composite film, comprising: dissolving the thermoplastic polymer material in an organic solvent S2, adding the MXene organic solvent dispersion, stirring evenly and pouring into a mold for curing to obtain the three-dimensional conductive MXene composite film.
[0022] In the method for preparing the above three-dimensional conductive MXene composite film:
[0023] The organic solvent S2 is the same as the organic solvent S1;
[0024] The concentration of the thermoplastic polymer material in the organic solvent S2 is 0.1 to 1 g / mL, preferably 0.2 to 0.5 g / mL;
[0025] The mass ratio of the thermoplastic polymer material to MXene is (1-10):1, preferably (3-5):1;
[0026] The curing may adopt the curing equipment and curing conditions commonly used in the art. Preferably, the mold may adopt the mold commonly used in the art, preferably a polytetrafluoroethylene mold. The curing conditions are: curing at 60-180°C for 3-6h, preferably curing at 60-120°C for 3-4h.
[0027] The fifth object of the present invention is to provide the use of the MXene organic solvent dispersion described in the first object of the present invention or the three-dimensional conductive MXene composite film described in the third object of the present invention in sensor materials. The sensor material provided by the present invention can be applied to human motion signal detection, health diagnosis and treatment, and human-computer interface interaction, but is not limited to the above fields, and can also be applied to other sensor material fields.
[0028] The present invention adopts multi-layer MXene centrifugal expansion in water, and increases the interlayer distance of multi-layer MXene by multiple centrifugation, expands the volume, and then removes the supernatant, retains the lower sediment, and adds an organic solvent. After mixing evenly, centrifugation is performed again to ensure that MXene exists in the solution in the form of a single layer, so that the polar organic solvent interacts with the polar groups on the surface of the MXene layer, and increases the dispersibility of MXene in the polar solvent. If there is a small amount of precipitation after centrifugation again, the centrifugation operation is repeated after shaking until no precipitation is generated. The preparation method provided by the present invention enables MXene to be widely used in the blending and modification of various polymers.
[0029] The present invention uses two-dimensional material MXene as a conductive material, a thermoplastic polymer material as a matrix layer, constructs a MXene three-dimensional conductive network in the matrix layer, obtains a three-dimensional conductive composite material based on MXene, and obtains a three-dimensional conductive pressure sensor with this composite material. In the three-dimensional conductive composite material, MXene has excellent conductive properties, and the thermoplastic polymer material has good mechanical properties and film-forming properties. The combination of the two makes the three-dimensional conductive composite material have good and stable pressure sensing performance and excellent wearing comfort, which has great advantages over traditional sensors.
[0030] The method for preparing MXene organic solvent dispersion by volume expansion method of the present invention has a concentration increased by 20 times compared with the MXene dispersion obtained by organic solvent dispersion using the traditional method, thereby achieving high-concentration dispersion of MXene in organic solvent. The high-concentration MXene organic solvent dispersion is then mixed with a thermoplastic polymer material to achieve uniform distribution of MXene in the polymer matrix, avoiding the decrease in device stability caused by MXene oxidation, thereby synergistically improving the conductivity, sensitivity and service life of the flexible sensor. The present invention successfully prepared a pressure sensor based on MXene composite materials using a simple operation method, and realized the sensor signal detection under different pressure conditions, providing a reliable solution for preparing a flexible pressure sensor with excellent sensing performance and good stability.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] 1. The preparation method provided by the present invention does not require the addition of additional additives. The dispersibility of MXene in various organic solvents can be significantly improved (up to 20 mg / mL) by simply changing the processing parameters, which can effectively solve the problem of dispersion in polymer substrates and broaden the application scope of MXene in the field of flexible sensors.
[0033] 2. The flexible sensor prepared by simple blending has good stability and fast responsiveness, and shows great application prospects in the fields of electronic skin, motion detection, human-computer interaction, and intelligent diagnosis and treatment;
[0034] 3. The preparation method provided by the present invention effectively solves the problem of easy oxidation of MXene materials. The prepared MXene solution can be stored for 180 days to maintain stable dispersion without being easily oxidized and precipitated, providing the possibility for long-term storage of MXene materials;
[0035] 4. The present invention is simple to prepare and has good repeatability, avoiding the loss of materials that may be caused by a complex synthesis process, effectively reducing the amount of organic solvents used in the preparation process, and does not require expensive equipment, providing ideas for the large-scale preparation of MXene materials;
[0036] 5. In the preparation method provided by the present invention, there are many types of organic solvents and thermoplastic polymers to choose from, the method is simple, low-cost, high-yield, and suitable for commercial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 is a photograph of the MXene-DMF dispersion prepared in Example 1;
[0038] Figure 2 This is a photo of the MXene-DMAc dispersion prepared in Example 2;
[0039] Figure 3 This is a photograph of the MXene-CH3OH dispersion prepared in Example 3;
[0040] Figure 4 This is a photograph of the MXene-C2H5OH dispersion prepared in Example 4;
[0041] Figure 5 is a photograph of the MXene-DMSO dispersion prepared in Example 5;
[0042] Figure 6 is a photograph of the MXene-NMP dispersion prepared in Example 6;
[0043] Figure 7 The pressure sensing signal response of the conductive MXene thin film sensor obtained in Example 8, the abscissa is time, the ordinate is the current signal response value, and the peak height scale is 5000;
[0044] Figure 8 The pressure sensing signal response of the conductive MXene film sensor obtained in Comparative Example 1, the abscissa is time, the ordinate is the current signal response value, and the peak height scale is 1000;
[0045] Fig. 9 This is a transmission electron microscope photograph of MXene in the MXene-DMF dispersion obtained in Example 1;
[0046] Fig.10 This is a photograph of the MXene-DMF dispersion obtained in Example 1 after storage for 180 days. DETAILED DESCRIPTION
[0047] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.
[0048] The instruments and manufacturers used in the examples are as follows:
[0049] Instrument Name Device Model factory Oil bath pot HWCL-3 Great Wall Science & Technology Co., Ltd. Desktop high speed centrifuge MG-1650M Merrick Instruments (Shanghai) Co., Ltd. Vertical freeze dryer LGJ-12 Beijing Songyuan Huaxing Technology Development Co., Ltd. Electronic analytical balance ME204 Mettler-Toledo Instruments (Shanghai) Co., Ltd. Oven DHG-9035A Shanghai-Heng Scientific Instrument Co., Ltd. Electrochemical workstation CHI660 Shanghai Chenhua Instrument Co., Ltd. Tensile testing machine ESM303 Mark-10 Transmission electron microscopy HT7700 HITACHI
[0050] The compounds and sources used in the examples are as follows:
[0051] Preparation of multi-layer MXene
[0052] Take 5ml water and 15ml hydrochloric acid and add them to a polytetrafluoroethylene beaker, shake the beaker gently, add 1g LiF and shake the beaker gently, slowly add 1g Ti3AlC2 within 10min, and stir in an oil bath at 35℃ for 24h. After etching, pour the solution into two centrifuge tubes so that the mass difference between the two tubes is less than 0.1g. Put the two tubes into a centrifuge, start the centrifuge at 3500rpm / min, wash the MXene until the pH is greater than 6, collect the bottom precipitate and freeze-dry it at -60℃ for later use.
[0053] Other raw materials are from the following sources:
[0054] Reagent name Purity and specifications factory <![CDATA[Ti3AlC2]]> AR Jilin Yiyi Technology Co., Ltd. hydrochloric acid AR Beijing Chemical Plant Lithium fluoride AR AlfaAesar N,N-Dimethylformamide AR Shanghai MacLean Biochemical Technology Co., Ltd. N,N-Dimethylacetamide AR Shanghai MacLean Biochemical Technology Co., Ltd. Methanol AR Fuchen (Tianjin) Chemical Reagent Co., Ltd. Ethanol AR Fuchen (Tianjin) Chemical Reagent Co., Ltd. Dimethyl sulfoxide AR Shanghai MacLean Biochemical Technology Co., Ltd. N-Methylpyrrolidone AR Shanghai MacLean Biochemical Technology Co., Ltd. Thermoplastic polyurethane 1185A BASF, Germany Polycaprolactone <![CDATA[M w =80000]]> Shanghai Xiensi Biochemical Technology Co., Ltd. Polylactic acid <![CDATA[M w =110000]]> Shanghai MacLean Biochemical Technology Co., Ltd. Polyvinyl alcohol Alcoholysis degree: 98~99% Shanghai Aladdin Biochemical Technology Co., Ltd.
[0055] Example 1 Preparation of MXene-DMF mixed solution
[0056] Take 0.3g of multi-layer MXene and place it in a centrifuge tube. Add 30ml of water to mix the two evenly. Centrifuge and save the lower precipitate. Add water to the lower precipitate and mix it evenly. Repeat the centrifugation process until the volume of the lower precipitate is observed to expand significantly. Remove the upper clear liquid, transfer the lower precipitate to a beaker, add 30ml of N,N-dimethylformamide (DMF), shake the beaker gently to mix the two evenly, pour the mixed solution into a centrifuge tube, centrifuge at 5000rpm / min, centrifuge for 1min, collect the black liquid, and you can get a MXene-DMF mixed solution with a MXene concentration of 10mg / ml.
[0057] Figure 1 This is a MXene-DMF dispersion solution. Due to its high concentration and high uniformity, the solution in the picture appears uniformly black. Figure 1 It can be seen that the MXene material is evenly dispersed in the DMF solvent, achieving high concentration dispersion of MXene in DMF.
[0058] Example 2 Preparation of MXene-DMAc mixed solution
[0059] Take 0.3g of multi-layer MXene and place it in a centrifuge tube. Add 60ml of water to mix the two evenly. Centrifuge and save the lower precipitate. Add water to the lower precipitate and mix it evenly. Repeat the centrifugation process until the volume of the lower precipitate is observed to expand significantly. Remove the upper clear liquid, transfer the lower precipitate to a beaker, add 15ml of N,N-dimethylacetamide (DMAc), shake the beaker gently to mix the two evenly, pour the mixed solution into a centrifuge tube, centrifuge at 5000rpm / min, centrifuge for 1min, collect the black liquid, and you can get a MXene-DMAc mixed solution with a MXene concentration of 20mg / ml.
[0060] Figure 2This is a MXene-DMAc dispersion solution. Due to its high concentration and high uniformity, the solution in the picture appears uniformly black. Figure 2 It can be seen that the MXene material is evenly dispersed in the DMAc solvent, achieving high concentration dispersion of MXene in DMAc.
[0061] Example 3 Preparation of MXene-CH3OH mixed solution:
[0062] Take 0.3g of multi-layer MXene and place it in a centrifuge tube. Add 90ml of water to mix the two evenly. Centrifuge and save the lower precipitate. Add water to the lower precipitate and mix it evenly. Repeat the centrifugation process until the volume of the lower precipitate is observed to expand significantly. Remove the upper clear liquid, transfer the lower precipitate to a beaker, add 20ml of methanol (CH3OH), shake the beaker gently to mix the two evenly, pour the mixed solution into a centrifuge tube, centrifuge at 5000rpm / min, centrifuge for 1min, collect the black liquid, and you can get a MXene-CH3OH mixed solution with a MXene concentration of 15mg / ml.
[0063] Figure 3 This is a MXene-CH3OH dispersed solution. Due to its high concentration and high uniformity, the solution in the picture appears uniformly black. Figure 3 It can be seen that the MXene material is evenly dispersed in the CH3OH solvent, achieving high concentration dispersion of MXene in CH3OH.
[0064] Example 4 Preparation of MXene-C2H5OH mixed solution
[0065] Take 0.3g of multi-layer MXene and place it in a centrifuge tube. Add 120ml of water to mix the two evenly. Centrifuge and save the lower precipitate. Add water to the lower precipitate and mix it evenly. Repeat the centrifugation process until the volume of the lower precipitate is observed to expand significantly. Remove the upper clear liquid, transfer the lower precipitate to a beaker, add 25ml of ethanol (C2H5OH), shake the beaker gently to mix the two evenly, pour the mixed solution into a centrifuge tube, centrifuge at 5000rpm / min, centrifuge for 1min, collect the black liquid, and you can get a MXene-C2H5OH mixed solution with a MXene concentration of 12mg / ml.
[0066] Figure 4 This is a MXene-C2H5OH dispersion solution. Due to its high concentration and high uniformity, the solution in the picture appears uniformly black. Figure 4 It can be seen that the MXene material is uniformly dispersed in the C2H5OH solvent, achieving high concentration dispersion of MXene in C2H5OH.
[0067] Example 5 Preparation of MXene-DMSO mixed solution
[0068] Take 0.3g of multi-layer MXene and place it in a centrifuge tube. Add 150ml of water to mix the two evenly. Centrifuge and save the lower precipitate. Add water to the lower precipitate and mix it evenly. Repeat the centrifugation process until the volume of the lower precipitate is observed to expand significantly. Remove the upper clear liquid, transfer the lower precipitate to a beaker, add 50ml of dimethyl sulfoxide (DMSO), shake the beaker gently to mix the two evenly, pour the mixed solution into a centrifuge tube, centrifuge at 5000rpm / min, centrifuge for 1min, collect the black liquid, and you can get a MXene-DMSO mixed solution with a MXene concentration of 6mg / ml.
[0069] Figure 5 This is a MXene-DMSO dispersion solution. Due to its high concentration and high uniformity, the solution in the picture appears uniformly black. Figure 5 It can be seen that the MXene material is evenly dispersed in the DMSO solvent, achieving high concentration dispersion of MXene in DMSO.
[0070] Example 6 Preparation of MXene-NMP mixed solution
[0071] Take 0.3g of multi-layer MXene and place it in a centrifuge tube. Add 200ml of water to mix the two evenly. Centrifuge and save the lower precipitate. Add water to the lower precipitate and mix it evenly. Repeat the centrifugation process until the volume of the lower precipitate is observed to expand significantly. Remove the upper clear liquid, transfer the lower precipitate to a beaker, add 60ml of N-methylpyrrolidone (NMP), shake the beaker gently to mix the two evenly, pour the mixed solution into a centrifuge tube, centrifuge at 5000rpm / min, centrifuge for 1min, collect the black liquid, and you can get a MXene-NMP mixed solution with a MXene concentration of 5mg / ml.
[0072] Figure 6 This is a MXene-NMP dispersion solution. Due to its high concentration and high uniformity, the solution in the picture appears uniformly black. Figure 6 It can be seen that the MXene material is evenly dispersed in the NMP solvent, achieving high concentration dispersion of MXene in NMP.
[0073] Example 7 Preparation of high concentration MXene-DMF mixed solution
[0074] Take 0.3g of multi-layer MXene and place it in a centrifuge tube. Add 30ml of water to mix the two evenly. Centrifuge and save the lower precipitate. Add water to the lower precipitate and mix it evenly. Repeat the centrifugation process until the volume of the lower precipitate is observed to expand significantly. Remove the upper clear liquid, transfer the lower precipitate to a beaker, add 15ml of N,N-dimethylformamide (DMF), shake the beaker gently to mix the two evenly, pour the mixed solution into a centrifuge tube, centrifuge at 5000rpm / min, centrifuge for 1min, collect the black liquid, and you can get a MXene-DMF mixed solution with a MXene concentration of 20mg / ml.
[0075] Example 8 Preparation of three-dimensional conductive MXene-polyurethane film
[0076] Thermoplastic polyurethane BASF-1185A was dissolved in DMF with a polyurethane concentration of 0.2 g / ml. 2 ml of the polyurethane solution was taken in a beaker, and 10 ml of the MXene-DMF mixed solution (Example 1) was slowly added thereto. After stirring at 500 rpm for 3 hours, a uniformly mixed MXene / TPU solution was obtained. The mixed MXene / TPU solution was poured into a polytetrafluoroethylene mold and dried at 110°C for 3 hours to remove the solvent, and a three-dimensional conductive MXene-polyurethane film was obtained with a film thickness of 0.3 mm.
[0077] Example 9 Preparation of three-dimensional conductive MXene-polyurethane film
[0078] Thermoplastic polyurethane BASF-1185A was dissolved in DMAc, the polyurethane concentration was 0.3g / ml, 2ml of the polyurethane solution was taken in a beaker, 7.5ml of the MXene-DMAc mixed solution (Example 2) was slowly added thereto, and after stirring at 500rpm for 3h, a uniformly mixed MXene / TPU solution was obtained. The mixed MXene / TPU solution was poured into a polytetrafluoroethylene mold, dried at 120℃ for 3h to remove the solvent, and a three-dimensional conductive MXene-polyurethane film was obtained with a film thickness of 0.45mm.
[0079] Example 10 Preparation of three-dimensional conductive MXene-polyurethane film
[0080] Thermoplastic polyurethane BASF-1185A was dissolved in DMSO with a polyurethane concentration of 0.35 g / ml. 2 ml of the polyurethane solution was taken in a beaker, and 30 ml of the MXene-DMSO mixed solution (Example 5) was slowly added thereto. After stirring at 500 rpm for 3 hours, a uniformly mixed MXene / TPU solution was obtained. The mixed MXene / TPU solution was poured into a polytetrafluoroethylene mold and dried at 110°C for 3 hours to remove the solvent, obtaining a three-dimensional conductive MXene-polyurethane film with a film thickness of 0.53 mm.
[0081] Example 11 Preparation of three-dimensional conductive MXene-polycaprolactone film
[0082] Dissolve polycaprolactone in DMF with a polycaprolactone concentration of 0.25 g / ml. Take 2 ml of the polycaprolactone solution in a beaker, slowly add 10 ml of the MXene-DMF mixed solution (Example 1), and stir at 500 rpm for 3 hours to obtain a uniformly mixed MXene / PCL solution. Pour the mixed MXene / PCL solution into a polytetrafluoroethylene mold and dry at 110 ° C for 3 hours to remove the solvent to obtain a three-dimensional conductive MXene-polycaprolactone film with a film thickness of 0.38 mm.
[0083] Example 12 Preparation of three-dimensional conductive MXene-polylactic acid film
[0084] Polylactic acid was dissolved in DMF with a concentration of 0.4 g / ml. 2 ml of the polylactic acid solution was taken in a beaker, and 20 ml of the MXene-DMF mixed solution (Example 1) was slowly added thereto. After stirring at 500 rpm for 3 hours, a uniformly mixed MXene / PLA solution was obtained. The mixed MXene / PLA solution was poured into a polytetrafluoroethylene mold and dried at 110 ° C for 3 hours to remove the solvent to obtain a three-dimensional conductive MXene-polylactic acid film with a film thickness of 0.6 mm.
[0085] Example 13 Preparation of three-dimensional conductive MXene-polyvinyl alcohol film
[0086] Dissolve polyvinyl alcohol in DMSO to a concentration of 0.5 g / ml. Take 2 ml of the polyvinyl alcohol solution in a beaker, slowly add 42.5 ml of the MXene-DMSO mixed solution (Example 5), and stir at 500 rpm for 3 hours to obtain a uniformly mixed MXene / PVA solution. Pour the mixed MXene / PVA solution into a polytetrafluoroethylene mold and dry at 110 ° C for 3 hours to remove the solvent to obtain a three-dimensional conductive MXene-polyvinyl alcohol film with a film thickness of 0.75 mm.
[0087] Test example: Three-dimensional conductive MXene composite film sensing performance test
[0088] The composite film piezoresistive sensing performance was tested using a tensile testing machine: the composite film was compressed by the tensile testing machine, and the piezoresistive signal was recorded by an electrochemical workstation.
[0089] The composite films obtained in Examples 8 to 10 were cut into 1.0×1.0 cm rectangular sensors for piezoresistive performance testing. The sensor quickly generates an electrical signal response under pressure, and the response disappears after the pressure is removed. The response signals of the three-dimensional conductive MXene-polyurethane film sensor prepared in Example 8 under different pressures are shown in Figure 2. Figure 7 As shown, as the applied pressure increases, the electrical signal generated by the sensor gradually increases, indicating that the sensor has good sensing performance.
[0090] Comparative Example 1
[0091] 0.3 g of multi-layer MXene was placed in a centrifuge tube, and 30 ml of N,N-dimethylformamide (DMF) was added to mix the two evenly. The centrifuge speed was 5000 rpm / min, and the mixture was centrifuged for 1 min. The black liquid was collected to obtain a MXene-DMF mixed solution with a MXene concentration of 1 mg / ml. The preparation of the three-dimensional conductive MXene composite film was the same as in Example 8. The sensing performance of the sensor was tested as follows: Figure 8 , the sensor response is weak.
[0092] The present invention achieves high-concentration dispersion of MXene materials in a variety of organic solvents. Compared with the MXene dispersion obtained by directly dispersing with organic solvents (Comparative Example 1), the concentration is 20 times higher, which solves the existing technical bottleneck. Moreover, the prepared MXene dispersion remains stably dispersed after 180 days of storage (such as Fig.10 The three-dimensional conductive sensor preparation method provided by the present invention is simple, has good repeatability, and has good sensing performance and a wide detection range, and provides a new method for preparing a three-dimensional conductive MXene sensor with good stability.
Claims
1. A method for preparing a MXene organic solvent dispersion, comprising: MXene is dispersed in water, and after multiple centrifugal separations, the lower precipitate is taken out and added to the organic solvent S1 and mixed evenly, and the liquid is collected by centrifugation to obtain the MXene organic solvent dispersion.
2. The preparation method according to claim 1, characterized in that: The MXene is a multi-layer MXene.
3. The preparation method according to claim 1, characterized in that: The mass ratio of the MXene to water is (0.0001-0.01):1, preferably (0.001-0.01):1; and / or, The centrifugal separation is performed at least 2 times, preferably 3 to 5 times; and / or, The organic solvent S1 is selected from polar organic solvents, preferably at least one selected from N,N-dimethylformamide, N,N-dimethylacetamide, methanol, ethanol, dimethyl sulfoxide, N-methylpyrrolidone, acetone, and ethylene carbonate.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The concentration of the MXene organic solvent dispersion is 0.1 to 100 mg / mL, preferably 1 to 20 mg / mL.
5. A MXene organic solvent dispersion prepared by the preparation method according to any one of claims 1 to 4.
6. A three-dimensional conductive MXene composite film prepared from a thermoplastic polymer material and the MXene organic solvent dispersion according to claim 5.
7. The three-dimensional conductive MXene composite film according to claim 6, characterized in that: The thermoplastic polymer material is selected from at least one of polyurethane, polycaprolactone, polylactic acid, polyvinyl alcohol, polyimide, polymethyl methacrylate, polyamide and polyacrylonitrile; and / or, The weight average molecular weight of the thermoplastic polymer is 2,000 to 200,000, preferably 5,000 to 150,000; and / or, The thickness of the composite film is 0.1 to 3 mm, preferably 0.1 to 1 mm.
8. A method for preparing the three-dimensional conductive MXene composite film according to claim 6 or 7, comprising: The thermoplastic polymer material is dissolved in an organic solvent S2, and the MXene organic solvent dispersion is added. After stirring evenly, the mixture is poured into a mold and solidified to obtain the three-dimensional conductive MXene composite film.
9. The preparation method according to claim 8, characterized in that: The organic solvent S2 is the same as the organic solvent S1; and / or, The concentration of the thermoplastic polymer material in the organic solvent S2 is 0.1 to 1 g / mL, preferably 0.2 to 0.5 g / mL; and / or, The mass ratio of the thermoplastic polymer material to MXene is (1-10):1, preferably (3-5):1; and / or, The mold is a polytetrafluoroethylene mold; and / or, The curing conditions are: curing at 60-180° C. for 3-6 hours, preferably curing at 60-120° C. for 3-4 hours.
10. Use of the MXene organic solvent dispersion according to claim 5 or the three-dimensional conductive MXene composite film according to claim 6 in sensor materials.