Waveguide having light shielding film formed thereon, and method for manufacturing same
By using a curable ink composition on the cutting surface of the waveguide edge side, the light shielding film with a thickness of 2 μm to 10 μm is solved, and the problem of inaccurate coating of the light shielding layer in the prior art is achieved, and efficient light shielding effect and excellent Adhesive properties are suitable for waveguide surfaces of various shapes.
Patent Information
- Application Number
- CN202410857071.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2016-12-14
- Filing Date
- 2017-11-23
- Publication Date
- 2024-11-05
AI Technical Summary
The prior art is difficult to accurately apply a light shielding layer on the narrow cut surface and curved or inclined surface of the waveguide by conventional means, especially in the case where the ink forms a light shielding film, and it is difficult to prevent light leakage and external light from flowing in.
A curable ink composition is used to form a light shielding film with a thickness of 2 μm to 10 μm on the edge side cutting surface of the planar waveguide, and accurately coats it on various shapes by inkjet printing, and achieves high optical density by UV curing. and excellent adhesion.
Light leakage prevention and external light flow at the edge of the waveguide is achieved, providing high optical density and excellent adhesion properties, suitable for waveguide surfaces of various shapes, improving image quality and user experience.
Smart Images

Figure CN118897342A_ABST
Abstract
Description
[0001] This application is a divisional application. The application number of the original application is 2017800601700, the application date is November 23, 2017, and the name of the invention is "Waveguide having a light-shielding film formed thereon and method for manufacturing the same". Technical Field
[0002] This application claims the benefit of priority from Korean Patent Application No. 10-2016-0170797, filed on Dec. 14, 2016, the disclosure of which is incorporated herein by reference in its entirety.
[0003] The present invention relates to a waveguide having a light-shielding film, and more particularly, to a waveguide including a light-shielding layer for suppressing leakage light and inflow of external light. Background Art
[0004] Wearable augmented reality devices represented by augmented reality (AR) glasses require near-eye displays (NEDs) to transmit digital images to the user's eyes. One of the components of NEDs is a planar waveguide. Light entering such a waveguide is transmitted in a direction parallel to the waveguide plane and reflected to a grating or a semi-transparent mirror to reach the user's eyes. At this time, some light propagates to the end of the waveguide and diverges to the edge of the waveguide, causing the following during the operation of the NED: Figure 1 The light leakage phenomenon shown in .
[0005] This light leakage phenomenon should be improved because it reduces user convenience and aesthetics when operating the product. In addition, external light entering from the edge of the waveguide may cause unintended optical interference, which may lead to degradation of image quality.
[0006] Therefore, the light shielding coating on the cut edge of the waveguide can suppress the inflow of external light, thereby suppressing the degradation of the image quality output from the NED. In the past, the waveguide was covered with a plastic shell or had tape attached to its edge to shield light.
[0007] However, in the above method, the thickness of the light shielding layer is as thick as tens of nanometers to several millimeters, and it is difficult to control the width of the light shielding coating layer to be thin and accurate to hundreds of nanometers to several micrometers.
[0008] [Prior art literature]
[0009] [Patent Document]
[0010] (Patent Document 1) KR 10-2012-0076973A Summary of the invention
[0011] Technical issues
[0012] In the case of forming a light shielding film using ink, it is difficult to coat the narrow cut surface of the waveguide by a conventional method such as contact printing, for example, screen printing. In addition, when the cut surface of the waveguide is processed into a curved surface or an inclined surface, it is difficult to accurately coat the light shielding layer by a conventional method. However, the inkjet printing method, which is a non-contact printing method, can accurately print even in a narrow cut area of a curved or inclined surface.
[0013] Therefore, an object of the present invention is to provide a waveguide which prevents light leakage occurring at the edge of the waveguide and external light from flowing into the waveguide by coating a cut surface of the waveguide with black ink to form a light shielding film.
[0014] Technical Solution
[0015] In order to solve the above problems, the present invention provides a waveguide having a light shielding film on a cut surface on an edge side of a planar waveguide, wherein the thickness of the light shielding film is 2 μm to 10 μm, and the optical density (OD) is 0.7 to 1.0 based on a light shielding film with a thickness of 1.0 μm.
[0016] In addition, the present invention provides a method for manufacturing the waveguide, comprising the following steps: a) forming a coating of a light-shielding film with a thickness of 2 μm to 10 μm on a cut surface of an edge side of a planar waveguide using a curable ink composition; and b) curing the pattern of the light-shielding film to form a light-shielding film with an optical density (OD) of 0.7 to 1.0 based on a light-shielding film with a thickness of 1.0 μm.
[0017] The present invention also provides a waveguide module comprising the waveguide.
[0018] Beneficial Effects
[0019] According to the present invention, even if the light shielding film is formed with a thin thickness, due to the excellent optical density and excellent adhesive force of the light shielding film, the light leakage phenomenon occurring at the edge of the waveguide and the inflow of external light into the waveguide can be prevented. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is a schematic diagram showing the purpose of a waveguide and the light leakage phenomenon;
[0021] Figure 2 is a schematic diagram showing the light propagation path along the waveguide of the present invention;
[0022] Figure 3 is a schematic diagram showing a process of forming a light-shielding film of a waveguide of the present invention;
[0023] Figure 4 A to Figure 4 C is a schematic diagram showing a method of forming a waveguide according to the shape of a cut surface of the waveguide of the present invention;
[0024] Figure 5 is a schematic diagram showing a cross section of a waveguide manufactured according to one embodiment of the present invention;
[0025] Figure 6 is a schematic diagram showing a front view of a waveguide fabricated according to one embodiment of the present invention. DETAILED DESCRIPTION
[0026] Hereinafter, the present invention will be described in more detail.
[0027] The present invention provides a waveguide on which a light shielding film is formed on a cut surface on an edge side of a planar waveguide.
[0028] For a planar waveguide, incident light is reflected by the inner wall of the waveguide. At this time, if an appropriate light shielding film is not formed on the cut surface, a problem of light emission (light leakage phenomenon) may occur or unnecessary light may enter from the outside.
[0029] The waveguide of the present invention can block the divergence of internal light and the inflow of external light by forming a light shielding film of a small thickness having excellent optical density (OD) on the cut surface of the edge side of the planar waveguide, such as Figure 2 as shown in .
[0030] The cut surface of the waveguide on which the light-shielding film is formed may be processed into a flat surface, a curved surface, or an inclined surface. In the present invention, light-shielding films of various shapes can be formed by the manufacturing method described below.
[0031] In addition, the light shielding film may be formed on the side and side edges of the cut surface of the waveguide. By forming the light shielding film not only on the side but also on the side edges, it is possible to block the divergence of internal light and block the inflow of external light.
[0032] The light-shielding film contains at least one black ink pigment selected from carbon black, graphite, metal oxides, and organic black pigments.
[0033] Examples of carbon black include: Cisto 5HIISAF-HS, Cisto KH, Cisto 3HHAF-HS, CistoNH, Cisto3M, Cisto 300HAF-LS, Cisto 116HMMAF-HS, Cisto 116MAF, Cisto FMFEF-HS, Cisto SOFEF, Cisto VGPF, Cisto SVHSRF-HS and Cisto SSRF (Donghae Carbon Co., Ltd.); diagram blackII, diagram black N339, diagram blackSH, diagram black H, diagram LH, diagram HA, diagram SF, diagram N550M, diagram M, diagram E, diagram G, diagram R, diagramN760M, diagram LR, #2700, #2600, #2400, #2350, #2300, #2200, #1000, #980, #900, MCF88, #52, #50, #47, #45, #45L, #25, #CF9, #95, #3030, #3050, MA7, MA77, MA8, MA11, MA100, MA40, OIL7B, OIL9B, OIL11B, OIL30B and OIL31B (Mitsubishi Chemical Corporation); PRINTEX-U, PRINTEX-V, PRINTEX-140U, PRINTEX-140V, PRINTEX-95, PRINTEX-85, PRINTEX-75, PRINTEX-55, PRINTEX-45, PRINTEX-300, PRINTEX-35, PRINTEX-25, PRINTEX-200, PRINTEX-40, PRINTEX-30, PRINTEX-3, PRINTEX-A, SPECIAL BLACK-550, SPECIAL BLACK-350, SPECIAL BLACK-250, SPECIAL BLACK-100 and LAMP BLACK-101 (Degussa Co., Ltd.); RAVEN-1100ULTRA, RAVEN-1080ULTRA, RAVEN-1060ULTRA, RAVEN-1040, RAVEN-1035, RAVEN-1020, RAVEN-1000, RAV EN-890H, RAVEN-890, RAVEN-880ULTRA, RAVEN-860ULTRA, RAVEN-850, RAVEN-820, RAVEN-790ULTRA, RAVEN-780ULTRA, RAVEN-760ULTRA, RAVEN-520, RAVEN-500, RAVEN-460, RAVEN-450, RAVEN-430ULTRA, RAVEN-420, RAVEN-410, RAVEN-25 00ULTRA、RAVEN-2000、RAVEN-1500、RAVEN-1255、RAVEN-1250、RAVEN-1200、RAVEN-1190ULTRA、RAVEN-1170(Columbia CarbonCo.), their mixtures, etc. .
[0034] As the organic black pigment, aniline black, lactam black, or perylene black series may be used, but the organic black pigment is not limited thereto.
[0035] The content of the black ink pigment may be 10 wt % to 25 wt % based on the total weight of the light-shielding film. The content of the black ink pigment should satisfy the above range to ensure the dispersion stability and storage stability of the ink and to prepare a light-shielding film having a high optical density per thickness without adversely affecting the UV curing of the film.
[0036] like Figure 3 As shown in , the waveguide of the present invention can suppress light leakage and block the inflow of external light by forming a light shielding film on the cut surface on the edge side of the waveguide.
[0037] For this reason, as described above, the thickness of the light-shielding film may be 2 μm to 10 μm, and more preferably 3 μm to 7 μm. In the prior art of adhering a light-shielding tape or covering with a shell, it is difficult to form such a light-shielding film with a thin thickness. However, in the present invention, by using the manufacturing method of the waveguide described later, even if the light-shielding film is formed with a thin thickness within the above range, light leakage can be suppressed and the inflow of external light can be blocked.
[0038] In addition, the total optical density (OD) of the waveguide of the present invention may be 2.5 or more so as to suppress light leakage and block the inflow of external light. When the optical density satisfies the above range, the shielding performance of the light-shielding film is sufficient. Preferably, the optical density (OD) of the light-shielding film is 0.7 to 1.0 based on a light-shielding film having a thickness of 1.0 μm.
[0039] In particular, based on a light-shielding film having a thickness of 1.0 μm, the optical density (OD) of a light-shielding film having a thickness of 2 μm to 5 μm can be 0.80 to 1.0. Based on a light-shielding film having a thickness of 1.0 μm, the optical density (OD) of a light-shielding film having a thickness of 5 μm to 10 μm can be 0.70 to 0.90. When the optical density (OD) of the light-shielding film satisfies the above range, the shielding performance of the light-shielding film of the present invention is optimized.
[0040] In addition, the light shielding film may have an adhesive force of 4B to 5B to the waveguide. Specifically, according to the ASTM D3359 standard, the adhesive force may be 4B to 5B, providing excellent adhesive performance and coating performance.
[0041] The present invention provides a method for manufacturing a waveguide as described above, comprising the steps of: a) forming a coating of a light-shielding film on a cut surface on an edge side of a planar waveguide using a curable ink composition; and b) curing the pattern of the light-shielding film to form a light-shielding film.
[0042] The curable ink composition is characterized by including a colorant, an epoxy compound, an oxetane compound, a photopolymerization initiator, and a solvent having a boiling point of 190° C. to 280° C.
[0043] The curable ink composition of the present invention may further include at least one selected from the group consisting of a surfactant, an adhesion promoter, a diluent, and a photosensitizer.
[0044] Typically, the curable ink composition contains a free radical polymerizable compound or a cationically polymerizable compound.
[0045] As for the radical polymerizable compound, it is not suitable for curing thin films because it has difficulty in curing due to oxygen and has low adhesion to a glass substrate due to a large amount of curing shrinkage, and is therefore not suitable for forming a light-shielding film. On the other hand, the cationically polymerizable compound is advantageous for curing thin films because the curing shrinkage is low and the influence of oxygen is small.
[0046] The curable ink composition used in the present invention contains an epoxy compound as a cation-curable component. Specifically, the epoxy compound is at least one selected from bisphenol epoxy compounds, novolac epoxy compounds, glycidyl ester epoxy compounds, glycidyl amine epoxy compounds, linear aliphatic epoxy compounds, biphenyl epoxy compounds and alicyclic epoxy compounds, or a mixture of two thereof.
[0047] The alicyclic epoxy compound may refer to a compound containing at least one epoxidized aliphatic ring group.
[0048] In the above-mentioned alicyclic epoxy compound containing an epoxidized alicyclic group, the epoxidized alicyclic group refers to an epoxy group bonded to an alicyclic ring. Examples thereof include functional groups such as 3,4-epoxycyclopentyl, 3,4-epoxycyclohexyl, 3,4-epoxycyclopentylmethyl, 3,4-epoxycyclohexylmethyl, 2-(3,4-epoxycyclopentyl)ethyl, 2-(3,4-epoxycyclohexyl)ethyl, 3-(3,4-epoxycyclopentyl)propyl or 3-(3,4-epoxycyclohexyl)propyl. The hydrogen atoms constituting the alicyclic ring may be optionally substituted by a substituent such as an alkyl. The alicyclic epoxy compound includes the compounds specifically exemplified below, but is not limited thereto.
[0049] For example, dicyclopentadiene dioxide, cyclohexene oxide, 4-vinyl-1,2-epoxy-4-vinylcyclohexene, vinylcyclohexene dioxide, limonene monoxide, limonene dioxide, (3,4-epoxycyclohexyl)methyl-3,4-epoxycyclohexanecarboxylate, 3-vinylcyclohexene oxide, bis(2,3-epoxycyclopentyl)ether, bis(3,4-epoxycyclohexylmethyl)adipate, bis(3,4-epoxy-6-methylcyclohexylmethyl)adipate, (3,4-epoxycyclohexyl)methanol, (3,4-epoxy-6-methylcyclohexyl)methyl-3,4-epoxy-6-methylcyclohexanecarboxylate, ethylene glycol bis(3,4-epoxycyclohexyl)ether, ethylene glycol diester of 3,4-epoxycyclohexenecarboxylate, (3,4-epoxycyclohexyl)ethyltrimethoxysilane, and Celloxide can be used. 8000 (manufactured by Daicel Corporation).
[0050] The content of the epoxy compound is preferably 5 to 40% by weight, more preferably 10 to 30% by weight, based on the total weight of the curable ink composition. If it exceeds 40% by weight, the viscosity of the composition increases. If it is less than 5% by weight, the curing sensitivity deteriorates.
[0051] The curable ink composition contains an oxetane compound as another cationically polymerizable monomer.
[0052] The oxetane compound is a compound having a quaternary cyclic ether group in its molecular structure, and can be used to reduce the viscosity of the cationically curable ink composition (eg, to less than 50 cPs at 25° C.).
[0053] In particular, 3-ethyl-3-hydroxymethyloxetane, 1,4-bis[(3-ethyl-3-oxetane)methoxymethyl]benzene, 3-ethyl-3-(phenoxymethyl)oxetane, di[(3-ethyl-3-oxetane)methyl]ether, 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane, 3-ethyl-3-cyclohexyloxymethyloxetane or phenol novolac oxetane can be exemplified. Examples of oxetane compounds include "Alon oxetane OXT-101", "Alon oxetane OXT-121", "Alon oxetane OXT-211", "Alon oxetane OXT-221", "Alonoxetane OXT-212", etc. They can be used alone or in combination of two or more.
[0054] The content of the oxetane compound is preferably 20 to 70% by weight, more preferably 40 to 60% by weight, based on the total weight of the curable ink composition. If it is greater than 70% by weight, curing sensitivity is low, and if it is less than 20% by weight, viscosity increases and coating properties deteriorate.
[0055] The oxetane compound of the present invention can be used in combination with an oxetane compound having an oxetane ring and an oxetane compound having two oxetane rings. When an oxetane compound having an oxetane ring and an oxetane compound having two oxetane rings are used together, the advantage is that the viscosity and flexibility of the film can be controlled. When two types of oxetane compounds are used together as described above, preferably, the oxetane compound having an oxetane ring: the content ratio of the oxetane compound having two oxetane rings is in the range of 1:16 to 1:3.
[0056] The ink composition of the present invention contains a compound that generates a cationic species or a Bronsted acid by ultraviolet irradiation as a cationic photopolymerization initiator, for example, an iodonium salt or a sulfonium salt, but is not limited thereto.
[0057] The iodonium salt or sulfonium salt causes a curing reaction, wherein monomers with unsaturated double bonds contained in the ink react to form polymers during the UV curing process. Depending on the polymerization efficiency, a photosensitizer may also be used.
[0058] As an example, the photopolymerization initiator may be a - 、AsF6- 、BF6 - 、(C6F5)4B - PF6 - or RfnF 6-n The anionic photopolymerization initiator represented by the invention is not limited thereto.
[0059] The content of the photopolymerization initiator is preferably 0.5 wt % to 10 wt % based on the total weight of the curable ink composition. When the content of the photopolymerization initiator is less than 0.5 wt %, the curing reaction is insufficient. When the content of the photopolymerization initiator is greater than 10 wt %, the photopolymerization initiator is not completely dissolved or the viscosity increases, and thus, the coating performance may be deteriorated.
[0060] The ink composition may contain a solvent having a boiling point of 190° C. to 280° C. in order to increase fluidity by reducing the viscosity of the ink to improve coating properties and prevent a decrease in light shielding density per unit thickness, more preferably 210° C. to 260° C. By using a solvent having a boiling point of 190° C. to 280° C. as described above, drying of the nozzle during inkjet printing and a decrease in the curing rate do not occur, and therefore, there is no problem in curing the coating film.
[0061] In the present invention, one or more selected from alcohols having a boiling point of 190° C. to 280° C., ethylene glycol, and ethylene glycol ether may be used as the solvent.
[0062] The glycol ether having a boiling point of 190° C. to 280° C. may be an alkylene glycol alkyl ether having 1 to 6 carbon atoms in the alkyl glycol portion, more preferably ethylene glycol alkyl ether, diethylene glycol alkyl ether, triethylene glycol alkyl ether, tetraethylene glycol alkyl ether, propylene glycol alkyl ether, dipropylene glycol alkyl ether and ethylene glycol dialkylene ether, most preferably a monoalkyl ether having one alkyl group having 1 to 4 carbon atoms in the alkyl ether portion, or a dialkyl ether having two alkyl groups having 1 to 4 carbon atoms in the alkyl ether portion.
[0063] The content of the solvent is preferably 1 wt % to 40 wt % based on the total weight of the curable ink composition. If the content of the solvent is greater than 40 wt %, curing sensitivity may be deteriorated.
[0064] The curable ink composition contains a colorant.
[0065] The colorant may be used in the form of a pigment dispersion containing one or more pigments, dyes, or a mixture thereof, and is not particularly limited as long as it can express a desired color.
[0066] In one embodiment of the present invention, carbon black, graphite, metal oxides, organic black pigments, etc. may be used as the pigment.
[0067] Examples of carbon black include: Cisto 5HIISAF-HS, Cisto KH, Cisto 3HHAF-HS, CistoNH, Cisto3M, Cisto 300HAF-LS, Cisto 116HMMAF-HS, Cisto 116MAF, Cisto FMFEF-HS, Cisto SOFEF, Cisto VGPF, Cisto SVHSRF-HS, and Cisto SSRF (Donghae Carbon Co., Ltd.); diagram blackII, diagram black N339, diagram blackSH, diagram black H, diagram LH, diagram HA, diagram SF, diagram N550M, diagram M, diagram E, diagram G, diagram R, diagramN760M, diagram LR, #2700, #2600, #2400, #2350, #2300, #2200, #1000, #980, #900, MCF88, #52, #50, #47, #45, #45L, #25, #CF9, #95, #3030, #3050, MA7, MA77, MA8, MA11, MA100, MA40, OIL7B, OIL9B, OIL11B, OIL30B, and OIL31B (Mitsubishi Chemical Corporation); PRINTEX-U, PRINTEX-V, PRINTEX-140U, PRINTEX-140V, PRINTEX-95, PRINTEX-85, PRINTEX-75, PRINTEX-55, PRINTEX-45, PRINTEX-300, PRINTEX-35, PRINTEX-25, PRINTEX-200, PRINTEX-40, PRINTEX-30, PRINTEX-3, PRINTEX-A, SPECIAL BLACK-550, SPECIAL BLACK-350, SPECIAL BLACK-250, SPECIAL BLACK-100, and LAMP BLACK-101 (Degussa Co., Ltd.); RAVEN-1100ULTRA, RAVEN-1080ULTRA, RAVEN-1060ULTRA, RAVEN-1040, RAVEN-1035, RAVEN-1020, RAVEN-1000, RAV EN-890H, RAVEN-890, RAVEN-880ULTRA, RAVEN-860ULTRA, RAVEN-850, RAVEN-820, RAVEN-790ULTRA, RAVEN-780ULTRA, RAVEN-760ULTRA, RAVEN-520, RAVEN-500, RAVEN-460, RAVEN-450, RAVEN-430ULTRA, RAVEN-420, RAVEN-410, RAVEN-25 00ULTRA、RAVEN-2000、RAVEN-1500、RAVEN-1255、RAVEN-1250、RAVEN-1200、RAVEN-1190ULTRA、RAVEN-1170(Columbia CarbonCo.), their mixtures, etc. .
[0068] As the organic black pigment, aniline black, lactam black, or perylene black series may be used, but the organic black pigment is not limited thereto.
[0069] In the present invention, the curable ink composition is cured by ultraviolet irradiation (e.g., 250nm or 450nm), more preferably by ultraviolet irradiation with a long wavelength (e.g., 360nm to 410nm), to achieve a specific level of OD. For this reason, based on the gross weight of the curable ink composition, the content of the colorant can be preferably 5% by weight to 20% by weight, more preferably 3% by weight to 10% by weight. If the content of the colorant is less than 5% by weight, the OD level applicable to light-shielding film can not be obtained. If it exceeds 20% by weight, the excessive colorant can not be dispersed in the ink, thus forming a precipitate, or the ultraviolet irradiation can not penetrate into the film after coating, thus, the film can not be fully cured.
[0070] The curable ink composition contains a surfactant that reduces the surface tension of the ink composition to exhibit a small cone angle.
[0071] As the surfactant, commercially available products can be used, for example, it can be selected from Megafack F-444, F-475, F-478, F-479, F-484, F-550, F-552, F-553, F-555, F-570 and RS-75 from DIC (Dai Nippon Ink & Chemicals), or Surflon S-111, S-112, S-113, S-121, S-131, S-132, S-141 and S-145 from Asahi Glass Co., Ltd., or Fluorad FC-93, FC-95, FC-98, FC-129, FC-135, FC-170C, FC-430 and FC-4430 from Sumitomo 3M Co., Ltd., or Zonyl FS-300, FSN, FSN-100 and FSO, or BYK-306, BYK-310, BYK-320, BYK-330, BYK-331, BYK-333, BYK-342, BYK-350, BYK-354, BYK-355, BYK-356, BYK-3 from BYK 58N, BYK-359, BYK-361N, BYK-381, BYK-370, BYK-371, BYK-378, BYK-388, BYK-392, BYK-394, BYK-399, BYK-3440, BYK-3441, BYKETOL-AQ, BYK-DYNWET 800, BYK-SILCLEAN 3700 and BYK-UV 3570, or Rad2100, Rad 2011, Glide 100, Glide 410, Glide 450, Flow 370 and Flow 425 from TEGO, etc.
[0072] The content of the surfactant is preferably 0.1 wt % to 5.0 wt %, more preferably 0.5 wt % to 3.0 wt %, based on the total weight of the curable ink composition. When the content of the surfactant is less than 0.1 wt %, the effect of reducing the surface tension of the composition is insufficient, resulting in coating failure when the composition is coated on a substrate. When the content exceeds 5.0 wt %, the surfactant is used in excess, causing the problem that the compatibility and defoaming properties of the composition are greatly reduced.
[0073] The curable ink composition may further include a photosensitizer to compensate for the curing performance with respect to long-wavelength active energy rays.
[0074] The photosensitizer may be at least one selected from the following: anthracene compounds, such as anthracene, 9,10-dibutoxyanthracene, 9,10-dimethoxyanthracene, 9,10-diethoxyanthracene and 2-ethyl-9,10-dimethoxyanthracene; benzophenone compounds, such as benzophenone, 4,4-bis(dimethylamino)benzophenone, 4,4-bis(diethylamino)benzophenone, 2,4,6-trimethylaminobenzophenone, methyl o-benzoylbenzoate, 3,3-dimethyl-4-methoxybenzophenone and 3,3,4,4-tetrakis(tert-butylperoxycarbonyl)benzophenone; acetophenone; ketone compounds, such as dimethoxyacetophenone, diethoxyacetophenone, 2-hydroxy-2-methyl-1- phenylpropan-1-one and acetone; perylene; fluorenone compounds such as 9-fluorenone, 2-chloro-9-fluorenone and 2-methyl-9-fluorenone; thioxanthone compounds such as thioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 1-chloro-4-propoxythioxanthone, isopropylthioxanthone (ITX), diisopropylthioxanthone; xanthone compounds such as xanthone and 2-methylxanthone; anthraquinone compounds such as anthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, tert-butylanthraquinone and 2,6-dichloro-9,10-anthraquinone; acridine compounds such as 9-phenylacridine, 1,7-bis(9-acridinyl)heptane, 1,5-bis(9-acridinyl)pentane and 1,3-bis(9-acridinyl)propane alkanes; dicarbonyl compounds such as benzyl, 1,7,7-trimethyl-bicyclo[2,2,1]heptane-2,3-dione and 9,10-phenanthrenequinone; phosphine oxide compounds such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide and bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide; benzoate compounds such as methyl-4-(dimethylamino)benzoate, ethyl-4-(dimethylamino)benzoate and 2-n-butoxyethyl-4-(dimethylamino)benzoate; amino synergists such as 2,5-bis(4-diethylaminobenzylidene)cyclopentanone, 2,6-bis(4-diethylaminobenzylidene)cyclohexanone and 2,6-bis(4-dimethylaminobenzylidene)cyclohexanone. ethylaminobenzylidene)-4-methyl-cyclopentanone; coumarin compounds such as 3,3-carbonylvinyl-7-(diethylamino)coumarin, 3-(2-benzothiazolyl)-7-(diethylamino)coumarin, 3-benzoyl-7-(diethylamino)coumarin, 3-benzoyl-7-methoxy-coumarin and 10,10-carbonylbis[1,1,7,7-tetramethyl-2,3,6,7-tetrahydro-1H,5H,11H-C1]benzopyrano[6,7,8-ij]-quinolizin-11-one; chalcone compounds such as 4-diethylaminochalcone and 4-azidobenzylideneacetophenone; 2-benzoylmethylene; and 3-methyl-b-naphthothiazoline.
[0075] The content of the photosensitizer is preferably 1 to 200 parts by weight, more preferably 10 to 100 parts by weight, based on 100 parts by weight of the photopolymerization initiator. If the amount is less than 1 part by weight, the synergistic effect of curing sensitivity at a desired wavelength cannot be obtained. If the amount is greater than 200 parts by weight, the photosensitizer cannot be dissolved and the bonding strength and crosslinking density of the pattern will decrease.
[0076] The curable ink composition may further comprise an adhesion promoter as an additive.
[0077] The light shielding film adhered to the cut surface of the waveguide repeatedly shrinks and expands according to the use conditions such as temperature and humidity, so that the light shielding film is stressed and may fall off the waveguide. In order to prevent this, at least one silane compound selected from alkoxysilane compounds, epoxysilane compounds, aminophenylsilane compounds, aminosilane compounds, mercaptosilane compounds and vinylsilane compounds can be used as an adhesion promoter.
[0078] Among them, epoxysilane compounds are more preferred as the adhesion promoter of the present invention.
[0079] The content of the adhesion promoter is preferably 0.1 wt % to 15 wt %, more preferably 2 wt % to 10 wt % based on the total weight of the ink composition. If the amount is less than 0.1 wt %, the light shielding film cannot be prevented from peeling off from the cut surface of the waveguide. If the amount is greater than 15 wt %, the viscosity of the ink solution increases and the dispersibility is low.
[0080] The curable ink composition used in the present invention spreads in a short time after coating, exhibiting excellent coating properties, and exhibits excellent adhesive properties through curing. Therefore, when the curable ink composition is used in an inkjet printer, it is preferred to set a UV lamp just behind the inkjet head so that curing can be performed while inkjet printing. The curing dose of the curable ink composition is 1 mJ / cm 2 Up to 10,000mJ / cm 2 , preferably 80 mJ / cm 2 Up to 2,000mJ / cm 2 The curable ink composition is cured by absorbing ultraviolet radiation having a wavelength in the range of 250 nm to 450 nm, preferably 360 nm to 410 nm.
[0081] For example, a curable ink composition having a viscosity of 1 to 20 mPa·s at 25° C. is suitable for the inkjet process. The curable ink composition having the above viscosity range has good jetting properties at the process temperature. The process temperature refers to the temperature heated in order to reduce the viscosity of the curable ink composition. The process temperature may be 10° C. to 100° C., preferably 20° C. to 70° C.
[0082] In addition, when the curable ink composition is evaporated, for example, in a convection oven at 35° C., the remaining mass after 2 hours may be 85% or more, and thus, the curing rate and film characteristics are not deteriorated while the evaporation rate is low.
[0083] In step a), inkjet printing or dispensing process can be used to form a coating of light shielding film on the cut surface of the edge of the planar waveguide. The inkjet printing method can be carried out in a conventional manner. The dispensing process can use a pneumatic or piezoelectric dispensing valve as a micro-dispensing device. Preferably, an inkjet printing method is used.
[0084] The inkjet printing method makes it possible to process curved surfaces ( Figure 4 B) or inclined surface ( Figure 4 C) and flat surfaces ( Figure 4 A) The cut surface on the edge side of the waveguide effectively forms a coating of a light shielding film, such as Figure 4 A to Figure 4 As shown in C.
[0085] The curing in step b) may be UV curing. For UV curing, a light source having a wavelength of 250 nm to 450 nm, more preferably 360 nm to 410 nm, may be used as the light source.
[0086] In addition, the thickness of the light-shielding film manufactured by the above-mentioned manufacturing method may be 2 μm to 10 μm, preferably 3 μm to 7 μm.
[0087] The optical density (OD) of the light-shielding film manufactured by the above manufacturing method may be 0.7 to 1.0 based on a light-shielding film having a thickness of 1.0 μm. The optical density (OD) of the light-shielding film having a thickness of 2 μm to 5 μm may be 0.8 to 1.0 based on a light-shielding film having a thickness of 1.0 μm. The optical density (OD) of the light-shielding film having a thickness of 5 μm to 10 μm may be 0.7 to 0.9 based on a light-shielding film having a thickness of 1.0 μm.
[0088] The light-shielding film manufactured by the above-mentioned manufacturing method may have an adhesive force of 4B to 5B with the waveguide.
[0089] The cut surface of the edge side of the waveguide on which the light shielding film is formed may be processed into a flat surface, a curved surface or an inclined surface. The light shielding film may be formed on the side and side edges of the cut surface of the waveguide.
[0090] The present invention also provides a waveguide module comprising the waveguide.
[0091] The waveguide module is not particularly limited as long as the waveguide of the present invention is used, but it may be used for augmented reality (AR) glasses or the like.
[0092] The present invention will be described in more detail with reference to the following examples, including comparative examples. However, these examples are provided for illustrative purposes only and are not intended to limit the scope of the present invention.
[0093] Example
[0094] [Preparation Example]
[0095] 55 wt % of a carbon black pigment dispersion (BK-5282, manufactured by Tokushiki Co., Ltd., pigment content: 25 wt %), 5 wt % of 3,4-epoxycyclohexylcarboxylate (TTA-21P, manufactured by JIANGSUTETRA NEW MATERIAL TECHNOLOGY CO., LTD.) as an epoxy compound, 15 wt % of 3-ethyl-3-[(2-ethylhexyloxy)methyl]oxetane ( DOX, manufactured by Guarson Chemical Co., Ltd.), 1 wt. % of UVI-6992 (manufactured by Dow Chemical) as a photoinitiator, 1 wt. % of KBM-303 (2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, manufactured by Shin Etsu Silicone) as an adhesion promoter and 23 wt. % of DEGDBE (diethylene glycol dibutyl ether, boiling point: 251° C.) as a solvent are mixed to prepare a composition for forming a light-shielding film.
[0096] [Example 1]
[0097] The composition prepared in the above-mentioned preparation example was applied to the cut surface of the edge of the clean waveguide by inkjet coating so that the thickness after curing was 4 μm. In order to prevent foreign matter from attaching, the coating was cured by irradiating ultraviolet rays under the following conditions within 1 minute to form a coating of a light shielding film. As a UV irradiator, a high-pressure mercury lamp was used and the UV irradiation rate was 1000 mJ / cm 2 of UV dose.
[0098] [Example 2]
[0099] The composition prepared in the above-mentioned preparation example was applied to the cut surface of the edge of the clean waveguide by inkjet coating so that the thickness after curing was 9 μm. In order to prevent foreign matter from attaching, the coating was cured by irradiating ultraviolet rays under the following conditions within 1 minute to form a coating of a light shielding film. As a UV irradiator, a high-pressure mercury lamp was used and the UV irradiation rate was 1000 mJ / cm 2 of UV dose.
[0100] [Comparative Example 1]
[0101] Agfa Jeti KM black ink, which is a commercially available UV curable light shielding ink composition, was applied to the cut surface of the edge of the clean waveguide by roller coating so that the thickness after curing was 80 μm. In order to prevent foreign matter from attaching, the coating was cured by irradiating ultraviolet rays under the following conditions within 1 minute to form a coating of a light shielding film. As a UV irradiator, a high pressure mercury lamp was used and the UV light was irradiated at 1000 mJ / cm 2 of UV dose.
[0102] Experimental example
[0103] <Experimental Example 1> Evaluation of OD of Light Shielding Film
[0104] The OD of the light-shielding films having the same thickness manufactured on the waveguide plane by using the same method as in Examples 1 and 2 and Comparative Example 1 was measured with an optical densitometer of X-rite, and the results are shown in Table 1 below.
[0105] <Experimental Example 2>: Cross Hatch Adhesion force
[0106] According to ASTM D3359, which is a cross-cut test standard, a cross-cut test was conducted on a light shielding film having the same thickness manufactured on a waveguide plane by using the same method as in Example 1 and Example 2 and Comparative Example 1. Specifically, 11 lines were drawn on the specimen at intervals of 1 mm in the transverse and longitudinal directions, respectively, to obtain 100 square grids with a width of 1 mm and a length of 1 mm. Then, CT-24 tape of Nichiban Co., Ltd. was adhered to the cut surface. When the tape was peeled off, the state of the surface separated from the tape was evaluated according to the following criteria. The results are shown in Table 1 below.
[0107] <Evaluation criteria for cross-line adhesion>
[0108] 5B: No regional separation.
[0109] 4B: Less than 5% separation relative to the total area.
[0110] 3B: 5% to 15% separation relative to the total area.
[0111] 2B: 15% to 35% separation relative to the total area.
[0112] 1B: 35% to 65% separation relative to the total area.
[0113] 0B: Most areas are separated.
[0114] [Table 1]
[0115] thickness Optical density / thickness Adhesion Example 1 4μm 0.90 / 1.0μm 5B Example 2 9μm 0.85 / 1.0μm 5B Comparative Example 1 80μm 0.037 / 1.0μm 1B
[0116] According to the results shown in Table 1, the optical density of the light-shielding film based on a thickness of 1.0 μm of Example 1 and Example 2 using the ink composition according to the present invention is as high as 0.90 and 0.70, respectively. Therefore, even if the thickness of the light-shielding layer is 10 μm or less, a light-shielding layer having an overall optical density of more than 3 can be manufactured. On the other hand, in Comparative Example 1 using a conventional ink composition, the optical density of the light-shielding film based on a thickness of 1.0 μm is as low as 0.037. Therefore, in order to obtain an optical density of 3.0, a light-shielding layer with a thickness of 80 μm should be manufactured. In other words, it can be found that by using the methods of Example 1 and Example 2, a light-shielding layer having a high optical density and a thickness of about 1 / 10 of the thickness of Comparative Example 1 can be formed.
[0117] In addition, in the case of the light shielding layers prepared in Examples 1 and 2, an adhesion of 5B was obtained without any heat treatment. On the other hand, the light shielding layer prepared in Comparative Example 1 showed an adhesion of 1B. It can be demonstrated that the light shielding layers prepared in Examples 1 and 2 are superior to conventional materials in terms of adhesion.
Claims
1. A waveguide comprising a light shielding film formed on a cut surface on an edge side of a planar waveguide: in, The thickness of the light shielding film is 2 μm to 10 μm, The light-shielding film has an optical density (OD) of 0.7 to 1.0 based on a light-shielding film having a thickness of 1.0 μm.
2. The waveguide according to claim 1, wherein The light-shielding film contains at least one black ink pigment selected from carbon black, graphite, metal oxides, and organic black pigments.
3. The waveguide according to claim 1, wherein: The black ink pigment is included in an amount of 10 to 25 wt % based on the total weight of the light-shielding film.
4. The waveguide according to claim 1, wherein: The light-shielding film has a thickness of 3 μm to 7 μm.
5. The waveguide according to claim 1, wherein The optical density (OD) of the light-shielding film having a thickness of 2 μm to 5 μm is 0.80 to 1.0 based on the light-shielding film having a thickness of 1.0 μm.
6. The waveguide according to claim 1, wherein The optical density (OD) of the light-shielding film having a thickness of 5 μm to 10 μm is 0.70 to 0.90 based on the light-shielding film having a thickness of 1.0 μm.
7. The waveguide according to claim 1, wherein: The adhesive force of the light shielding film of the waveguide is 4B to 5B.
8. The waveguide according to claim 1, wherein The cut surface of the waveguide on which the light shielding film is formed is a flat surface, a curved surface, or an inclined surface.
9. The waveguide according to claim 1, wherein: The light shielding film is formed on the side surfaces and side edges of the cut surface of the waveguide.
10. A method for manufacturing a waveguide, comprising: a) applying a curable ink composition to a thickness of 2 μm to 10 μm on the cut surface on the edge side of the planar waveguide to form a coating layer of a light shielding film; as well as b) curing the coating to form a light-shielding film having an optical density (OD) of 0.7 to 1.0 based on the light-shielding film having a thickness of 1.0 μm, wherein the thickness of the light-shielding film is 2 μm to 10 μm.
11. The method for manufacturing a waveguide according to claim 10, wherein: The curable ink composition includes a colorant, an epoxy compound, an oxetane compound, a photopolymerization initiator, and a solvent having a boiling point of 190° C. to 280° C.
12. The method for manufacturing a waveguide according to claim 10, wherein: The coating of forming the light shielding film on the cut surface on the edge side of the planar waveguide in step a) is performed by using an inkjet printing or dispensing process.
13. The method for manufacturing a waveguide according to claim 10, wherein: The curing in step b) is UV curing.
14. The method for manufacturing a waveguide according to claim 10, wherein: The light-shielding film has a thickness of 3 μm to 7 μm.
15. The method for manufacturing a waveguide according to claim 10, wherein: The optical density (OD) of the light-shielding film having a thickness of 2 μm to 5 μm is 0.8 to 1.0 based on the light-shielding film having a thickness of 1.0 μm.
16. The method for manufacturing a waveguide according to claim 10, wherein: The optical density (OD) of the light-shielding film having a thickness of 5 μm to 10 μm is 0.7 to 0.9 based on the light-shielding film having a thickness of 1.0 μm.
17. The method for manufacturing a waveguide according to claim 10, wherein: The adhesive force of the light shielding film of the waveguide is 4B to 5B.
18. The method for manufacturing a waveguide according to claim 10, wherein: The cut surface of the waveguide on which the light shielding film is formed is processed into a flat surface, a curved surface, or an inclined surface.
19. The method for manufacturing a waveguide according to claim 10, wherein: The light shielding film is formed on the side surfaces and side edges of the cut surface of the waveguide.
20. A waveguide module comprising the waveguide according to claim 1.