Flame-retardant and fire-resistant optical cable and preparation method thereof

By optimizing the optical cable structure and material combination, a multi-layer protective layer is formed, which solves the problems of complex structure and insufficient flame retardant effect of existing optical cables, and achieves improved light transmittance and fire resistance, making it suitable for fire-prone environments.

CN118897364APending Publication Date: 2024-11-05HENGTONG OPTIC ELECTRIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411249504.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing flame-retardant and fire-resistant optical cables have complex structures, complicated manufacturing processes, limited flame-retardant effects, and large overall thickness, making it difficult to meet the requirements of high light transmittance and fire resistance.

Method used

The structure adopts an outside-in design, including an outer sheath, steel strip, fiberglass yarn, inner sheath, and cable core. The outer sheath and steel strip form the first protective layer, the inner sheath and aluminum strip form the second protective layer, the fiberglass yarn is located in the middle, and the padding layer uses low-smoke halogen-free flame-retardant materials. The optical cable is manufactured through specific materials and processes to form a multi-layer protective structure.

Benefits of technology

It achieves high light transmittance, excellent flame retardancy and fire resistance of optical cables, can maintain communication during fires, meets standard requirements, and is suitable for fire-prone environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118897364A_ABST
    Figure CN118897364A_ABST
Patent Text Reader

Abstract

The invention discloses a flame-retardant fire-resistant optical cable and a preparation method thereof, the optical cable comprises an outer sheath, a steel belt, a glass fiber yarn, an inner sheath, an aluminum belt and a cable core, the cable core comprises a reinforcing member and a plurality of optical units arranged around the periphery of the reinforcing member, and the outer wall of the reinforcing member is coated with a cushion layer. The outer protection layer and the steel belt form the first protection layer, and the first protection layer mainly plays a role in preventing flame temperature from being quickly transferred to the inner protection layer and suppressing smoke; the inner protection layer and the aluminum tape form a second protection layer, and the second protection layer can form a compact heat insulation and oxygen isolation layer after combustion, so that external heat is effectively prevented from permeating into the cable core; the glass fiber yarn is arranged between the first protective layer and the second protective layer, so that the optical cable can be ensured to be qualified in stretching and water seepage, a certain heat insulation effect can be achieved, and the influence on the optical fiber caused by expansion or shrinkage of the glass fiber due to a heat flow effect during combustion is prevented; and the cushion layer is made of a low-smoke halogen-free flame-retardant polyolefin material, so that a good thermal insulation effect on the reinforcer is achieved, and the influence on the optical fiber caused by shrinkage of the reinforcer due to violent temperature change is prevented.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of optical cables, and in particular relates to a flame-retardant and fire-resistant optical cable and a preparation method thereof. Background Art

[0002] Currently available flame-retardant and fire-resistant optical cables generally include a cable core, an inner sheath and an outer sheath arranged from the inside to the outside. Usually, multiple layers of mica tape or other insulation structures are wrapped around the outside of the cable core and the outside of the inner sheath to achieve flame retardant and fire-resistant effects. The optical cable is overall thick, the production process is complicated, and the flame retardant effect still has room for improvement. Summary of the invention

[0003] In order to solve the technical problems existing in the prior art, the object of the present invention is to provide a flame retardant and fire resistant optical cable and a preparation method thereof.

[0004] In order to achieve the above purpose and the above technical effect, the technical solution adopted by the present invention is:

[0005] A flame retardant and fire resistant optical cable comprises an outer sheath, a steel belt, a glass fiber yarn, an inner sheath, an aluminum belt and a cable core which are arranged in sequence from outside to inside. The cable core comprises a reinforcement and a plurality of optical units arranged around the reinforcement. The outer wall of the reinforcement is coated with a cushion layer.

[0006] Furthermore, the cable core also includes a plurality of binding yarns, and the binding yarns are arranged in the gap between two adjacent optical units.

[0007] Furthermore, the cable core is filled with cable paste.

[0008] Furthermore, the optical unit includes a loose tube and a plurality of optical fibers arranged therein, and the loose tube is filled with fiber paste.

[0009] Furthermore, the thickness of the outer protection is 1.6 to 3 mm, the oxygen index is ≧40, and the raw materials for preparing the outer protection include: aluminum hydroxide, magnesium hydroxide and outer protection carrier resin, the outer protection carrier resin is one or a combination of POE and EVA, the weight ratio of aluminum hydroxide to magnesium hydroxide is 2:3 to 3:2, and the weight ratio of the sum of the weights of aluminum hydroxide and magnesium hydroxide to the outer protection carrier resin is 1:1 to 2:3.

[0010] Furthermore, the thickness of the inner protection is 2 to 3.5 mm, the oxygen index is ≧40, and the raw materials for preparing the inner protection include: aluminum hydroxide, magnesium hydroxide, and carrier resin, the carrier resin is one or a combination of POE and EVA, the weight ratio of aluminum hydroxide to magnesium hydroxide is 3:1 to 4:1, and the weight ratio of the sum of the weights of aluminum hydroxide and magnesium hydroxide to the carrier resin is 3:2 to 2:1.

[0011] Furthermore, the thickness of the cushion layer is 2 to 10 mm, the oxygen index is ≧36, and the raw materials for preparing the cushion layer include: aluminum hydroxide, magnesium hydroxide, and resin, wherein the resin is one or a combination of POE and EVA, the weight ratio of aluminum hydroxide to magnesium hydroxide is 5:2 to 3:1, and the weight ratio of the sum of the weights of aluminum hydroxide and magnesium hydroxide to the resin is 1:1 to 2:3.

[0012] Furthermore, the thickness of the steel strip and the aluminum strip is 0.25-0.55 mm respectively.

[0013] Furthermore, the thickness of the glass fiber yarn is 0.2-0.6 mm, and the wrapping pitch is 150-400 mm; and the reinforcement is made of any one of steel wire, FRP, and KFRP.

[0014] The present invention also discloses a method for preparing a flame retardant and fire resistant optical cable, comprising the following steps:

[0015] Step 1: Fiber storage;

[0016] Step 2: Fiber Coloring

[0017] According to the color requirements, the optical fibers are colored respectively to obtain colored optical fibers;

[0018] Step 3: Plastic coating

[0019] A loose tube is squeezed out of the colored optical fiber, and fiber paste is uniformly filled inside the loose tube to obtain an optical unit;

[0020] Step 4: Making the cable core

[0021] Using conventional cabling equipment, the optical unit and the reinforcement member with the cushion layer are tied together by yarn tying to form a cable core;

[0022] Step 5: Wrap a layer of aluminum tape on the outside of the cable core. The overlap width of the aluminum tape must be no less than 50mm. At the same time, evenly apply cable paste on the overlap. Use conventional optical cable sheathing equipment to extrude a layer of inner sheath on the outside of the aluminum tape. The extrusion temperature is 120-170℃.

[0023] Step 6: Wrap a layer of glass fiber yarn around the outside of the inner protection, the pitch of the glass fiber yarn is 150-400mm, and adjust the pay-off tension to 20N; then wrap a layer of steel belt around the outside of the glass fiber yarn 3, the overlap width of the steel belt must be not less than 50mm; then extrude a layer of outer protection around the steel belt, the extrusion temperature is 120-180℃;

[0024] Step 7: Finished product testing

[0025] Check whether the attenuation and other performance of finished optical cables meet the requirements;

[0026] Step 8: Finished product delivery

[0027] Finished optical cables can only be released from the warehouse after passing the inspection.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] The invention discloses a flame-retardant and fire-resistant optical cable and a preparation method thereof. The outer sheath and the steel belt form a first protective layer, which mainly prevents the flame temperature from being quickly transmitted to the inner sheath and suppresses smoke, and is a core structure that enables the optical cable to reach a light transmittance of ≧60%; the inner sheath and the aluminum belt form a second protective layer, which can form a dense heat-insulating and oxygen-insulating layer after combustion, effectively isolating the external heat from penetrating into the cable core; the glass fiber yarn is placed between the first protective layer and the second protective layer, which can ensure that the optical cable is stretched and water-permeable, and can also play a certain role in heat insulation and temperature insulation, and can prevent the glass fiber from expanding due to the heat flow during combustion. The cushion layer is made of low-smoke halogen-free flame-retardant polyolefin material with an oxygen index of ≥36, which has a good thermal insulation effect on the reinforcement and prevents the shrinkage caused by the drastic temperature change of the reinforcement from affecting the optical fiber. The overall structure of the optical cable is simple and reasonable, with excellent flame retardancy, fire resistance and smoke suppression performance. It can replace the existing flame retardant and fire-resistant optical cables, and can reduce losses in the event of a fire. It meets the 90-minute fire condition and 15-minute natural cooling condition in the standard GB / T19666-2015 / IEC60331-25 to maintain communication. The optical fiber attenuation is less than 0.9dB, the transmittance is ≥60% under the conditions of GBT 17651.2-1998, and the bundle A to D tests are met under the conditions of GBT18380.(33-36.)-2008. It is suitable for promotion and use in fire-prone places such as railways, buildings, and transportation. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a structural schematic diagram of the present invention. DETAILED DESCRIPTION

[0031] The present invention is described in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.

[0032] A brief summary of one or more aspects is given below to provide a basic understanding of these aspects. This summary is not an exhaustive overview of all conceived aspects, and is neither intended to identify the key or critical elements of all aspects nor to define the scope of any or all aspects. Its only purpose is to give some concepts of one or more aspects in a simplified form as a prelude to a more detailed description that will be given later.

[0033] like Figure 1As shown, a flame retardant and fire resistant optical cable comprises an outer sheath 1, a steel belt 2, a glass fiber yarn 3, an inner sheath 4, an aluminum belt 5 and a cable core which are sequentially arranged from the outside to the inside, wherein the cable core comprises a reinforcement member 6 located at a central position and a plurality of optical units 7 uniformly distributed around the periphery of the reinforcement member 6, the outer wall of the reinforcement member 6 is coated with a cushion layer 8, the optical unit 7 comprises a loose tube 9 and a plurality of optical fibers arranged therein, the loose tube 9 is filled with fiber paste 10, the cable core further comprises a plurality of binding yarns 11, the binding yarns 11 are used to bind to form a cable core, and the cable core is filled with cable paste 12.

[0034] The outer sheath 1 is made of low-smoke halogen-free flame-retardant polyolefin with a thickness of 1.6 to 3 mm and an oxygen index of ≧40, which can effectively slow down the temperature rise of the cable core and achieve the effect of smoke suppression. The raw materials for preparing the outer sheath 1 include: aluminum hydroxide, magnesium hydroxide and outer sheath carrier resin, which are mixed evenly by a mixer and then extruded and granulated by an extruder, wherein the outer sheath carrier resin is a combination of one or two of POE and EVA, the weight ratio of aluminum hydroxide to magnesium hydroxide is 2:3 to 3:2, and the weight ratio of the sum of the weights of aluminum hydroxide and magnesium hydroxide to the outer sheath carrier resin is 1:1 to 2:3. The steel belt 2 is a single-sided coated steel belt with a thickness of 0.25 to 0.55 mm. The outer sheath 1 and the steel belt 2 constitute the first protective layer, which mainly prevents the flame temperature from being quickly transmitted to the inner sheath 4 and suppresses smoke, and is the core structure that makes the light transmittance of the optical cable reach ≧60%.

[0035] The glass fiber yarn 3 is wrapped around the outer wall of the inner protection 4, with a thickness of 0.2 to 0.6 mm. It is a water-blocking glass fiber yarn with a wrapping pitch of 150 to 400 mm, preferably 200 mm. The glass fiber yarn 3 can meet the attenuation requirements of the optical cable under a certain weight tensile force while also playing a certain role in heat insulation and temperature insulation. Placing the glass fiber yarn 3 outside the inner protection 4 rather than outside the cable core can prevent the glass fiber from expanding or contracting due to the heat flow during combustion and affecting the optical fiber.

[0036] The inner protection 4 is made of low-smoke halogen-free ceramic polyolefin material with a thickness of 2 to 3.5 mm and an oxygen index of ≧40. The ceramic hard shell after burning has a good thermal insulation effect. The raw materials for preparing the inner protection 4 include: aluminum hydroxide, magnesium hydroxide, and carrier resin, which are mixed evenly by a mixer and then extruded and granulated by an extruder. Among them, the carrier resin is one or a combination of POE and EVA, the weight ratio of aluminum hydroxide to magnesium hydroxide is 3:1 to 4:1, and the weight ratio of the sum of the weight of aluminum hydroxide and magnesium hydroxide to the carrier resin is 3:2 to 2:1. The aluminum strip 5 is a single-sided coated aluminum strip with a thickness of 0.25 to 0.55 mm. The inner protection 4 and the aluminum strip 5 constitute the second protective layer. The second protective layer can form a dense heat-insulating and oxygen-insulating layer after combustion, which effectively isolates the external heat from penetrating into the cable core.

[0037] The reinforcement member 6 is made of any one of steel wire, FRP, and KFRP. The cushion layer 8 of the outer wall of the reinforcement member 6 is made of low-smoke halogen-free flame-retardant polyolefin material with a thickness of 2 to 10 mm and an oxygen index of ≧36, which has a good thermal insulation effect on the reinforcement member 6 and prevents the shrinkage caused by the drastic temperature change of the reinforcement member 6 from affecting the optical fiber. The raw materials for preparing the cushion layer 8 include: aluminum hydroxide, magnesium hydroxide, and resin, which are mixed evenly by a mixer and then extruded and granulated by an extruder, wherein the resin is one or a combination of POE and EVA, the weight ratio of aluminum hydroxide to magnesium hydroxide is 5:2 to 3:1, and the weight ratio of the sum of the weight of aluminum hydroxide and magnesium hydroxide to the resin is 1:1 to 2:3.

[0038] The loose tube 9 is made of any one of PBT, PC, PP and TPEE.

[0039] A method for preparing a flame retardant and fire resistant optical cable comprises the following steps:

[0040] Step 1: Fiber storage;

[0041] Step 2: Fiber coloring. According to the color requirements, the optical fibers are colored to obtain colored optical fibers;

[0042] Step 3: Sheathing. Extrude a loose tube 9 outside the colored optical fiber, and evenly fill the inside of the loose tube 9 with fiber paste to obtain an optical unit 7;

[0043] Step 4: Manufacturing the cable core. Using conventional cabling equipment, the optical unit 7 and the reinforcement member 6 with the cushion layer 8 are tied together by tying yarn 11 to form a cable core;

[0044] Step 5: Wrap a layer of aluminum tape 5 on the outside of the cable core. The overlap width of the aluminum tape 5 must be no less than 50 mm. At the same time, evenly apply cable paste 12 on the overlap. Use conventional optical cable sheathing equipment to extrude a layer of inner sheath 4 on the outside of the aluminum tape 5. The extrusion temperature is 120-170°C.

[0045] Step 6: Wrap a layer of glass fiber yarn 3 around the outside of the inner protection 4, the pitch of the glass fiber yarn 3 is 150-400mm, preferably 200mm, and the pay-off tension is adjusted to 20N; then wrap a layer of steel belt 2 around the outside of the glass fiber yarn 3, the overlap width of the steel belt 2 must be not less than 50mm; then extrude a layer of outer protection 1 around the outside of the steel belt 2, and the extrusion temperature is 120-180°C;

[0046] Step 7: Finished product inspection. Check whether the attenuation and other performance of the finished optical cable meet the requirements;

[0047] Step 8: Finished products are shipped out. The finished optical cables can be shipped out only after they have passed the inspection.

[0048] Example 1

[0049] like Figure 1As shown, a flame retardant and fire resistant optical cable comprises an outer sheath 1, a steel belt 2, a glass fiber yarn 3, an inner sheath 4, an aluminum belt 5 and a cable core which are sequentially arranged from the outside to the inside, wherein the cable core comprises a reinforcement member 6 located at a central position and 8 optical units 7 uniformly distributed around the periphery of the reinforcement member 6, the outer wall of the reinforcement member 6 is coated with a cushion layer 8, the optical unit 7 comprises a loose tube 9 and 12 optical fibers arranged therein, the loose tube 9 is filled with fiber paste 10, the loose tube 9 is made of PBT, the cable core further comprises a plurality of binding yarns 11, the binding yarns 11 are used to bind to form a cable core, and the cable core is filled with cable paste 12.

[0050] The outer sheath 1 is made of low-smoke halogen-free flame-retardant polyolefin with a thickness of 3mm and an oxygen index of 41, which can effectively slow down the temperature rise of the cable core and achieve the effect of smoke suppression. The raw materials for preparing the outer sheath 1 include: aluminum hydroxide, magnesium hydroxide and outer sheath carrier resin, which are evenly mixed by a mixer and then extruded and granulated by an extruder. Among them, the outer sheath carrier resin is EVA, the weight ratio of aluminum hydroxide to magnesium hydroxide is 1:1, and the weight ratio of the sum of the weight of aluminum hydroxide and magnesium hydroxide to the outer sheath carrier resin is 4:5. Steel belt 2 is a single-sided coated steel belt with a thickness of 0.25mm. The outer sheath 1 and steel belt 2 constitute the first protective layer, which mainly prevents the flame temperature from quickly transmitting to the inner sheath 4 and suppresses smoke. It is the core structure that makes the light transmittance of the optical cable reach ≧60%.

[0051] The glass fiber yarn 3 is wrapped around the outer wall of the inner protection 4, with a thickness of 0.2mm. It is a water-blocking glass fiber yarn with a wrapping pitch of 200mm. The glass fiber yarn 3 can meet the attenuation requirements of the optical cable under a certain weight tensile force while also playing a certain role in heat insulation and temperature insulation. Placing the glass fiber yarn 3 outside the inner protection 4 instead of outside the cable core can prevent the glass fiber from expanding or contracting due to the heat flow during combustion and affecting the optical fiber.

[0052] The inner sheath 4 is made of low-smoke halogen-free ceramic polyolefin material with a thickness of 2mm and an oxygen index of 40. The ceramic hard shell after burning has a good thermal insulation effect. The raw materials for preparing the inner sheath 4 include: aluminum hydroxide, magnesium hydroxide, and carrier resin, which are mixed evenly by a mixer and then extruded and granulated by an extruder. Among them, the carrier resin is POE, the weight ratio of aluminum hydroxide to magnesium hydroxide is 4:1, and the weight ratio of the sum of the weight of aluminum hydroxide and magnesium hydroxide to the carrier resin is 8:5. The aluminum strip 5 is a single-sided coated aluminum strip with a thickness of 0.25mm. The inner sheath 4 and the aluminum strip 5 constitute the second protective layer. The second protective layer can form a dense heat-insulating and oxygen-insulating layer after combustion, which effectively isolates the external heat from penetrating into the cable core.

[0053] The reinforcement member 6 is made of steel wire. The cushion layer 8 of the outer wall of the reinforcement member 6 is made of low-smoke halogen-free flame-retardant polyolefin material with a thickness of 2.5 mm and an oxygen index of 36, which has a good thermal insulation effect on the reinforcement member 6 and prevents the shrinkage caused by the drastic temperature change of the reinforcement member 6 from affecting the optical fiber. The raw materials for preparing the cushion layer 8 include: aluminum hydroxide, magnesium hydroxide, and resin, which are mixed evenly by a mixer and then extruded and granulated by an extruder, wherein the resin is EVA, the weight ratio of aluminum hydroxide to magnesium hydroxide is 5:2, and the weight ratio of the sum of the weight of aluminum hydroxide and magnesium hydroxide to the resin is 1:1.

[0054] A method for preparing a flame retardant and fire resistant optical cable comprises the following steps:

[0055] Step 1: Fiber storage;

[0056] Step 2: Fiber coloring. According to the color requirements, the optical fibers are colored to obtain colored optical fibers;

[0057] Step 3: Sheathing. Extrude a loose tube 9 outside the colored optical fiber, and evenly fill the inside of the loose tube 9 with fiber paste to obtain an optical unit 7. A total of 8 optical units 7 are manufactured, and there are 8 loose tubes 9 in total. The number of optical fiber cores in each loose tube 9 is 12;

[0058] Step 4: Make the cable core. Use conventional cabling equipment to tie eight optical units 7 and a reinforcing member 6 with a cushion layer 8 through two binding yarns 11 to form a cable core. The eight optical units 7 are evenly distributed around the reinforcing member 6, and the cable core is filled with cable paste 12.

[0059] Step 5: Wrap a layer of aluminum tape 5 on the outside of the cable core. The aluminum tape 5 must meet the overlap width of 55mm, and evenly apply cable paste 12 on the overlap. Use conventional optical cable sheathing equipment to extrude a layer of inner sheath 4 on the outside of the aluminum tape 5. The temperature of each section of the extruder is 120℃ / 125℃ / 130℃ / 135℃ / 140℃ / 145℃ / 150℃ / 160℃.

[0060] Step 6: Wrap a layer of glass fiber yarn 3 around the outside of the inner protection 4, the pitch of the glass fiber yarn 3 is 200mm, and adjust the pay-off tension to 20N; then wrap a layer of steel belt 2 around the outside of the glass fiber yarn 3, and the steel belt 2 needs to meet the overlap width of 55mm; then extrude a layer of outer protection 1 around the outside of the steel belt 2, and the temperature of each zone of the extruder is 130℃ / 135℃ / 140℃ / 145℃ / 150℃ / 155℃ / 160℃ / 170℃;

[0061] Step 7: Finished product inspection. Check whether the attenuation and other performance of the finished optical cable meet the requirements;

[0062] Step 8: Finished products are shipped out. The finished optical cables can be shipped out only after they have passed the inspection.

[0063] Parts or structures not specifically described in the present invention may adopt existing technologies or existing products and will not be described in detail here.

[0064] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A flame retardant and fire resistant optical cable, characterized in that: It comprises an outer protection, a steel belt, a glass fiber yarn, an inner protection, an aluminum belt and a cable core which are arranged in sequence from the outside to the inside. The cable core comprises a reinforcement member and a plurality of optical units arranged around the reinforcement member. The outer wall of the reinforcement member is covered with a cushion layer.

2. A flame retardant and fire resistant optical cable according to claim 1, characterized in that: The cable core also includes a plurality of binding yarns, which are arranged in the gap between two adjacent optical units.

3. The flame-retardant and fire-resistant optical cable according to claim 1, characterized in that: The cable core is filled with cable paste.

4. The flame-retardant and fire-resistant optical cable according to claim 1, characterized in that: The optical unit comprises a loose tube and a plurality of optical fibers arranged therein, and the loose tube is filled with fiber paste.

5. The flame-retardant and fire-resistant optical cable according to claim 1, characterized in that: The thickness of the outer protection is 1.6 to 3 mm, and the oxygen index is ≧40. The raw materials for preparing the outer protection include: aluminum hydroxide, magnesium hydroxide and outer protection carrier resin. The outer protection carrier resin is one or a combination of POE and EVA. The weight ratio of aluminum hydroxide to magnesium hydroxide is 2:3 to 3:2, and the weight ratio of the sum of the weights of aluminum hydroxide and magnesium hydroxide to the outer protection carrier resin is 1:1 to 2:

3.

6. The flame-retardant and fire-resistant optical cable according to claim 1, characterized in that: The thickness of the inner protection is 2 to 3.5 mm, and the oxygen index is ≧40. The raw materials for preparing the inner protection include: aluminum hydroxide, magnesium hydroxide, and carrier resin. The carrier resin is one or a combination of POE and EVA. The weight ratio of aluminum hydroxide to magnesium hydroxide is 3:1 to 4:1, and the weight ratio of the sum of the weights of aluminum hydroxide and magnesium hydroxide to the carrier resin is 3:2 to 2:

1.

7. The flame-retardant and fire-resistant optical cable according to claim 1, characterized in that: The thickness of the cushion layer is 2 to 10 mm, and the oxygen index is ≧36. The raw materials for preparing the cushion layer include: aluminum hydroxide, magnesium hydroxide, and resin, wherein the resin is one or a combination of POE and EVA, the weight ratio of aluminum hydroxide to magnesium hydroxide is 5:2 to 3:1, and the weight ratio of the sum of the weights of aluminum hydroxide and magnesium hydroxide to the resin is 1:1 to 2:

3.

8. The flame-retardant and fire-resistant optical cable according to claim 1, characterized in that: The thickness of the steel strip and the aluminum strip are respectively 0.25-0.55 mm.

9. The flame-retardant and fire-resistant optical cable according to claim 1, characterized in that: The thickness of the glass fiber yarn is 0.2-0.6 mm, and the wrapping pitch is 150-400 mm; the reinforcement member is made of any one of steel wire, FRP and KFRP.

10. A method for preparing a flame retardant and fire resistant optical cable according to any one of claims 1 to 9, comprising the following steps: Step 1: Fiber storage; Step 2: Fiber Coloring According to the color requirements, the optical fibers are colored respectively to obtain colored optical fibers; Step 3: Plastic coating A loose tube is squeezed out of the colored optical fiber, and fiber paste is uniformly filled inside the loose tube to obtain an optical unit; Step 4: Making the cable core Using conventional cabling equipment, the optical unit and the reinforcement member with the cushion layer are tied together by yarn tying to form a cable core; Step 5: Wrap a layer of aluminum tape on the outside of the cable core. The overlap width of the aluminum tape must be no less than 50mm, and evenly apply cable paste on the overlap; Use conventional optical cable sheathing equipment to extrude a layer of inner sheath on the outside of the aluminum tape, with an extrusion temperature of 120-170°C; Step 6: Wrap a layer of glass fiber yarn around the outside of the inner protection, the pitch of the glass fiber yarn is 150-400mm, and adjust the pay-off tension to 20N; Then, a layer of steel belt is coated on the outside of the glass fiber yarn 3, and the overlap width of the steel belt must be not less than 50 mm; and then a layer of outer protection is extruded on the outside of the steel belt, and the extrusion temperature is 120-180°C; Step 7: Finished product testing Check whether the attenuation and other performance of finished optical cables meet the requirements; Step 8: Finished product delivery Finished optical cables can only be released from the warehouse after passing the inspection.