Method for efficiently preparing glass through hole with high-precision aperture size

Through the method of alternately using acidic and alkaline corrosion liquids, combined with ultrasonic stirring and corrosion treatment at different temperatures, the problem of high error or low rate etching rate in the prior art is solved, and high accuracy is achieved Pore ​​size glass through-hole preparation improves efficiency and reduces costs.

CN118899261APending Publication Date: 2024-11-0558TH RES INST OF CETC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410991238.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In the existing laser-induced modification glass through-hole preparation process, glass through-holes with high etching rate but large errors, or low etching rate and low efficiency, making it difficult to achieve high-precision pore size glass through-holes.

Method used

Using the method of alternately using acid corrosion liquid and alkaline corrosion liquid, the glass through holes are corroded at different temperatures through ultrasonic and stirring. The high etching rate of acid corrosion liquid and the low etching rate of alkaline corrosion liquid are used to control the etching. Time to achieve high precision pore size glass through-hole preparation.

Benefits of technology

Improves the accuracy of glass through-hole apertures, improves processing efficiency, and reduces manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899261A_ABST
    Figure CN118899261A_ABST
Patent Text Reader

Abstract

The invention discloses a method for efficiently preparing a glass through hole with a high-precision aperture size, which comprises the following steps of: immersing a glass wafer modified by laser in an acidic corrosive liquid, adding ultrasonic waves, stirring and circulating for a first time, and corroding a modified area at a first temperature to form the glass through hole; performing ultrasonic cleaning at a second temperature, taking out and drying, and measuring the aperture of the glass through hole to obtain a measured value 1 of the aperture of the glass through hole; the glass wafer is immersed in the alkaline corrosive liquid, ultrasonic treatment is carried out, stirring circulation is carried out for a second time, the glass through hole is corroded at a third temperature, and the diameter size of the glass through hole is increased to a target value; and after ultrasonic cleaning for a second preset time at a second temperature, taking out and drying to complete preparation of the glass through hole. According to the method, the characteristics of high etching rate of the acidic etching liquid and low etching rate of the alkaline etching liquid are utilized, flexible selection is carried out according to needs, and the preparation efficiency is greatly improved on the premise that the high-precision size of the aperture of the glass through hole is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a packaging technology for integrated circuits, and in particular to a method for efficiently preparing a glass through hole with a high-precision aperture size. Background Art

[0002] With the development of semiconductor packaging technology, based on adapter board technology, the packaging technology has been expanded from the planar 2D dimension to the vertical 2.5D / 3D dimension, which greatly improves the system integration, significantly improves space utilization, shortens the interconnection length, and reduces power consumption. It can be widely used in emerging fields such as smart phones, Internet of Things, automotive electronics, high-performance computing, 5G, and artificial intelligence.

[0003] According to the different packaging materials, the adapter board can be divided into three categories, namely organic adapter board, silicon adapter board and glass adapter board. The poor thermal stability of the organic adapter board, the poor CTE matching with the silicon chip and the difficulty of high-density I / O processing restrict the application of high-density integrated packaging of the organic adapter board. The silicon adapter board has been widely used due to its good CTE matching with the silicon chip, excellent thermal conductivity, good compatibility with existing integrated circuit processes and equipment, and extremely high I / O port density. However, since silicon is a semiconductor material with conductivity, it is easy to cause leakage and crosstalk and coupling of the transmission signal under high frequency conditions, which seriously restricts the application of silicon adapter boards. Based on the characteristics of glass materials, the glass adapter board has high resistivity, good insulation performance, good signal isolation, and reduced crosstalk between signals. It has advantages that silicon adapter boards cannot match in the transmission of high-frequency signals.

[0004] Realizing high-quality, high-aspect-ratio glass through holes is one of the key technologies in preparing glass adapter plates. The glass through hole preparation method based on laser-induced modification first uses pulsed laser to induce glass modification, and then uses corrosive liquid to selectively corrode to form through holes. The etching selectivity is high and has certain advantages in practical applications.

[0005] In the existing laser-induced modified glass through-hole preparation process, for example, the invention application of Cai Xingzhou et al. (patent authorization number CN112864026 B) discloses a process for processing TGV through-holes by laser combined with HF wet etching. During the etching process of this process, the etching rate of HF is high, the error is large, and it is difficult to control the aperture size of the glass through-hole by etching time. The aperture precision of the etched glass through-hole is low. The invention application of Yin Chunyan et al. (patent publication number CN 116161870 A) discloses a method for processing high aspect ratio glass through-holes by multi-pulse picosecond laser assisted KOH wet etching. During the etching process of this method, high-precision glass through-holes can be obtained, but the etching rate of KOH etching solution is low, the etching time is long, and the efficiency is low. The invention application of Xue Cheng et al. (patent publication number CN116177897 A) discloses a method for preparing glass wafer through-holes by acid-base alternating etching. During the etching process of this method, acid-base alternation cycles are required for multiple times, which affects the processing efficiency.

[0006] Therefore, a method for efficiently preparing glass through holes with high-precision aperture size is developed. Summary of the invention

[0007] The purpose of the present invention is to provide a method for efficiently preparing a glass through hole with a high-precision aperture size.

[0008] The technical solution to achieve the purpose of the present invention is: a method for efficiently preparing a glass through hole with a high-precision aperture size, comprising: Step 1, immersing the laser-modified glass wafer in an acidic etching solution, adding ultrasound and stirring for a first time, and etching the modified area at a first temperature to form a glass through hole; Step 2, ultrasonically cleaning at a second temperature, taking out and drying, measuring the aperture of the through-glass hole, and obtaining a through-glass hole aperture measurement value 1; Step 3, immersing the glass wafer in an alkaline etching solution, adding ultrasound and stirring for a second time, etching the through-glass hole at a third temperature, so that the diameter of the through-glass hole increases to a target value; Step 4: After ultrasonic cleaning at a second temperature for a second preset time, taking out and drying, the through-glass hole preparation is completed.

[0009] Optionally, the glass wafer includes but is not limited to quartz glass, borosilicate glass, high aluminum glass, alkali-free borosilicate glass, soda-lime glass, photosensitive microcrystalline glass, etc.

[0010] Optionally, the acidic corrosive liquid includes but is not limited to hydrofluoric acid, a mixture of hydrofluoric acid and fluoride, and the fluoride includes ammonium fluoride, sodium fluoride, potassium fluoride, etc.; The first time is calculated based on the average etching rate of the acidic etching solution and the target aperture value of the through-glass hole, that is, the target aperture value of the through-glass hole×95%÷the average etching rate of the acidic etching solution.

[0011] The average etching rate of the acidic etching solution is an average value of at least 3 acidic etching rates measured experimentally. The acidic etching rate is measured under the same etching conditions by measuring the thickness reduction of the glass before and after etching in the acidic etching solution and dividing the result by the etching time.

[0012] Optionally, the alkaline corrosive solution includes but is not limited to potassium hydroxide, sodium hydroxide, tetramethylammonium hydroxide, calcium hydroxide, etc.; The second time is calculated based on the etching rate of the alkaline etching solution and the target aperture value of the through-glass hole, that is, (target aperture value of the through-glass hole-measured aperture value of the through-glass hole 1)÷average etching rate of the alkaline etching solution.

[0013] The average etching rate of the alkaline etching solution is an average value based on at least 3 experimental measurements of the alkaline etching rate. The alkaline etching rate is measured under the same etching conditions by measuring the thickness reduction of the glass before and after etching in the alkaline etching solution and dividing the result by the etching time.

[0014] Optionally, the first temperature is 20°C~30°C, the second temperature is 10°C~30°C, and the third temperature is 65°C~95°C.

[0015] Compared with the prior art, the present invention has the significant advantage that by adopting such an etching method, the high etching rate of the acidic etching solution and the low etching rate of the alkaline etching solution can be utilized as much as possible, effectively improving the aperture accuracy of the glass through hole and improving the processing efficiency, thereby improving performance and reducing manufacturing costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a flow chart of the method for preparing glass through-hole with high efficiency and high precision aperture size of the present invention; Figure 2 is the measurement result of the aperture of the glass through hole after HF solution corrosion in Example 1; Figure 3 is the measurement result of the aperture of the glass through hole after being corroded by KOH solution in Example 1; Figure 4 is the measurement result of the aperture of the glass through hole after HF solution corrosion in Example 2; Figure 5 is the measurement result of the aperture of the glass through hole after being etched by KOH solution in Example 2; Figure 6 The results of measuring the aperture of the glass through hole after HF solution corrosion in Comparative Example 1; Figure 7 This is the measurement result of the aperture of the glass through hole after being corroded by KOH solution in comparative example 2; Figure 8 The results are shown in Table 3. The results are shown in Table 3. The results are shown in Table 3. DETAILED DESCRIPTION

[0017] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0018] Figure 1 The present invention provides a method for efficiently preparing a glass through hole with a high-precision aperture size, and the method comprises the following steps: Step 1, immersing the laser-modified glass wafer in an acidic etching solution, adding ultrasound and stirring for a first time, and etching the modified area at a first temperature to form a glass through hole; Step 2, ultrasonic cleaning at a second temperature, taking out and drying, measuring the aperture of the glass through hole, and obtaining the glass through hole aperture measurement value 1; Step 3, immersing the glass wafer in an alkaline etching solution, adding ultrasound and stirring for a second time, etching the glass through hole at a third temperature, so that the diameter of the glass through hole increases to a target value; Step 4, ultrasonic cleaning at the second temperature for a second preset time, taking out and drying, and completing the preparation of the glass through hole.

[0019] Wherein, the glass wafer includes quartz glass, borosilicate glass, high aluminum glass, alkali-free boron aluminum glass, soda-lime glass, and photosensitive microcrystalline glass; Specifically, the first temperature is 20°C to 30°C, the second temperature is 10°C to 30°C, and the third temperature is 65°C to 95°C; more preferably, the first temperature and the second temperature are both 23°C, and the third temperature is 85°C; in a specific implementation, the first temperature and the second temperature are closer to the laboratory temperature of the dust-free workshop and are easier to control; the third temperature is selected to be increased, and during the heating process, the temperature rises too fast, and there is a risk of boiling the solution; the selected temperature is lowered, and the etching rate is reduced, affecting the processing efficiency; Specifically, the acidic corrosive liquid is hydrofluoric acid, a mixture of hydrofluoric acid and ammonium fluoride, a mixture of hydrofluoric acid and sodium fluoride, or a mixture of hydrofluoric acid and potassium fluoride; Specifically, the average etching rate of the acidic etching solution is obtained by measuring the etching rate of the glass in the acidic etching solution three times and then taking the average value, wherein the average rate of each time is obtained by measuring the thickness reduction of the glass before and after etching in the acidic etching solution under the same etching conditions and dividing the result by the etching time; Specifically, the first time is the target aperture value of the through-glass hole×95%÷the average etching rate of the acidic etching solution; Specifically, the alkaline corrosive solution includes potassium hydroxide, sodium hydroxide, tetramethylammonium hydroxide, and calcium hydroxide; Specifically, the average etching rate of the alkaline etching solution is obtained by measuring the etching rate of the glass in the alkaline etching solution three times and then taking the average value, wherein the average rate of each time is obtained by measuring the thickness reduction of the glass before and after etching in the alkaline etching solution under the same etching conditions and dividing the measured value by the etching time; Specifically, the second time is (target aperture value of the through-glass hole-aperture measurement value after etching with the acidic etching solution)×95%÷average etching rate of the alkaline etching solution.

[0020] The following is a detailed description of a method for efficiently preparing a glass through hole with a high-precision aperture size provided by the present invention in conjunction with embodiments. Example

[0021] The laser-modified quartz glass wafer was immersed in HF solution, ultrasonic and stirred in circulation. The concentration of HF solution was 40%, the etching temperature was 23°C, the average etching rate was 0.6μm / min, and the target aperture value of the etched glass through hole was 28μm. It was calculated that 44.5 minutes were required to etch to 95% of the target aperture, i.e. 26.6μm.

[0022] After etching, the glass was taken out and ultrasonically cleaned in deionized water at a temperature of 23°C. After cleaning, it was dried and the diameter of the glass through-hole was measured. The test value was 27.17 μm.

[0023] Then immerse the glass wafer in KOH solution, add ultrasound and stir and circulate, the concentration of KOH solution is 32%, the etching temperature is 85℃, the average etching rate is 0.02μm / min, and it is calculated that another 42min of etching is required.

[0024] After etching, the glass was taken out and put into deionized water for ultrasonic cleaning at a temperature of 23°C. After cleaning, it was dried and the preparation of the through-glass hole was completed. The test showed that the aperture of the through-glass hole was 28.05 μm. Example

[0025] The laser-modified quartz glass wafer was immersed in HF solution, ultrasonic and stirred in circulation, the HF solution concentration was 40%, the etching temperature was 23°C, the average etching rate was 0.6μm / min, and the target aperture value of the etched glass through hole was 60μm. It was calculated that it would take 95 minutes to etch to 95% of the target aperture, i.e. 57μm.

[0026] After etching, the glass was taken out and ultrasonically cleaned in deionized water at a temperature of 23°C. After cleaning, it was dried and the diameter of the glass through-hole was measured. The test value was 58.49 μm.

[0027] Then immerse the glass wafer in KOH solution, add ultrasound and stir and circulate, the concentration of KOH solution is 32%, the etching temperature is 85℃, the average etching rate is 0.02μm / min, and it is calculated that another 75.5min of etching is required.

[0028] After etching, the glass was taken out and put into deionized water for ultrasonic cleaning at a temperature of 23°C. After cleaning, it was dried and the preparation of the through-glass hole was completed. The test showed that the aperture of the through-glass hole was 60.02 μm. Example

[0029] The acidic etching solution in Example 1 or Example 2 is replaced by a mixture of hydrofluoric acid and ammonium fluoride, a mixture of hydrofluoric acid and sodium fluoride, or a mixture of hydrofluoric acid and potassium fluoride, and the alkaline etching solution is replaced by sodium hydroxide, tetramethylammonium hydroxide, or calcium hydroxide to carry out a through-glass hole preparation experiment.

[0030] Comparative Example 1 The target value of the through-glass hole diameter is the same as that in Example 1. The laser-modified quartz glass wafer is immersed in an HF solution, ultrasonically added and stirred and circulated. The HF solution concentration is 40%, the etching temperature is 23°C, and the average etching rate is 0.6 μm / min. After calculation, the etching time is 47 min.

[0031] After etching, the glass was taken out and put into deionized water for ultrasonic cleaning at a temperature of 23°C. After cleaning, it was dried and the preparation of the through-glass hole was completed. The test showed that the aperture of the through-glass hole was 29.05 μm.

[0032] Comparative Example 2 The target value of the through-glass hole diameter is the same as that in Example 1. The laser-modified quartz glass wafer is immersed in a KOH solution, ultrasonically added and stirred in circulation. The KOH solution concentration is 32%, the etching temperature is 85°C, and the average etching rate is 0.02 μm / min. According to calculation, etching time is 1400 min.

[0033] After etching, the glass was taken out and put into deionized water for ultrasonic cleaning at a temperature of 23°C. After cleaning, it was dried and the preparation of the through-glass hole was completed. The test showed that the aperture of the through-glass hole was 28.03 μm.

[0034] Comparative Example 3 The target value of the through-glass hole diameter is the same as that in Example 2. The laser-modified quartz glass wafer is immersed in an HF solution, ultrasonically added and stirred and circulated. The HF solution concentration is 40%, the etching temperature is 23°C, and the average etching rate is 0.6 μm / min. According to calculation, etching takes 100 min.

[0035] After etching, the glass was taken out and put into deionized water for ultrasonic cleaning at a temperature of 23°C. After cleaning, it was dried and the preparation of the through-glass hole was completed. The test showed that the aperture of the through-glass hole was 64.59 μm.

[0036] Comprehensively comparing the embodiments and comparative examples, the acidic etching solution has a fast etching rate and high efficiency, but a large error. By controlling the etching time, the aperture size accuracy of the glass through hole is still poor. The alkaline etching solution has a slow etching rate. By controlling the etching time, the aperture size accuracy of the glass through hole is good, but the efficiency is low. The present invention utilizes the characteristics of high etching rate of the acidic etching solution and low etching rate of the alkaline etching solution, and flexibly selects them according to needs, thereby greatly improving the preparation efficiency while ensuring the high-precision aperture size of the glass through hole.

[0037] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0038] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.

Claims

1. A method for efficiently preparing glass through holes with high-precision aperture size, It is characterized in that include: Step 1, immersing the laser-modified glass wafer in an acidic etching solution, adding ultrasound and stirring for a first time, and etching the modified area at a first temperature to form a glass through hole; Step 2, ultrasonically cleaning at a second temperature, taking out and drying, measuring the aperture of the through-glass hole, and obtaining a through-glass hole aperture measurement value 1; Step 3, immersing the glass wafer in an alkaline etching solution, adding ultrasound and stirring for a second time, etching the through-glass hole at a third temperature, so that the diameter of the through-glass hole increases to a target value; Step 4: After ultrasonic cleaning at a second temperature for a second preset time, taking out and drying, the through-glass hole preparation is completed.

2. The method for efficiently preparing a through-glass hole with a high-precision aperture size as claimed in claim 1, It is characterized in that The glass wafer includes quartz glass, borosilicate glass, high aluminum glass, alkali-free boron aluminum glass, soda-lime glass, and photosensitive microcrystalline glass.

3. The method for efficiently preparing a through-glass hole with a high-precision aperture size as claimed in claim 1, It is characterized in that The acidic corrosive liquid includes hydrofluoric acid or a mixture of hydrofluoric acid and fluoride, and the fluoride includes ammonium fluoride, sodium fluoride and potassium fluoride.

4. The method for efficiently preparing a through-glass hole with a high-precision aperture size as claimed in claim 1, It is characterized in that The first time is calculated based on the average etching rate of the acidic etching solution and the target aperture value of the through-glass hole, that is, the target aperture value of the through-glass hole×95%÷the average etching rate of the acidic etching solution.

5. The method for efficiently preparing a through-glass hole with a high-precision aperture size as claimed in claim 4, It is characterized in that The average etching rate of the acidic etching solution is based on experimental measurement. Under the same etching conditions, the thickness reduction of the glass before and after etching in the acidic etching solution is measured and divided by the etching time. The average value is then obtained through at least three measurements.

6. The method for efficiently preparing a through-glass hole with a high-precision aperture size as claimed in claim 1, It is characterized in that The alkaline corrosive solution includes potassium hydroxide, sodium hydroxide, tetramethylammonium hydroxide and calcium hydroxide.

7. The method for efficiently preparing a through-glass hole with a high-precision aperture size as claimed in claim 1, It is characterized in that The second time is calculated based on the average etching rate of the alkaline corrosive solution and the target aperture value of the through-glass hole, that is, (target aperture value of the through-glass hole-measured aperture value of the through-glass hole 1) ÷ the average etching rate of the alkaline corrosive solution.

8. The method for efficiently preparing a through-glass hole with a high-precision aperture size as claimed in claim 7, It is characterized in that The average etching rate of the alkaline etching solution is based on experimental measurement. Under the same etching conditions, the thickness reduction of the glass before and after etching in the alkaline etching solution is measured and divided by the etching time. The average value is then obtained through at least three measurements.

9. The method for efficiently preparing a through-glass hole with a high-precision aperture size as claimed in claim 1, It is characterized in that The first temperature is 20°C to 30°C, the second temperature is 10°C to 30°C, and the third temperature is 65°C to 95°C.