Manufacturing method of wafer structure

By using high-k dielectric layer and work function layer structure in semiconductor devices, combined with the doping state of the substrate, the problem of insufficient threshold voltage regulation capability in traditional MOSFET structure is solved, and different threshold voltages are manufactured on the same wafer Devices, improving manufacturing efficiency and device reliability.

CN118899265APending Publication Date: 2024-11-05GUANGDONG GREATER BAY AREA INST OF INTEGRATED CIRCUIT & SYST +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410978479.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

At nodes below 28nm, due to the short channel effect, the gate control ability of the channel current is reduced, and the threshold voltage cannot be effectively regulated, resulting in the limitation of device power consumption and switching speed, and the prior art is difficult to manufacture in the same batch. Devices with different threshold voltages.

Method used

By forming a plurality of semiconductor device groups on the substrate, each device group including a buried oxygen layer, a channel layer and a gate structure consisting of a high k dielectric layer, an N-type work function layer and a metal gap filling layer. The threshold voltage of the device is regulated by the P-type work function layer and the doping state of the substrate to realize device manufacturing with different threshold voltages.

Benefits of technology

It realizes the manufacturing of devices with different threshold voltages on the same wafer, improves manufacturing efficiency, avoids the irreversibility and performance damage caused by channel doping, and enhances the reliability and manufacturing flexibility of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899265A_ABST
    Figure CN118899265A_ABST
Patent Text Reader

Abstract

The invention provides a manufacturing method of a wafer structure, which comprises the steps of providing a substrate and forming a plurality of semiconductor device groups on the substrate, each semiconductor device group comprises at least one semiconductor device, and each semiconductor device comprises a buried oxide layer, a channel layer on the buried oxide layer and a gate structure on the channel layer, the gate structure comprises a high-k dielectric layer, an N-type work function layer and a metal gap filling layer which are sequentially stacked upwards from the channel layer, the plurality of semiconductor device groups comprise a first device group and a second device group, and the semiconductor structures in the first device group and the second device group further comprise P-type work function layers. The thicknesses of the P-type work function layers in the semiconductor devices in the first device group and the semiconductor devices in the second device group are different, and / or the doping states of the substrates below the semiconductor devices in the first device group and the semiconductor devices in the second device group are different, so that devices with different threshold voltages can be manufactured on the same wafer; and the manufacturing efficiency of the device is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductors, and in particular to a method for manufacturing a wafer structure. Background Art

[0002] At nodes below 28nm, the control of the gate over the channel current in the traditional planar bulk silicon metal oxide semiconductor field effect transistor (MOSFET) structure has dropped to an unacceptable level due to the short channel effect, and a process with stronger gate control capability is required to optimize device performance. Advanced node semiconductor devices with stronger gate control capabilities mainly include fin field effect transistors (Fin Field Effect Transistor, FinFET) and fully depleted silicon on insulator transistors (Fully Depleted Silicon on Insulator, FDSOI).

[0003] FDSOI devices use a special structure to improve the performance and power consumption of semiconductor devices. They form an insulating layer and a thin layer of single crystal silicon in the insulating layer on the substrate. The insulating layer is usually silicon dioxide, called a buried oxide layer (BOX), and the thin layer of single crystal silicon is called the top silicon or SOI layer. The thin layer of single crystal silicon acts as a carrier channel with an extremely thin thickness. Under the influence of the gate voltage, it can form a fully depleted region outside the surface conduction channel, greatly reducing the leakage current. The buried oxide layer isolates the flow of current between the SOI layer and the substrate, thereby reducing the impact of leakage current and interconnect capacitance, and improving the switching speed and capacitance storage effect of the device. Because FDSOI devices reduce current loss and electron scattering, they can provide higher switching speeds, lower power consumption and better radiation resistance. FDSOI technology has been widely used in high-performance microprocessors, memory, and radio frequency circuits.

[0004] The threshold voltage of FDSOI affects the power consumption and operating speed of the device. The lower the threshold voltage, the higher the effective driving voltage at the same operating voltage. Therefore, the smaller the saturation voltage, the larger the output current, and the higher the current switching speed. However, too low a threshold voltage will cause the off-state current to rise sharply, resulting in increased leakage and increased power consumption. Conversely, the larger the threshold voltage, the slower the switching speed of the device and the lower the power consumption.

[0005] Devices with different threshold voltages can be selected according to different design requirements. Devices with different threshold voltages can be obtained without changing the device structure, which can improve the manufacturing efficiency of the device. Summary of the invention

[0006] In view of this, the purpose of the present application is to provide a method for manufacturing a wafer structure, which can set semiconductor devices with different threshold voltages on the same wafer structure to improve the manufacturing efficiency of the devices.

[0007] The present application provides a method for manufacturing a wafer structure, including:

[0008] providing a substrate;

[0009] forming a plurality of semiconductor device groups on the substrate; each semiconductor device group includes at least one semiconductor device;

[0010] The formation process of the semiconductor device includes:

[0011] Forming a buried oxide layer on the substrate, a channel layer on the buried oxide layer, and a gate structure on the channel layer, wherein the gate structure comprises a high-k dielectric layer, an N-type work function layer, and a metal gap filling layer stacked in sequence from the channel layer upward;

[0012] The plurality of semiconductor device groups include a first device group and a second device group, and the semiconductor structures in the first device group and the second device group further include a P-type work function layer between the high-k dielectric layer and the N-type work function layer;

[0013] The thickness of the P-type work function layer in the semiconductor devices in the first device group and the semiconductor devices in the second device group is different, and / or the doping states of the substrates under the semiconductor devices in the first device group and the semiconductor devices in the second device group are different, and the doping states include the doping types of the substrate and the channel layer on the substrate being the same or opposite.

[0014] Optionally, if the thickness of the P-type work function layer in the semiconductor devices in the first device group and the semiconductor devices in the second device group are different, the process of forming the gate structure includes:

[0015] forming a high-k dielectric layer on the channel layer in the first device group and the second device group;

[0016] Blocking the area where the first device group is located to form a P-type work function layer in the second device group, and blocking the area where the second device group is located to form a P-type work function layer in the first device group;

[0017] forming an N-type work function layer on the P-type work function layer in the first device group and the second device group;

[0018] A metal gap-filling layer is formed on the N-type work function layer in the first device group and the second device group.

[0019] Optionally, if the thickness of the P-type work function layer in the semiconductor devices in the first device group and the semiconductor devices in the second device group are different, the process of forming the gate structure includes:

[0020] forming a high-k dielectric layer on the channel layer in the first device group and the second device group;

[0021] forming a P-type work function layer having a preset thickness in the first device group and the second device group;

[0022] The area where the first device group is located is shielded to thin the P-type work function layer in the second device group, and / or the area where the second device group is located is shielded to thin the P-type work function layer in the first device group;

[0023] forming an N-type work function layer on the P-type work function layer in the first device group and the second device group;

[0024] A metal gap-filling layer is formed on the N-type work function layer in the first device group and the second device group.

[0025] Optionally, if the doping states of the substrates under the semiconductor devices in the first device group and the semiconductor devices in the second device group are different, the method further includes:

[0026] The substrate in the area where the first device group is located is shielded so as to dope the substrate in the area where the second device group is located; and / or, the substrate in the area where the second device group is located is shielded so as to dope the substrate in the area where the first device group is located.

[0027] Optionally, the thickness range of the P-type work function layer is (0nm, 6nm].

[0028] Optionally, the thickness ranges of the P-type work function layers in the semiconductor devices in the first device group and the semiconductor devices in the second device group are different, and the thickness range includes one of a first range, a second range and a third range, the first range is [1.5nm, 2nm], the second range is [2.7nm, 4nm], and the third range is (4nm, 6nm].

[0029] Optionally, the doping type of the channel layer in the semiconductor device in the first device group is N-type, the thickness of the P-type work function layer in the semiconductor device in the first device group belongs to the first range, and at least one of the first device and the second device in the first device group, the substrate under the first device and the channel layer in the first device have the same doping type, and the substrate under the second device and the channel layer in the second device have opposite doping types.

[0030] Optionally, the doping type of the channel layer in the semiconductor devices in the second device group is P-type, the second device group includes at least one of the first group and the second group, the thickness of the P-type work function layer in the semiconductor devices in the first group belongs to the second range, and the thickness of the P-type work function layer in the semiconductor devices in the second group belongs to the third range;

[0031] The first group includes at least one of a third device and a fourth device, the substrate under the third device and the channel layer in the third device have the same doping type, and the substrate under the fourth device and the channel layer in the fourth device have opposite doping types;

[0032] The second group includes at least one of a fifth device and a sixth device, the substrate under the fifth device and the channel layer in the fifth device have the same doping type, and the substrate under the sixth device and the channel layer in the sixth device have opposite doping types.

[0033] Optionally, the plurality of semiconductor device groups further include a third device group, and the semiconductor devices in the third device group do not have a P-type work function layer; and the process of forming the gate structure includes:

[0034] forming a high-k dielectric layer on the channel layer in the first device group, the second device group, and the third device group;

[0035] Blocking the area where the first device group and the third device group are located to form a P-type work function layer in the second device group, and blocking the area where the second device group and the third device group are located to form a P-type work function layer in the first device group;

[0036] forming an N-type work function layer on the P-type work function layer in the first device group, the second device group, and the third device group;

[0037] A metal gap-filling layer is formed on the N-type work function layer in the first device group, the second device group, and the third device group.

[0038] Optionally, the doping type of the channel layer in the semiconductor device in the third device group is N-type;

[0039] The third device group includes at least one of a seventh device and an eighth device, the substrate under the seventh device and the channel layer in the seventh device have the same doping type, and the substrate under the eighth device and the channel layer in the eighth device have opposite doping types.

[0040] Optionally, in the plurality of semiconductor device groups, semiconductor devices having the same P-type work function layer thickness and the same doping state are arranged within the same area.

[0041] Optionally, the method further includes:

[0042] forming a dummy gate structure on the channel layer;

[0043] A source structure and a drain structure located on both sides of the dummy gate structure;

[0044] The dummy gate structure is removed to obtain a dummy gate trench, and the dummy gate trench is used to form the gate structure.

[0045] Optionally, the method further includes:

[0046] At least one of an oxide layer between the high-k dielectric layer and the channel layer, a high-k dielectric protection layer and an etching barrier layer between the high-k dielectric layer and the N-type work function layer, and a barrier layer between the N-type work function layer and the metal gap filling layer is formed.

[0047] Optionally, the material of the oxide layer is silicon oxide, and the thickness range is [3nm, 4nm];

[0048] And / or, the material of the high-k dielectric layer is HfO2, and the thickness range is [1nm, 1.5nm];

[0049] And / or, the material of the high-k dielectric protection layer is TiN, and the thickness range is [0.8nm, 1.2nm];

[0050] And / or, the material of the etching stop layer is tantalum nitride or tantalum compound, and the thickness range is [0.5nm, 0.9nm];

[0051] And / or, the material of the P-type work function layer is TiN; the material of the N-type work function layer is titanium aluminum, titanium aluminum carbide or titanium aluminum oxide, and the thickness range is [4.5nm, 5.5nm];

[0052] And / or, the material of the barrier layer is TiN, and the thickness range is [1.5nm, 2.5nm];

[0053] And / or, the material of the metal gap filling layer is tungsten; the sum of the thicknesses of the metal gap filling layer and the P-type work function layer is a preset value;

[0054] And / or, the buried oxide layer has a thickness of 15 nm, and the channel layer is made of silicon with a thickness of 5 nm.

[0055] Optionally, the method further includes:

[0056] A back gate connected to the substrate under the semiconductor device is formed.

[0057] The present application provides a method for manufacturing a wafer structure, including providing a substrate, and forming a plurality of semiconductor device groups on the substrate, each semiconductor device group including at least one semiconductor device, the semiconductor device including a buried oxide layer, a channel layer on the buried oxide layer, and a gate structure on the channel layer, the gate structure including a high-k dielectric layer, an N-type work function layer, and a metal gap filling layer stacked in sequence from the channel layer upward, the plurality of semiconductor device groups including a first device group and a second device group, the semiconductor structures in the first device group and the second device group also including a P-type work function layer between the high-k dielectric layer and the N-type work function layer. The thickness of the P-type work function layer in the semiconductor devices in the first device group and the semiconductor devices in the second device group is different, and / or the doping state of the substrate under the semiconductor devices in the first device group and the semiconductor devices in the second device group is different, the doping state including the substrate and the channel layer on the substrate being the same or opposite, so that the semiconductor devices in the first device group and the second device group can have different threshold voltages, the different threshold voltages are regulated by at least one of the thickness of the P-type work function layer and the doping state of the substrate, the device structure difference is small, so that devices with different threshold voltages can be manufactured on the same wafer, which is easy to implement and improves the manufacturing efficiency of the device. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0059] Figure 1 A schematic diagram of the structure of an FDSOI device provided in an embodiment of the present application is shown;

[0060] Figure 2 A flow chart of a method for manufacturing a wafer structure provided in an embodiment of the present application;

[0061] Figure 3 A schematic diagram of a wafer structure provided in an embodiment of the present application;

[0062] Figure 4 A schematic diagram of the structure of an SOI substrate provided in an embodiment of the present application;

[0063] Figure 5 A schematic diagram of a gate structure provided in an embodiment of the present application;

[0064] Figure 6A schematic diagram of another gate structure provided in an embodiment of the present application;

[0065] Figure 7 A schematic flow chart of another method for manufacturing a wafer structure provided in an embodiment of the present application. DETAILED DESCRIPTION

[0066] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0067] In the following description, many specific details are set forth to facilitate a full understanding of the present application, but the present application may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present application. Therefore, the present application is not limited to the specific embodiments disclosed below.

[0068] This application is described in detail with reference to schematic diagrams. When describing the embodiments of this application in detail, for the sake of convenience, the cross-sectional diagrams showing the device structure will not be partially enlarged according to the general scale, and the schematic diagrams are only examples, which should not limit the scope of protection of this application. In addition, in actual production, the three-dimensional dimensions of length, width and depth should be included.

[0069] At present, the threshold voltage of FDSOI devices affects the power consumption and operating speed of the devices. Devices with different threshold voltages can be selected according to different design requirements. Devices with different threshold voltages can be obtained without changing the device structure, which can improve the manufacturing efficiency of the device.

[0070] refer to Figure 1 As shown, it is a schematic diagram of the structure of an FDSOI device provided in an embodiment of the present application. In the FDSOI device, a gate (gate, G), a source (source, S) and a drain (drain, D) are arranged on a thin layer of silicon. Under the control of the gate voltage, the interface between the channel and the gate forms or closes a channel that gathers electrons or holes, thereby turning the device on or off.

[0071] At present, the threshold voltage of FDSOI can be changed by channel doping. Channel doping refers to changing the material doping concentration in the channel region of a semiconductor device, thereby changing the electrical properties of the channel region. When the channel doping concentration increases, the carrier density in the channel region also increases, which causes the resistance of the channel region to decrease. In a field effect transistor, when the channel doping concentration changes, its threshold voltage also changes. The threshold voltage refers to the minimum voltage value applied between the gate and the source to form a conductive channel in the channel region.

[0072] When the doping concentration of the channel region changes, the corresponding number of carriers in the channel region will change accordingly, so the threshold voltage will also change accordingly. Therefore, channel doping is a basic method to control the electrical characteristics of field effect transistors. The threshold voltage and resistance characteristics can be adjusted by changing the channel doping concentration, thereby achieving more precise circuit control.

[0073] However, channel doping is difficult to achieve precise control in the actual process because in actual operation, the doping process may be affected by some uncertain factors, such as material heterogeneity and process changes. This may lead to large deviations between devices, making it impossible to achieve the required precise control. In addition, once the channel doping operation to change the threshold voltage is performed, it cannot be reversed. Because doping is a permanent change and has a significant impact on the subsequent process and performance of the transistor. Therefore, if it is found later that the threshold voltage needs to be adjusted, the device may need to be redesigned and manufactured. In addition, changes in device performance due to channel doping may have a negative impact on the reliability of the device. For example, an increase in leakage current may shorten the life of the device and increase the risk of failure.

[0074] The inventors have found through research that the threshold voltage (Threshold Voltage) of the FDSOI device at turn-on or turn-off may vary due to differences in gate dielectric materials, processes and thicknesses.

[0075] The gate structure of FDSOI usually needs to use multiple materials to form a multi-layer structure to adapt to different uses. In FDSOI devices, the gate structure is usually composed of gate metal, gate dielectric and gate silicon. Gate metal is mainly used to provide gate voltage, and the gate electric field controls the flow of carriers in the channel through the channel to achieve the switching function, and the effect of controlling the flow of electrons through the gate area. Common gate metal materials include aluminum (Al), tungsten (W), copper (Cu), etc. The gate dielectric needs to have the characteristics of high insulation and low leakage current. Commonly used gate dielectric materials include silicon oxide (SiO2), high dielectric constant materials such as high dielectric constant (High-k, HfO2) dielectric materials, etc. The gate dielectric is mainly used to isolate the gate metal from the silicon layer to realize MOS capacitance and reduce the capacitance. The thinner the gate dielectric layer is, the more it is beneficial to achieve a larger unit area capacitance, thereby increasing gate control, reducing the operating voltage and reducing power consumption. Gate silicon refers to the silicon layer deposited on the gate dielectric; the gate silicon can be materials such as single crystal silicon, polycrystalline silicon or silicon amide.

[0076] However, there is currently a lack of solutions for regulating the threshold voltage through the gate structure, and it is impossible to produce devices with different threshold voltages in the same batch manufacturing process.

[0077] Based on the above technical problems, the embodiment of the present application provides a method for manufacturing a wafer structure, including providing a substrate, and forming a plurality of semiconductor device groups on the substrate, each semiconductor device group including at least one semiconductor device, the semiconductor device including a buried oxide layer, a channel layer on the buried oxide layer, and a gate structure on the channel layer, the gate structure including a high-k dielectric layer, an N-type work function layer, and a metal gap filling layer stacked in sequence from the channel layer upward, the plurality of semiconductor device groups including a first device group and a second device group, the semiconductor structures in the first device group and the second device group also including a P-type work function layer between the high-k dielectric layer and the N-type work function layer. The thickness of the P-type work function layer in the semiconductor devices in the first device group and the semiconductor devices in the second device group is different, and / or the doping state of the substrate under the semiconductor devices in the first device group and the semiconductor devices in the second device group is different, the doping state includes the substrate and the channel layer on the substrate being the same or opposite, so that the semiconductor devices in the first device group and the second device group can have different threshold voltages, and the different threshold voltages are regulated by at least one of the thickness of the P-type work function layer and the doping state of the substrate, the device structure difference is small, easy to implement, and the manufacturing efficiency of the device is improved.

[0078] In order to better understand the technical solution and technical effects of the present application, specific embodiments will be described in detail below with reference to the accompanying drawings.

[0079] See also Figure 2 FIG. 1 is a flow chart of a method for manufacturing a wafer structure provided in an embodiment of the present application. The method may include:

[0080] S101, providing a substrate.

[0081] S102, forming a plurality of semiconductor device groups on a substrate.

[0082] See also Figure 3 , which is a schematic diagram of a wafer structure provided by an embodiment of the present application, the wafer structure includes a substrate 100, and a plurality of semiconductor device groups on the substrate, each semiconductor device group includes at least one semiconductor device. The semiconductor devices in different semiconductor device groups have different threshold voltages.

[0083] The semiconductor devices in each semiconductor device group may have exactly the same structure and parameters, or may have the same structure and different parameters. The semiconductor devices in the same semiconductor device group may be arranged within the same region, so as to facilitate the simultaneous formation of devices with the same threshold voltage or similar threshold voltage. Among them, semiconductor devices with the same structure and parameters (with the same threshold voltage and manufacturing process) may be arranged within the same region, so as to facilitate the manufacturing management of the devices.

[0084] In the embodiment of the present application, the substrate is used to provide support for the film layer thereon, and may be a semiconductor substrate such as a silicon substrate, a germanium substrate, etc., specifically a silicon wafer or a germanium wafer.

[0085] The semiconductor device includes a buried oxide layer 120, a channel layer 130 on the buried oxide layer 120, and a gate structure 180 on the channel layer 130. Figure 1 As shown. Among them, the material of the buried oxide layer can be silicon oxide, and the thickness can be 15nm, and the material of the channel layer can be silicon, and the thickness can be 5nm, so that the semiconductor device corresponds to the 12nm node. Of course, when the device corresponds to other nodes, the thickness of the buried oxide layer and the channel layer can be adjusted accordingly. The ultra-thin silicon on insulator naturally limits the source-drain junction depth, and also limits the depletion region of the source-drain junction, thereby improving short channel effects such as drain induced barrier lowering (DIBL). The thinned BOX layer improves the back gate control capability and enhances the flexibility of circuit design.

[0086] In addition, the semiconductor structure may further include a source structure 151 and a drain structure 152 located on both sides of the gate structure on the channel layer, and may further include a back gate connected to the substrate under the semiconductor device. Metal contacts may also be formed on the source structure, the drain structure and the back gate. Adjacent semiconductor structures are isolated by a shallow trench isolation (STI) structure, and the isolation structure includes a first structure 141 located on one side of the source structure 151 and a second structure 142 located on one side of the drain structure 152. The sidewalls of the gate structure also include sidewalls, and the sidewalls include a left sidewall 161 and a right sidewall 162.

[0087] The formation process of the semiconductor device may include: forming a buried oxide layer 120 on a substrate 110, and a channel layer 130 on the buried oxide layer 120. The structure is recorded as an SOI substrate. Figure 4 , which is a schematic diagram of the structure of an SOI substrate provided in an embodiment of the present application. The buried oxide layer can be formed by a deposition process or an oxidation process, and the channel layer can be formed by an epitaxial process. The buried oxide layer and the channel layer in different semiconductor devices can be formed simultaneously.

[0088] After forming the channel layer, a gate structure can be formed on the channel layer. The gate structure can be formed by a deposition process. The gate structure can be formed before the source structure and the drain structure (called the gate-first process), or after the source structure and the drain structure (called the gate-last process). Due to the presence of a film layer that is not resistant to high temperatures in the gate structure, the gate-last process can ensure the integrity of the gate structure and the stability of the performance, so the gate-last process has a more accurate ability to adjust the threshold voltage. By adjusting the electric field distribution between the gate and the channel, a more accurate threshold voltage adjustment is achieved, achieving the purpose of achieving different threshold voltages simultaneously under the same process flow. In contrast, the gate-first technology is limited by the limitations of materials and processes, and the threshold voltage adjustment accuracy is low. The gate-last technology enables the device to have higher electron mobility and lower leakage current under different working conditions.

[0089] In the gate-first process, the gate structure may be formed first, and then the source structure and the drain structure may be formed. The sidewalls of the gate structure form sidewalls, which may protect the gate structure.

[0090] In the gate-last process, a dummy gate structure and a sidewall of the dummy gate structure may be formed first, and then a source structure and a drain structure may be formed, the dummy gate structure may be removed to obtain a dummy gate trench, and a gate structure may be formed in the dummy gate trench. The source structure in different semiconductor devices may be formed simultaneously, the drain structure may be formed simultaneously, the dummy gate trench may be formed simultaneously, and the same film layer in the gate structure may be formed simultaneously.

[0091] Specifically, refer to Figure 3As shown, a dummy gate dielectric layer can be formed on the SOI substrate. The material of the dummy gate dielectric layer can be silicon nitride, and the formation method can be chemical vapor deposition. The silicon nitride film prepared by this method has good density, can meet the stoichiometric ratio, and has strong adhesion to the upper surface of the silicon on insulator (channel layer 130), and at the same time acts as a hard mask to protect the silicon on insulator (channel layer 130); a dummy gate material is formed on the dummy gate dielectric layer and patterned (for example, by photolithography and etching process) to obtain a dummy gate structure. The material of the dummy gate structure is Polycrystalline silicon, polycrystalline silicon pseudo-gate has high temperature resistance and realizes self-aligned graphics, and the length can be, for example, 20nm; sidewalls (including left side wall 161 and right side wall 162) are formed on the sidewalls of the pseudo-gate structure, and the sidewall material can be, for example, SiCO, and the formation method can be a low-temperature deposition process, and the thickness can be 11nm. SiCO has a low dielectric constant, which reduces the parasitic capacitance between the source and drain electrodes to the gate and the channel, and improves the frequency characteristics of the device; then, the source and drain region patterns can be defined, and the pseudo-gate dielectric layer on the surface of the source and drain regions is removed by an etching process, and a source structure and a drain structure are formed on the surface of the source and drain regions, wherein silicon material (source structure 151 and drain structure 152) can be epitaxially generated, with a thickness of about 18nm, and doping and high-temperature annealing (for example, 1050°C) are performed in the silicon material to activate, and the source structure and the drain structure are obtained, and the doping material can be boron ions, and the doping method can be an ion implantation process, and metal silicide can also be formed on the source structure and the drain structure; then, an etching stop layer and an intermediate layer can be formed and polished (for example, a chemical mechanical polishing method) , an exposed pattern area is formed at the dummy gate position, the material of the etch stop layer can be silicon nitride, and the material of the middle layer can be silicon oxide, both of which have high density and strong hardness, forming a gate hard mask pattern; the dummy gate structure is removed (for example, by ion beam etching) in the exposed pattern area to form a dummy gate trench, and the dummy gate dielectric layer at the bottom of the dummy gate trench is removed (for example, by phosphoric acid wet etching) until the channel layer is exposed; then a gate structure can be formed in the dummy gate trench, the wet etching selectivity is high, and at the same time, no substrate damage is generated, and the silicon interface on the insulator is protected.

[0092] refer to Figure 5 , which is a schematic diagram of a gate structure provided by an embodiment of the present application, the gate structure may include a high-k (high dielectric constant, High-k) dielectric layer (HK layer for short), an N-type work function layer, and a metal gap filling layer stacked in sequence from the channel layer upward. Figure 6 As shown, it is a structural schematic diagram of another gate structure provided in an embodiment of the application. The gate structure may also include a P-type work function layer between the high-k dielectric layer and the N-type work function layer, that is, the gate structure may include a high-k dielectric layer, a P-type work function layer, an N-type work function layer and a metal gap filling layer stacked in sequence from the channel layer upward.

[0093] The plurality of semiconductor device groups may include a first device group 1100 and a second device group 1200, wherein the semiconductor structures in the first device group and the second device group include a P-type work function layer. The plurality of semiconductor device groups may further include a third device group, wherein the semiconductor structures in the third device group do not include a P-type work function layer.

[0094] In addition, the semiconductor device may further include an oxide layer between the high-k dielectric layer and the channel layer (ie, an oxide layer 170 may be provided between the gate structure 180 and the channel layer 130, see Figure 1 As shown in the figure, it may also include a high-k dielectric protection layer (HK protection layer for short) and an etching barrier layer between the high-k dielectric layer and the N-type work function layer. When the semiconductor device includes a P-type work function layer, the high-k dielectric protection layer and the etching barrier layer are located between the high-k dielectric layer and the P-type work function layer. It may also include a barrier layer between the N-type work function layer and the metal gap filling layer. The above oxide layer, high-k dielectric protection layer, etching barrier layer and barrier layer may be provided with only one or more of them.

[0095] The oxide layer serves as a dielectric material and a buffer layer between the high-k dielectric layer and the channel layer. Because directly contacting the hafnium dioxide as a high-k dielectric layer with the silicon channel may increase the interface state density: hydrogen atoms on the surface of the silicon channel are easily adsorbed by hafnium dioxide and form hydrogen defects and silicon oxide interface states. The number of these interface states will increase, resulting in a decrease in the performance of the transistor, especially the subthreshold swing. The addition of the oxide layer can avoid the increase in the number of interface states and the decrease in transistor performance. The material of the oxide layer can be silicon oxide (SiO2), with a thickness range of [3nm, 4nm].

[0096] High-K Metal Gate (HKMG) is a semiconductor manufacturing technology. In the traditional manufacturing process, the gate of the transistor is polysilicon, and silicon dioxide is usually used as a dielectric layer between the insulating layer. However, as the chip size continues to shrink, problems such as leakage and charge leakage when the transistor is turned on and off begin to appear. In order to solve these problems, HKMG technology was introduced into the manufacturing process. It uses a material with a high dielectric constant (High-K) as a dielectric layer to replace the traditional silicon dioxide, and uses metal (usually a metal gate) as the gate material. High dielectric constant materials can provide better electrical insulation performance and reduce charge leakage problems, while metal gates can improve the switching characteristics of transistors. As a high dielectric constant material, the high-k dielectric layer brings higher capacitance and stronger gate control capability, which is conducive to controlling the short channel effect to achieve smaller leakage current, and is conducive to further miniaturization of device size. Optional materials include hafnium dioxide (HfO2), etc., with a thickness range of [1nm, 1.5nm].

[0097] The high-k dielectric protection layer (HK protection layer) serves as a buffer protection layer to prevent the sputtering process in the subsequent process from damaging the hafnium dioxide film. It also has good electron mobility, thermal stability and anti-reactivity (not easy to react with HfO2). Optional materials include titanium nitride (TiN), etc., with a thickness range of [0.8nm, 1.2nm].

[0098] The etch barrier layer has the characteristics of high hardness, etching resistance and good adhesion, protecting the HK layer from the influence of etching. The optional material is tantalum nitride (TaN) or tantalum compound, and the thickness range is [0.5nm, 0.9nm].

[0099] The P-type work function layer has a lower work function, which is beneficial to control the hole channel and improve the hole transmission efficiency. At the same time, this layer of material has excellent thermal stability, electrical properties and interface performance, which is suitable for packaging and manufacturing requirements. Optional materials include titanium nitride (TiN) and so on.

[0100] The N-type work function layer can freely adjust the threshold voltage of the transistor according to the difference in thickness and material ratio. The material is titanium aluminum (TiAl), titanium aluminum carbide (TiAlC) or titanium aluminum oxide (TiAlO), and the thickness range is [4.5nm, 5.5nm].

[0101] The barrier layer is used to highly prevent metal migration, that is, as a diffusion barrier, and the material is titanium nitride (TiN) with a thickness of about [1.5nm, 2.5nm].

[0102] The metal gap filling layer has a better filling ability and is used as a wiring material to supplement the thickness of the gate structure, so that the thickness of the gate structure in each semiconductor device is the same, ensuring the smoothness of the device surface.

[0103] In the embodiment of the present application, the semiconductor devices in the first device group and the second device group may have different threshold voltages. Specifically, the thickness of the P-type work function layer in the semiconductor devices in the first device group and the semiconductor devices in the second device group is different, and / or the doping state of the substrate under the semiconductor devices in the first device group and the semiconductor devices in the second device is different, and the doping state includes the substrate and the channel layer on the substrate being the same or opposite in doping type. In other words, the threshold voltage of the semiconductor device can be regulated by the thickness of the P-type work function layer and the doping state of the substrate, so as to obtain a semiconductor device that meets the requirements, and the requirements of simultaneously producing devices with different threshold voltages can be met while the overall process remains basically the same, so that devices with different threshold voltages can be produced in the same batch manufacturing process, avoiding channel doping of two threshold voltages of HVT and LVT, improving channel mobility, and reducing mismatch, so as to meet the growing demand for device miniaturization.

[0104] The adjustable range of the thickness of the P-type work function layer is (0nm, 6nm], and the sum of the thicknesses of the metal gap filling layer and the P-type work function layer is a preset value, which is a fixed value, so that the sum of the thicknesses of the two is fixed, thereby making the thickness of the gate structure in each semiconductor device consistent.

[0105] The thickness ranges of the P-type work function layers in the semiconductor devices in the first device group and the semiconductor devices in the second device group are different, and the thickness range includes one of a first range, a second range and a third range. The first range is [1.5nm, 2nm], the second range is [2.7nm, 4nm], and the third range is (4nm, 6nm). Different thickness ranges correspond to different threshold voltages.

[0106] According to the different requirements of integrated circuits for performance or operating speed, the threshold voltage can be divided into SLVT (Super Low Threshold Voltage), LVT (Low Threshold Voltage), RVT (Regular Threshold Voltage), HVT (High Threshold Voltage) from small to large (corresponding to the operating speed from fast to slow). Power consumption control and operating speed have always been a contradiction, that is, SLVT has the lowest threshold voltage and the fastest speed, but the highest power consumption; HVT has the highest device threshold voltage and the slowest speed, but its leakage power consumption is the lowest. Depending on the design requirements, devices with different threshold voltages can be selected. Considering that the devices on the same wafer are manufactured at the same time, it is necessary to strictly control the gap in the process flow required for different devices, and ensure that the difference in thickness of the final products of different devices is minimized to ensure the stability and consistency of device performance.

[0107] Flip-well is the reverse doping of the substrate, that is, the doping type of the substrate is opposite to the doping type of the channel. Conventional planar MOSFET devices use conventional wells, that is, the doping type of the substrate is the same as the doping type of the channel. In order to prevent leakage from the drain to the substrate, the doping of the conventional well forms an inverse PN junction with the device itself. In FDSO, due to the presence of the buried oxide layer, the leakage path from the source to the substrate is blocked, the leakage current can be ignored, and there is no need to form a reverse PN junction. In this case, Flip-Well technology can be applied in FDSOI devices. For FDSOI, by changing the Conventional-well to Flip-well, the work function of the channel can be adjusted, thereby achieving the effect of lowering the threshold voltage. The optional range of Flip-well doping concentration in the present invention is about 10 15 ~10 17 / cm 3 The higher the concentration, the lower the threshold voltage. The Conventional-well structure has higher current carrying capacity and lower noise, suitable for high-speed and high-power applications. The Flip-well structure has lower leakage current and is suitable for low-power and low-voltage applications.

[0108] Back biasing is a way to adjust device performance by changing the substrate voltage to adjust parameters such as current and speed. This technique is particularly useful in FDSOI because the substrate is an insulating layer in which electrons move more slowly, which means that the structure can better control the flow of electrons. In addition, back biasing of FDSOI can also be used to adjust the device threshold voltage to enhance the performance of the device. In contrast, in planar MOSFET devices, the substrate continues to act as a ground terminal between the source and drain, so back biasing is not commonly used. In planar MOSFETs, current can only flow from the ground to the lead, while in FDSOI devices, back biasing can provide an electric field to the channel layer, which makes back biasing technology possible.

[0109] In the embodiment of the present application, since the doping state of the P-type work function layer and the substrate can both affect the threshold voltage of the device, devices with different threshold voltages can be obtained by combining the two. Referring to Table 1, the structural parameters corresponding to different threshold voltage states are shown.

[0110] Table 1 Structural parameters corresponding to different threshold voltage states

[0111] P-type work function thickness 0 1.5~2nm 2.7~4nm 4~6nm Conventional trap N-type HVT N type RVT P-type RVT P-type HVT Inversion Trap N-type LVT N-type SLVT P-type SLVT P-type LVT

[0112] For the sake of convenience of explanation, the semiconductor device corresponding to N-type RVT can be recorded as the first device, the semiconductor device corresponding to N-type SLVT can be recorded as the second device, the semiconductor device corresponding to P-type RVT can be recorded as the third device, the semiconductor device corresponding to P-type SLVT can be recorded as the fourth device, the semiconductor device corresponding to P-type HVT can be recorded as the fifth device, the semiconductor device corresponding to P-type LVT can be recorded as the sixth device, the semiconductor device corresponding to N-type HVT can be recorded as the seventh device, and the semiconductor device corresponding to N-type LVT can be recorded as the eighth device.

[0113] That is, the doping type of the channel layer in the semiconductor device in the first device is N-type, the thickness of the P-type work function layer belongs to the first range, and the substrate under the first device has the same doping type as the channel layer in the first device; the doping type of the channel layer in the semiconductor device in the second device is N-type, the thickness of the P-type work function layer belongs to the first range, and the substrate under the second device has opposite doping types to the channel layer in the second device. The doping type of the channel layer in the semiconductor device in the third device is P-type, the thickness of the P-type work function layer belongs to the second range, and the substrate under the third device has the same doping type as the channel layer in the third device; the doping type of the channel layer in the semiconductor device in the fourth device is P-type, the thickness of the P-type work function layer belongs to the second range, and the substrate under the fourth device has opposite doping types to the channel layer in the fourth device. The doping type of the channel layer in the semiconductor device in the fifth device is P-type, the thickness of the P-type work function layer belongs to the third range, and the substrate under the fifth device has the same doping type as the channel layer in the fifth device; the doping type of the channel layer in the semiconductor device in the sixth device is P-type, the thickness of the P-type work function layer belongs to the third range, and the substrate under the sixth device has opposite doping types to the channel layer in the sixth device. The doping type of the channel layer in the semiconductor device in the seventh device is P-type, there is no P-type work function layer, and the doping type of the substrate under the seventh device and the channel layer in the seventh device are the same; the doping type of the channel layer in the semiconductor device in the eighth device is P-type, there is no P-type work function layer, and the doping type of the substrate under the eighth device and the channel layer in the eighth device are opposite.

[0114] In specific implementation, at least two semiconductor devices of the above eight devices can be arranged on the wafer structure, corresponding to at least two of the above eight threshold voltage states. For example, devices with the same channel doping type and different threshold voltages can be arranged, or devices with the same substrate doping state and different threshold voltages can be arranged, or devices with the same P-type work function layer thickness and different threshold voltages can be arranged, thereby further simplifying the process.

[0115] Of course, more devices corresponding to threshold voltages can also be set according to actual needs, and devices with the same channel doping type and different threshold voltages, or devices with the same substrate doping state and different threshold voltages, or devices with the same P-type work function layer thickness and different threshold voltages can be set in adjacent areas to reduce the impact on devices in other areas. Among the multiple semiconductor device groups, semiconductor devices with the same P-type work function layer thickness and the same doping state are set within the same area.

[0116] For example, the first device group may include at least one of the first device and the second device, then the doping type of the channel layer in the semiconductor device in the first device group is N-type, and the thickness of the P-type work function layer in the semiconductor device in the first device group belongs to the first range; the second device group may include at least one of the first group and the second group, the first group may include at least one of the third device and the fourth device, and the second group may include at least one of the fifth device and the sixth device, then the doping type of the channel layer in the semiconductor device in the second device group is P-type, the thickness of the P-type work function layer in the semiconductor device in the first group belongs to the second range, and the thickness of the P-type work function layer in the semiconductor device in the second group belongs to the third range.

[0117] The multiple semiconductor devices may further include a third device group, the third device group including at least one of the seventh device and the eighth device. Then the multiple semiconductor device groups also include a third device group, the semiconductor devices in the third device group do not have a P-type work function layer; the doping type of the channel layer in the semiconductor devices in the third device group is N-type.

[0118] In the process of forming the gate structure, an oxide layer and a high-k dielectric layer can be formed in all regions first. The oxide layer can be formed by chemical vapor deposition, and the high-k dielectric layer can be formed by atomic layer deposition. The oxidized silicon gate oxide layer forms excellent interface characteristics with silicon on insulator, and plays a buffering role between the high-k dielectric layer and the silicon on insulator. The high-k hafnium oxide dielectric layer has a low equivalent oxide layer (EOT), improves the gate's channel control capability, and reduces the short channel effect of the 12nm node FDSOI device. Afterwards, a high-k dielectric protection layer and an etching stop layer can be formed in all regions.

[0119] If the thickness of the P-type work function layer in the semiconductor devices in the first device group and the second device group is different, the area where the first device group is located can be shielded first to form the P-type work function layer in the second device group, and the area where the second device group is located can be shielded to form the P-type work function layer in the first device group. Among them, P-type work function layers of different thicknesses belonging to the same device group can be deposited separately. If a third device group is also formed on the wafer structure, when shielding the area where the first device group is located, the area where the third device group is located can also be shielded, and when shielding the area where the second device group is located, the area where the third device group is located can also be shielded to avoid forming a P-type work function layer in the area where the third device group is located.

[0120] Alternatively, a P-type work function layer with a preset thickness can be first formed in the area where the first device group and the second device group are located, and then the area where the first device group is located can be shielded to thin the P-type work function layer in the second device group, and / or, the area where the second device group is located can be shielded to thin the P-type work function layer in the first device group. Among them, P-type work function layers of different thicknesses belonging to the same device group can also be deposited simultaneously and then etched separately, which will not be repeated again. If a third device group is also formed on the wafer structure, the first device group and the second device group can be shielded to remove the P-type work function layer in the third device group.

[0121] Afterwards, an N-type work function layer, a barrier layer and a metal gap filling layer may be formed in each device region to obtain a gate structure, and the gate structure may be planarized by chemical mechanical polishing to complete the preparation of the gate structure.

[0122] refer to Figure 7 As shown, a flow chart of another method for manufacturing a wafer structure provided in an embodiment of the present application, the method may include: S210, providing an SOI substrate; S220, forming a dummy gate oxide and forming a polysilicon dummy gate electrode (i.e., a dummy gate structure); S230, forming side walls on both sides of the polysilicon dummy gate; S240, removing the dummy gate oxide layer on the surface of the source and drain regions, growing a silicon epitaxial layer, forming boron ion doping and annealing activation; S250, forming a dummy gate trench, removing the dummy gate oxide layer at the bottom of the dummy gate trench; S260, forming a bottom gate oxide layer and a high-k dielectric layer, and filling multiple layers of metal to form a metal gate.

[0123] In addition, if the doping states of the substrates under the semiconductor devices in the first device group and the semiconductor devices in the second device group are different, then the substrate in the area where the first device group is located is shielded to dope the substrate in the area where the second device group is located; and / or, the substrate in the area where the second device group is located is shielded to dope the substrate in the area where the first device group is located. Substrates with different doping states belonging to the same device group can be doped separately. If a third device group is also formed on the wafer structure, doping can be performed according to the doping state of the substrate of the third device group.

[0124] After obtaining the wafer structure, the wafer structure may be cut to obtain a plurality of semiconductor devices, and the plurality of semiconductor devices may be put into use according to actual needs.

[0125] The present application provides a method for manufacturing a wafer structure, including providing a substrate, and forming a plurality of semiconductor device groups on the substrate, each semiconductor device group including at least one semiconductor device, the semiconductor device including a buried oxide layer, a channel layer on the buried oxide layer, and a gate structure on the channel layer, the gate structure including a high-k dielectric layer, an N-type work function layer, and a metal gap filling layer stacked in sequence from the channel layer upward, the plurality of semiconductor device groups including a first device group and a second device group, the semiconductor structures in the first device group and the second device group also including a P-type work function layer between the high-k dielectric layer and the N-type work function layer. The thickness of the P-type work function layer in the semiconductor devices in the first device group and the semiconductor devices in the second device group is different, and / or the doping state of the substrate under the semiconductor devices in the first device group and the semiconductor devices in the second device group is different, the doping state including the substrate and the channel layer on the substrate being the same or opposite, so that the semiconductor devices in the first device group and the second device group can have different threshold voltages, the different threshold voltages are regulated by at least one of the thickness of the P-type work function layer and the doping state of the substrate, the device structure difference is small, easy to implement, and the manufacturing efficiency of the device is improved. In addition, gate conductivity, high-k layer compatibility, and no decrease in channel mobility can be guaranteed.

[0126] The above is only a preferred implementation of the present application. Although the present application has been disclosed as a preferred embodiment, it is not intended to limit the present application. Any technician familiar with the art can use the above disclosed methods and technical contents to make many possible changes and modifications to the technical solution of the present application without departing from the scope of the technical solution of the present application, or modify it into an equivalent embodiment of equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present application without departing from the content of the technical solution of the present application still falls within the scope of protection of the technical solution of the present application.

Claims

1. A method for manufacturing a wafer structure, characterized in that: include: providing a substrate; forming a plurality of semiconductor device groups on the substrate; Each semiconductor device group includes at least one semiconductor device; The formation process of the semiconductor device includes: Forming a buried oxide layer on the substrate, a channel layer on the buried oxide layer, and a gate structure on the channel layer, wherein the gate structure comprises a high-k dielectric layer, an N-type work function layer, and a metal gap filling layer stacked in sequence from the channel layer upward; The plurality of semiconductor device groups include a first device group and a second device group, and the semiconductor structures in the first device group and the second device group further include a P-type work function layer between the high-k dielectric layer and the N-type work function layer; The thickness of the P-type work function layer in the semiconductor devices in the first device group and the semiconductor devices in the second device group is different, and / or the doping states of the substrates under the semiconductor devices in the first device group and the semiconductor devices in the second device group are different, and the doping states include the doping types of the substrate and the channel layer on the substrate being the same or opposite.

2. The method according to claim 1, characterized in that If the thickness of the P-type work function layer in the semiconductor devices in the first device group and the semiconductor devices in the second device group are different, the process of forming the gate structure includes: forming a high-k dielectric layer on the channel layer in the first device group and the second device group; Blocking the area where the first device group is located to form a P-type work function layer in the second device group, and blocking the area where the second device group is located to form a P-type work function layer in the first device group; forming an N-type work function layer on the P-type work function layer in the first device group and the second device group; A metal gap-filling layer is formed on the N-type work function layer in the first device group and the second device group.

3. The method according to claim 1, characterized in that: If the thickness of the P-type work function layer in the semiconductor devices in the first device group and the semiconductor devices in the second device group are different, the process of forming the gate structure includes: forming a high-k dielectric layer on the channel layer in the first device group and the second device group; forming a P-type work function layer having a preset thickness in the first device group and the second device group; The area where the first device group is located is shielded to thin the P-type work function layer in the second device group, and / or the area where the second device group is located is shielded to thin the P-type work function layer in the first device group; forming an N-type work function layer on the P-type work function layer in the first device group and the second device group; A metal gap-filling layer is formed on the N-type work function layer in the first device group and the second device group.

4. The method according to claim 1, characterized in that If the doping states of the substrates under the semiconductor devices in the first device group and the semiconductor devices in the second device group are different, the method further includes: The substrate in the area where the first device group is located is shielded so as to dope the substrate in the area where the second device group is located; and / or, the substrate in the area where the second device group is located is shielded so as to dope the substrate in the area where the first device group is located.

5. The method according to any one of claims 1 to 4, characterized in that: The thickness range of the P-type work function layer is (0nm, 6nm].

6. The method according to claim 5, characterized in that The thickness ranges of the P-type work function layers in the semiconductor devices in the first device group and the semiconductor devices in the second device group are different, and the thickness range includes one of a first range, a second range and a third range. The first range is [1.5nm, 2nm], the second range is [2.7nm, 4nm], and the third range is (4nm, 6nm].

7. The method according to claim 6, characterized in that The doping type of the channel layer in the semiconductor device in the first device group is N-type, the thickness of the P-type work function layer in the semiconductor device in the first device group belongs to the first range, and for at least one of the first device and the second device in the first device group, the substrate under the first device and the channel layer in the first device have the same doping type, and the substrate under the second device and the channel layer in the second device have opposite doping types.

8. The method according to claim 6, characterized in that The doping type of the channel layer in the semiconductor devices in the second device group is P type, the second device group includes at least one of the first group and the second group, the thickness of the P type work function layer in the semiconductor devices in the first group belongs to the second range, and the thickness of the P type work function layer in the semiconductor devices in the second group belongs to the third range; The first group includes at least one of a third device and a fourth device, the substrate under the third device and the channel layer in the third device have the same doping type, and the substrate under the fourth device and the channel layer in the fourth device have opposite doping types; The second group includes at least one of a fifth device and a sixth device, the substrate under the fifth device and the channel layer in the fifth device have the same doping type, and the substrate under the sixth device and the channel layer in the sixth device have opposite doping types.

9. The method according to any one of claims 1 to 4, characterized in that: The plurality of semiconductor device groups further include a third device group, and the semiconductor devices in the third device group do not have a P-type work function layer; the formation process of the gate structure includes: forming a high-k dielectric layer on the channel layer in the first device group, the second device group, and the third device group; Blocking the area where the first device group and the third device group are located to form a P-type work function layer in the second device group, and blocking the area where the second device group and the third device group are located to form a P-type work function layer in the first device group; forming an N-type work function layer on the P-type work function layer in the first device group, the second device group, and the third device group; A metal gap-filling layer is formed on the N-type work function layer in the first device group, the second device group, and the third device group.

10. The method according to claim 7, characterized in that The doping type of the channel layer in the semiconductor device in the third device group is N-type; The third device group includes at least one of a seventh device and an eighth device, the substrate under the seventh device and the channel layer in the seventh device have the same doping type, and the substrate under the eighth device and the channel layer in the eighth device have opposite doping types.

11. The method according to any one of claims 1 to 4, characterized in that: In the plurality of semiconductor device groups, semiconductor devices having the same P-type work function layer thickness and the same doping state are arranged within the same region.

12. The method according to any one of claims 1 to 4, characterized in that: The method further comprises: forming a dummy gate structure on the channel layer; A source structure and a drain structure located on both sides of the dummy gate structure; The dummy gate structure is removed to obtain a dummy gate trench, and the dummy gate trench is used to form the gate structure.

13. The method according to any one of claims 1 to 4, characterized in that: The method further comprises: At least one of an oxide layer between the high-k dielectric layer and the channel layer, a high-k dielectric protection layer and an etching barrier layer between the high-k dielectric layer and the N-type work function layer, and a barrier layer between the N-type work function layer and the metal gap filling layer is formed.

14. The method according to claim 13, characterized in that The material of the oxide layer is silicon oxide, and the thickness range is [3nm, 4nm]; And / or, the material of the high-k dielectric layer is HfO2, and the thickness range is [1nm, 1.5nm]; And / or, the material of the high-k dielectric protection layer is TiN, and the thickness range is [0.8nm, 1.2nm]; And / or, the material of the etching stop layer is tantalum nitride or tantalum compound, and the thickness range is [0.5nm, 0.9nm]; And / or, the material of the P-type work function layer is TiN; the material of the N-type work function layer is titanium aluminum, titanium aluminum carbide or titanium aluminum oxide, and the thickness range is [4.5nm, 5.5nm]; And / or, the material of the barrier layer is TiN, and the thickness range is [1.5nm, 2.5nm]; And / or, the material of the metal gap filling layer is tungsten; the sum of the thicknesses of the metal gap filling layer and the P-type work function layer is a preset value; And / or, the buried oxide layer has a thickness of 15 nm, and the channel layer is made of silicon with a thickness of 5 nm.

15. The method according to any one of claims 1 to 4, characterized in that: The method further comprises: A back gate connected to the substrate under the semiconductor device is formed.