Cu2O / MgZnO II type heterojunction-based self-powered ultraviolet detector and preparation method thereof
Through Cu2O/MgZnO type II heterojunction structure, combined with sol-gel method and SILAR technology, the problem of insufficient performance of MgZnO self-powered ultraviolet detectors is solved, and high responsiveness, low dark current and fast response are achieved.
Patent Information
- Application Number
- CN202410924204.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
AI Technical Summary
At this stage, the comprehensive performance of the self-powered ultraviolet detector based on MgZnO has not yet reached a satisfactory level, and it is necessary to improve the responsiveness, reduce dark current, improve the response speed and improve the spectral response characteristics.
Cu2O/MgZnO type II heterojunction structure was used to prepare MgZnO nanofilm and continuous ion layer adsorption and reaction technology (SILAR) through sol-gel method, and Au electrode was vacuum deposition on the surface of Cu2O film to form Type II The energy band arrangement structure is used to realize the conversion of photoelectric signals.
It effectively reduces dark current, improves ultraviolet light absorption efficiency and interface charge dynamics, and improves the comprehensive performance of self-powered ultraviolet detectors.
Smart Images

Figure CN118899352A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ultraviolet photoelectric detection, and specifically relates to a high-performance self-powered ultraviolet detector based on a Cu2O / MgZnO II type heterojunction and a preparation method thereof. Background Art
[0002] UV photodetectors have important applications in the fields of cell detection, remote control, environmental monitoring, and optoelectronic integrated circuits. Self-powered means obtaining energy in a usable form in the environment to drive the operation of low-power devices. Self-powered photodetectors can convert incident light radiation into measurable electrical signals without external bias, and monitor ambient light in an independent, sustainable, and maintenance-free manner. They have the advantages of small size, low energy consumption, and fast response speed. They have become a hot topic in the field of UV detection technology. PN junction UV detectors are composed of P-type semiconductors and N-type semiconductors with band gap alignment. The principle lies in the built-in electric field formed inside the PN junction. In self-powered UV detectors, the formation of PN junctions is not only the basis for realizing photoelectric conversion, but also the key to optimizing device performance, improving detection sensitivity, and response speed. The PN heterojunction based on the type II band arrangement structure can effectively reduce the recombination of electron-hole pairs, so that electrons and holes move directionally along the energy band steps, and then are collected by electrodes to form photocurrent.
[0003] With the continuous development of science and technology, various application fields have put forward higher requirements for the performance parameters of self-powered UV detectors, such as sensitivity, response speed and detection limit, to meet the needs of different application scenarios. ZnO is a semiconductor material with a direct bandgap and wide bandgap (3.37eV). Through the incorporation of Mg, a MgZnO alloy with an adjustable bandgap width from 3.3eV to 7.8eV can be realized. Due to its excellent optoelectronic properties, it is considered to be one of the most ideal materials for preparing solar-blind and visible-blind UV detectors. However, due to some inherent deficiencies of MgZnO, such as low carrier mobility, short exciton lifetime, surface state, and energy level matching problems between materials, the comprehensive performance of the current MgZnO-based self-powered UV detector still has a lot of room for improvement. It is necessary to further improve the responsivity of existing devices, reduce dark current, increase response speed, and improve spectral response characteristics. Therefore, on the basis of MgZnO materials and mainstream device structures, using reasonable and simple methods to improve and innovate in the preparation of new composite materials and device physical mechanisms to achieve the improvement of the comprehensive performance of the device has become a hot spot and mainstream direction of research in the field of self-powered UV detection technology. Summary of the invention
[0004] In view of the above problems, the present invention discloses a self-powered ultraviolet detector based on Cu2O / MgZnOII type heterojunction and a preparation method thereof.
[0005] The purpose of the present invention is achieved through the following technical solutions.
[0006] like Figure 1 As shown, a self-powered ultraviolet detector based on Cu2O / MgZnO type II heterojunction, the detector is composed of a)-b) from bottom to top, wherein
[0007] a) FTO glass substrate;
[0008] b) MgZnO nanofilm: prepared on FTO glass substrate by sol-gel method;
[0009] c) Cu2O thin film: prepared on the surface of MgZnO thin film using continuous ion layer adsorption and reaction SILAR technology;
[0010] d) Au electrode: prepared by vacuum evaporation on the surface of Cu2O film.
[0011] Furthermore, the self-powered ultraviolet detector based on Cu2O / MgZnO type II heterojunction is optionally:
[0012] a) The thickness of the FTO glass substrate is 1 to 2 mm;
[0013] b) The thickness of the MgZnO nanofilm is 100-160 nm;
[0014] c) The thickness of the Cu2O film is 5 to 30 nm;
[0015] d) The thickness of the Au electrode is 90 to 120 nm.
[0016] The present invention also discloses a method for preparing the self-powered ultraviolet detector based on the Cu2O / MgZnO type II heterojunction, comprising the following steps:
[0017] (1) The FTO glass substrate was placed in acetone, ethanol and deionized water for ultrasonic cleaning for 10-20 minutes, then dried with a nitrogen gun, and then placed in a UV-ozone machine for 5-15 minutes;
[0018] (2) Preparation of MgZnO nanofilm
[0019] First, prepare MgZnO sol: add 0.53-2.63 g zinc acetate, 0.13-0.64 g magnesium acetate and 0.19-0.93 mL ethanolamine to 10-50 mL isopropanol at 60-80°C and continue stirring until a colorless transparent colloid is obtained, and then stand for aging for 12-15 hours;
[0020] A MgZnO nanofilm is prepared on the surface of the FTO glass substrate cleaned in step (1): MgZnO sol is spin-coated on the surface of the FTO glass substrate to form a film; then, the film is dried at 160-200° C. for 10-15 min, and after the substrate is cooled to room temperature, the spin coating and drying steps are repeated 3-7 times; finally, the MgZnO sol film is sintered together with the quartz substrate at 450-700° C. for 2-4 h, thereby obtaining a MgZnO nanofilm on the surface of the FTO glass substrate with a thickness of 100-160 nm;
[0021] (3) Preparation of Cu2O thin film
[0022] In one SILAR cycle, the FTO glass substrate covered with the MgZnO nanofilm prepared in step (1) is first immersed in a 60-70° C. aqueous solution containing 0.2-0.5M sodium hydroxide for 5-10 seconds; the substrate is then immersed in a 0.01-0.05M copper sulfate aqueous solution containing 0.04-0.08M sodium thiosulfate for 5-10 seconds, and then rinsed with deionized water for 10-20 seconds; 3-17 SILAR cycles are performed, and finally dried in air, thereby obtaining a Cu2O film with a thickness of 5-30nm on the surface of the MgZnO nanofilm;
[0023] (4) Preparation of Au Electrode
[0024] The Au electrode was prepared on the surface of Cu2O film by vacuum evaporation method with a vacuum degree of 4.0×10 -4 ~8.0×10 -4 Pa, the evaporation time is 10 to 20 minutes; after the evaporation is completed, an Au electrode is obtained on the surface of the Cu2O film with a thickness of 90 to 120 nm, the bottom FTO and the top Au are the cathode and the anode respectively, and the self-powered ultraviolet detector based on the Cu2O / MgZnOⅡ type heterojunction is prepared.
[0025] Furthermore, in the above preparation method, in the step (2), the MgZnO sol film is formed on the FTO surface by spin coating at a spin coating speed of 2000 to 3500 rpm and a spin coating time of 20 to 30 s.
[0026] Furthermore, in the above preparation method, in the step (3), the immersion time of forming the Cu2O film on the surface of the MgZnO film by the method of continuous ion layer adsorption and reaction is 5 to 10 seconds, and the deionized water rinsing time is 10 to 20 seconds.
[0027] Furthermore, in the above preparation method, in step (4), the vacuum degree of the Au electrode prepared by vacuum evaporation technology is 4.0×10 -4 ~8.0×10 -4Pa, the evaporation time is 10 to 20 minutes.
[0028] The invention also discloses the use of the ultraviolet detector in the fields of cell detection, remote control, environmental monitoring or photoelectric integrated circuits.
[0029] The invention also discloses the use of the preparation method in the fields of cell detection, remote control, environmental monitoring or photoelectric integrated circuits.
[0030] Compared with the existing technology, the present invention has the following advantages and beneficial effects:
[0031] The present invention discloses a high-performance ultraviolet detector based on self-powered and SILAR technology of Cu2O / MgZnO type II heterojunction. Its main working principle is: the energy levels of the conduction band and valence band of MgZnO are lower than those of Cu2O, and a type II energy band arrangement structure is formed at the heterojunction, which is conducive to the rapid separation and transmission of photogenerated electron-hole pairs. When the two materials of N-type MgZnO and P-type Cu2O are in contact, a depletion region and a built-in electric field directed from MgZnO to Cu2O are generated in the type II heterojunction. In the dark state, the high potential barrier and depletion region of the heterojunction region can effectively limit the transmission of free carriers, the majority carrier concentration in the composite material will be significantly reduced, and the device will be in a high resistance state, thereby reducing the dark current of the device. Under ultraviolet light, the built-in electric field will quickly separate the photogenerated electron-hole pairs generated in the depletion region. The electrons in Cu2O flow to MgZnO, and the holes in MgZnO flow to Cu2O. The separated carriers are transmitted to the electrodes at both ends without external bias, thereby generating self-powered performance to complete the conversion of photoelectric signals.
[0032] The present invention uses SILAR technology to introduce Cu2O as a P-type semiconductor and a surface modification layer of MgZnO, forming a type II energy band arrangement structure at the contact interface. In the dark state, a depletion region is formed near the heterojunction, so that the majority carriers in the composite thin film material are greatly depleted, and the dark current of the device can be effectively suppressed. Under ultraviolet light, the built-in electric field can promote the rapid separation and transmission of photogenerated electron-hole pairs. The present invention constructs a Cu2O / MgZnO type II heterojunction, effectively improves the ultraviolet light absorption efficiency and improves the interface charge dynamics, so that the performance of the self-powered ultraviolet detector based on the Cu2O / MgZnO heterojunction is comprehensively improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 : A schematic diagram of the structure of the device of the present invention;
[0034] Figure 2 : Current-voltage characteristic curve of the device involved in the present invention (Cu2O film thickness is 7nm);
[0035] Figure 3 : Current-voltage characteristic curve of the device involved in the present invention (Cu2O film thickness is 16nm);
[0036] Figure 4 : Current-voltage characteristic curve of the device involved in the present invention (Cu2O film thickness is 25nm). DETAILED DESCRIPTION
[0037] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below through the accompanying drawings and embodiments. However, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0038] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0039] Example 1
[0040] A method for preparing a self-powered ultraviolet detector based on a Cu2O / MgZnO II heterojunction comprises the following steps:
[0041] (1) A 15 mm × 15 mm × 1 mm FTO glass substrate was placed in acetone, ethanol and deionized water for ultrasonic cleaning for 15 minutes, then dried with a nitrogen gun, and then placed in a UV-ozone machine for treatment for 10 minutes.
[0042] (2) Prepare MgZnO nanofilm on FTO glass substrate by sol-gel method. First, prepare MgZnO sol: at 75°C, add 1.58g zinc acetate, 0.39g magnesium acetate and 0.56mL ethanolamine to 30mL isopropanol in sequence and stir continuously until a colorless transparent colloid is obtained, and then stand for aging for 15 hours; spin-coat the MgZnO sol on the surface of the FTO glass substrate to form a film, the spin coating speed is 3000 rpm, and the spin coating time is 30 seconds; then dry at 180°C for 10 minutes, and repeat the above spin coating and drying steps 5 times after the substrate is cooled to room temperature. Finally, sinter the MgZnO sol film together with the FTO glass substrate at 500°C for 2 hours, thereby obtaining a MgZnO nanofilm with a thickness of 140nm on the surface of the FTO glass substrate;
[0043] (3) In one SILAR cycle, the FTO glass substrate covered with the MgZnO nanofilm prepared above was immersed in a 60°C aqueous solution containing 0.2M sodium hydroxide for 5 seconds; then the substrate was immersed in a 0.01M copper sulfate aqueous solution containing 0.04M sodium thiosulfate for 5 seconds, and then rinsed with deionized water for 10 seconds; 5 SILAR cycles were performed, and finally dried in air, thereby obtaining a Cu2O film with a thickness of 7nm on the surface of the MgZnO nanofilm.
[0044] (4) The Au electrode was prepared by vacuum evaporation technology with a vacuum degree of 6×10 -4 Pa, the evaporation time is 15 minutes; after the evaporation is completed, an Au electrode with a thickness of 100 nm is obtained on the surface of the Cu2O film, and the device is completed.
[0045] Performance Test:
[0046] After the device with Cu2O thickness of 7nm was prepared, the light and dark current-voltage characteristics of the device were tested. Figure 2 As shown in the figure, in the dark state, the dark current of the device is 1.01nA under 0V bias; at a wavelength of 325nm and a light intensity of 420mW / cm 2 Under ultraviolet light irradiation, the photocurrent of the device is 0.44μA at 0V bias, and the light-to-dark current ratio of the device is 435.
[0047] Example 2
[0048] A method for preparing a self-powered ultraviolet detector based on a Cu2O / MgZnO II heterojunction comprises the following steps:
[0049] (1) A 15 mm × 15 mm × 1 mm FTO glass substrate was placed in acetone, ethanol and deionized water for ultrasonic cleaning for 15 minutes, then dried with a nitrogen gun, and then placed in a UV-ozone machine for treatment for 10 minutes.
[0050] (2) Prepare MgZnO nanofilm on FTO glass substrate by sol-gel method. First, prepare MgZnO sol: at 75°C, add 1.58g zinc acetate, 0.39g magnesium acetate and 0.56mL ethanolamine to 30mL isopropanol in sequence and stir continuously until a colorless transparent colloid is obtained, and then stand for aging for 15 hours; spin-coat the MgZnO sol on the surface of the FTO glass substrate to form a film, the spin coating speed is 3000 rpm, and the spin coating time is 30 seconds; then dry at 180°C for 10 minutes, and repeat the above spin coating and drying steps 5 times after the substrate is cooled to room temperature. Finally, sinter the MgZnO sol film together with the FTO glass substrate at 500°C for 2 hours, thereby obtaining a MgZnO nanofilm with a thickness of 140nm on the surface of the FTO glass substrate;
[0051] (3) In one SILAR cycle, the FTO glass substrate covered with the MgZnO nanofilm prepared above was immersed in a 60°C aqueous solution containing 0.2M sodium hydroxide for 5 seconds; then the substrate was immersed in a 0.01M copper sulfate aqueous solution containing 0.04M sodium thiosulfate for 5 seconds, and then rinsed with deionized water for 10 seconds; 10 SILAR cycles were performed, and finally dried in air, thereby obtaining a Cu2O film with a thickness of 16nm on the surface of the MgZnO nanofilm.
[0052] (4) The Au electrode was prepared by vacuum evaporation technology with a vacuum degree of 6×10 -4 Pa, the evaporation time is 15 minutes; after the evaporation is completed, an Au electrode with a thickness of 100 nm is obtained on the surface of the Cu2O film, and the device is completed.
[0053] Performance Test:
[0054] After the device with Cu2O thickness of 16nm was prepared, the light and dark current-voltage characteristics of the device were tested. Figure 3 As shown in the figure, in the dark state, the dark current of the device is 1.27nA under 0V bias; at a wavelength of 325nm and a light intensity of 420mW / cm 2 Under ultraviolet light irradiation, the photocurrent of the device is 1.63μA at 0V bias, and the light-to-dark current ratio of the device is 1283.
[0055] Example 3
[0056] A method for preparing a self-powered ultraviolet detector based on a Cu2O / MgZnO II heterojunction comprises the following steps:
[0057] (1) By ultrasonic cleaning, an FTO glass substrate with a size of 15 mm × 15 mm × 1 mm was placed in acetone, ethanol and deionized water for ultrasonic cleaning for 15 minutes, then dried with a nitrogen gun, and then placed in a UV-ozone machine for treatment for 10 minutes.
[0058] (2) Prepare MgZnO nanofilm on FTO glass substrate by sol-gel method. First, prepare MgZnO sol: at 75°C, add 1.58g zinc acetate, 0.39g magnesium acetate and 0.56mL ethanolamine to 30mL isopropanol in sequence and stir continuously until a colorless transparent colloid is obtained, and then stand for aging for 15 hours; spin-coat the MgZnO sol on the surface of the FTO glass substrate to form a film, the spin coating speed is 3000 rpm, and the spin coating time is 30 seconds; then dry at 180°C for 10 minutes, and repeat the above spin coating and drying steps 5 times after the substrate is cooled to room temperature. Finally, sinter the MgZnO sol film together with the FTO glass substrate at 500°C for 2 hours, thereby obtaining a MgZnO nanofilm with a thickness of 140nm on the surface of the FTO glass substrate;
[0059] (3) In one SILAR cycle, the prepared FTO glass substrate covered with the MgZnO nanofilm is immersed in a 60°C aqueous solution containing 0.2M sodium hydroxide for 5 seconds; the substrate is then immersed in a 0.01M copper sulfate aqueous solution containing 0.04M sodium thiosulfate for 5 seconds, and then rinsed with deionized water for 10 seconds; 15 SILAR cycles are performed, and finally dried in air, thereby obtaining a Cu2O film with a thickness of 25nm on the surface of the MgZnO nanofilm;
[0060] (4) The Au electrode was prepared by vacuum evaporation technology with a vacuum degree of 6×10 -4 Pa, the evaporation time is 15 minutes; after the evaporation is completed, an Au electrode with a thickness of 100 nm is obtained on the surface of the Cu2O film, and the device is completed.
[0061] Performance Test:
[0062] After the device with Cu2O thickness of 25nm was prepared, the light and dark current-voltage characteristics of the device were tested. Figure 4 As shown in the figure, in the dark state, the dark current of the device is 1.33nA under 0V bias; at a wavelength of 325nm and a light intensity of 420mW / cm 2 Under ultraviolet light irradiation, the photocurrent of the device is 1.08μA at 0V bias, and the light-to-dark current ratio of the device is 812.
[0063] From the above embodiments, it can be seen that the present invention uses SILAR technology to introduce Cu2O as a P-type semiconductor and a surface modification layer of MgZnO to form a type II energy band arrangement structure at the contact interface. In the dark state, a depletion region will be formed near the heterojunction so that the majority of carriers in the composite thin film material are greatly depleted, and the dark current of the device can be effectively suppressed. Under ultraviolet light, the built-in electric field can promote the rapid separation and transmission of photogenerated electron-hole pairs. The present invention constructs a Cu2O / MgZnO type II heterojunction, effectively improves the ultraviolet light absorption efficiency and improves the interface charge dynamics, so that the performance of the self-powered ultraviolet detector based on the Cu2O / MgZnO heterojunction is comprehensively improved.
[0064] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Therefore, based on the innovative concept of the present invention, changes and modifications to the embodiments described herein, or equivalent structural or equivalent process transformations made using the contents of the specification and drawings of the present invention, directly or indirectly applying the above technical solutions to other related technical fields are all included in the protection scope of the patent of the present invention.
Claims
1. A self-powered ultraviolet detector based on Cu2O / MgZnO type II heterojunction, characterized in that: The detector is composed of a)-b) from bottom to top, wherein a) FTO glass substrate; b) MgZnO nanofilm: prepared on FTO glass substrate by sol-gel method; c) Cu2O thin film: prepared on the surface of MgZnO thin film using continuous ion layer adsorption and reaction SILAR technology; d) Au electrode: prepared by vacuum evaporation on the surface of Cu2O film.
2. A self-powered ultraviolet detector based on Cu2O / MgZnO type II heterojunction as claimed in claim 1, characterized in that: Optional, a) The thickness of the FTO glass substrate is 1 to 2 mm; b) The thickness of the MgZnO nanofilm is 100-160 nm; c) The thickness of the Cu2O film is 5 to 30 nm; d) The thickness of the Au electrode is 90 to 120 nm.
3. The method for preparing a self-powered ultraviolet detector based on Cu2O / MgZnO type II heterojunction according to claim 1, characterized in that: The following steps are involved: (1) The FTO glass substrate was placed in acetone, ethanol and deionized water for ultrasonic cleaning for 10-20 minutes, then dried with a nitrogen gun, and then placed in a UV-ozone machine for 5-15 minutes; (2) Preparation of MgZnO nanofilm First, prepare MgZnO sol: add 0.53-2.63 g zinc acetate, 0.13-0.64 g magnesium acetate and 0.19-0.93 mL ethanolamine to 10-50 mL isopropanol at 60-80°C and continue stirring until a colorless transparent colloid is obtained, and then stand for aging for 12-15 hours; A MgZnO nanofilm is prepared on the surface of the FTO glass substrate cleaned in step (1): MgZnO sol is spin-coated on the surface of the FTO glass substrate to form a film; then, the film is dried at 160-200° C. for 10-15 min, and after the substrate is cooled to room temperature, the spin coating and drying steps are repeated 3-7 times; finally, the MgZnO sol film is sintered together with the quartz substrate at 450-700° C. for 2-4 h, thereby obtaining a MgZnO nanofilm on the surface of the FTO glass substrate with a thickness of 100-160 nm; (3) Preparation of Cu2O thin film In one SILAR cycle, the FTO glass substrate covered with the MgZnO nanofilm prepared in step (1) is first immersed in a 60-70° C. aqueous solution containing 0.2-0.5M sodium hydroxide for 5-10 seconds; the substrate is then immersed in a 0.01-0.05M copper sulfate aqueous solution containing 0.04-0.08M sodium thiosulfate for 5-10 seconds, and then rinsed with deionized water for 10-20 seconds; 3-17 SILAR cycles are performed, and finally dried in air, thereby obtaining a Cu2O film with a thickness of 5-30nm on the surface of the MgZnO nanofilm; (4) Preparation of Au Electrode The Au electrode was prepared on the surface of Cu2O film by vacuum evaporation method with a vacuum degree of 4.0×10 -4 ~8.0×10 -4 Pa, evaporation time is 10 to 20 minutes; After the evaporation is completed, an Au electrode is obtained on the surface of the Cu2O film with a thickness of 90 to 120 nm. The bottom FTO and the top Au are the cathode and the anode respectively, and the self-powered ultraviolet detector based on the Cu2O / MgZnO II type heterojunction is prepared.
4. The method for preparing a self-powered ultraviolet detector based on a Cu2O / MgZnO type II heterojunction according to claim 3, characterized in that: In step (2), the MgZnO sol film is formed on the FTO surface by spin coating at a spin coating speed of 2000 to 3500 rpm and a spin coating time of 20 to 30 s.
5. The method for preparing a self-powered ultraviolet detector based on a Cu2O / MgZnO type II heterojunction according to claim 3, characterized in that: In step (3), the immersion time of forming the Cu2O film on the surface of the MgZnO film by the method of continuous ion layer adsorption and reaction is 5 to 10 seconds, and the deionized water rinsing time is 10 to 20 seconds.
6. The method for preparing a self-powered ultraviolet detector based on a Cu2O / MgZnO type II heterojunction according to claim 3, characterized in that: In step (4), the vacuum degree of the Au electrode prepared by vacuum evaporation technology is 4.0×10 -4 ~8.0×10 -4 Pa, the evaporation time is 10 to 20 minutes.
7. Use of the ultraviolet detector according to any one of claims 1 to 2 in the field of cell detection, remote control, environmental monitoring or optoelectronic integrated circuits.
8. Use of the preparation method according to any one of claims 3 to 6 in the field of cell detection, remote control, environmental monitoring or optoelectronic integrated circuits.