MXene edge growth metal sulfide composite material as well as preparation method and application thereof

The growth of metal sulfide composite materials at the edge of MXene as a catalyst solves the problems of poor sulfur conductivity and slow reaction kinetics in sodium-sulfur batteries, improves the capacity and cycle life of the battery, and achieves efficient sulfur cathode utilization and structural stability.

CN118899441AActive Publication Date: 2024-11-05TIANJIN NORMAL UNIVERSITY

Patent Information

Application Number
CN202410891997.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-11-05
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

Due to problems such as poor sulfur conductivity, slow reaction kinetics, and large volume expansion, sodium-sulfur batteries have fast capacity decay and poor reversible capacity, and lack high-performance multifunctional S catalytic support materials.

Method used

Using MXene edge-growing metal sulfide composite material as a catalyst, the in-situ growth metal sulfide is designed and constructed through positive and negative charge suction characteristics, which improves sulfur conductivity and reaction kinetics, inhibits volume expansion and shuttle effects, and enhances the physics of polysulfides. and chemical adsorption.

Benefits of technology

The specific capacity and cycle life of room temperature Na-S batteries are significantly improved, the utilization efficiency and structural stability of sulfur cathode are enhanced, and the volume expansion and shuttle effects are suppressed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899441A_ABST
    Figure CN118899441A_ABST
Patent Text Reader

Abstract

The invention discloses an MXene edge growth metal sulfide composite material as well as a preparation method and application thereof, and belongs to the field of electrochemical energy storage. The preparation method of the composite material comprises the following steps: dissolving MXene, metal anion salt, thiourea and polyvinylpyrrolidone in a mixed solution of water and ethylene glycol, and obtaining the MXene edge growth metal sulfide composite material through a one-step hydrothermal method. The composite material takes two-dimensional MXene as a conductive substrate, metal sulfide is uniformly loaded on the edge to form a'fishing net 'structure, and the material is simple in synthesis operation and high in repeatability. The exposed surface of MXene can improve electron conduction of S and inhibit volume expansion of S as a conductive substrate, a fishing net structure can physically limit polysulfide, metal sulfide can serve as a catalyst for S species conversion, conversion reaction of S species is accelerated, dissolution of polysulfide is reduced, shuttle effect is inhibited, and the stability of S species conversion is improved. Therefore, the sodium storage material as a multifunctional S catalytic carrier material of a room-temperature Na-S battery shows more excellent sodium storage performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of electrochemical energy storage, and in particular relates to a MXene edge-grown metal sulfide composite material and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries (LIBs) are widely used in portable devices, electric vehicles, smart grids and other fields as energy storage and power systems. However, the scarcity and uneven distribution of lithium resources inevitably restrict the large-scale application of LIBs. Among many electrochemical energy storage systems, sodium batteries are expected to become the most promising alternative to lithium batteries because the earth has more sodium reserves than lithium. Among them, room-temperature sodium-sulfur (Na-S) batteries based on multi-electron conversion reactions exhibit ultra-high theoretical energy density (1274Wh / kg), and the raw materials are abundant in nature (sodium abundance is about 25670ppm, sulfur abundance is about 953ppm), low in price (metallic sodium: 230,000 yuan / ton), and environmentally friendly, making them extremely competitive in the field of large-scale safe energy storage.

[0003] Similar to Li-S batteries, Na-S batteries also face some challenges, such as fast capacity decay, low sulfur utilization and poor reversible capacity. These problems are usually caused by a variety of factors, including the poor conductivity of sulfur and its discharge products, the slow reaction kinetics of solid sulfur and sodium, the "shuttle effect" caused by the dissolution / diffusion of polysulfides in the electrolyte, and the huge volume expansion (~260%) during the charge / discharge process. The ideal S support material should not only provide high electronic conductivity and increase the chemical adsorption of sodium polysulfide, but also have the catalyst function to accelerate the conversion reaction of sodium polysulfide and improve its reaction kinetics, so as to achieve efficient utilization and high performance of the S positive electrode. Therefore, the development of multifunctional S catalytic support materials with high conductivity, high adsorption capacity, high catalytic activity, high specific surface area and high stability is the key to promote the commercialization of high-performance room-temperature Na-S batteries for large-scale energy storage. To this end, we propose a MXene edge-grown metal sulfide composite material and its preparation method, and its application as an efficient S host in room-temperature Na-S batteries. Summary of the invention

[0004] The purpose of the present invention is to overcome the above-mentioned shortcomings of the prior art, and to provide a MXene edge-grown metal sulfide composite material and a preparation method and application thereof. The positive and negative charge attraction characteristics are utilized to make the metal anion salt preferentially adsorbed on the positively charged MXene edge, and a multifunctional catalyst for in-situ growth of metal sulfide on the MXene edge is designed and constructed, which is used as a host catalytic material for the sulfur positive electrode of a room temperature sodium-sulfur battery. Based on the two-dimensional highly conductive exposed polar surface of MXene, the conductivity of sulfur species can be improved, the volume expansion can be buffered, and the physical and chemical adsorption of polysulfides can be increased. The two-dimensional metal sulfide with high catalytic activity on the MXene edge can further achieve physical and chemical confinement of polysulfides, and accelerate the catalytic conversion of sodium polysulfide, thereby effectively preventing the shuttle effect of sodium polysulfide and improving the specific capacity and cycle life of the room temperature Na-S battery.

[0005] The purpose of the present invention is achieved through the following technical solutions:

[0006] A method for preparing a MXene edge-grown metal sulfide composite material comprises the following steps:

[0007] (1) MXene, metal anion salt, thiourea and polyvinyl pyrrolidone were added to 10 mL of water and 20 mL of ethylene glycol in a mass ratio of 1: (5-20): (20-100): (1-5), and ultrasonic stirring was performed for 30 minutes to form a mixed solution.

[0008] (2) The mixed solution was added to a 50 mL polytetrafluoroethylene liner and sealed in a stainless steel reactor. The mixture was kept in an oven at 180-220°C for 12-48 hours. After cooling to room temperature, the precipitate was centrifugally washed with water and anhydrous ethanol for 3 times each. The final precipitate was freeze-dried to obtain a MXene edge-growth metal sulfide composite material.

[0009] Preferably, the MXene in step (1) is Ti3C2T x 、Ti2CT x 、Mo2CT x 、V2CT x or V4C3T x One or more of .

[0010] Preferably, the metal anion salt in step (1) is one or more of ammonium molybdate tetrahydrate, ammonium perrhenate, ammonium vanadium oxide, vanadium acetylacetonate, ammonium tungstate, iron acetylacetonate, cobalt acetylacetonate, nickel acetylacetonate, manganese acetylacetonate, copper acetylacetonate or sodium stannate.

[0011] The present invention also provides a MXene edge-growth metal sulfide composite material obtained according to the aforementioned preparation method.

[0012] The present invention also provides the use of the above-mentioned MXene edge-grown metal sulfide composite material as an S carrier to prepare a mixed S electrode and in a room temperature sodium-sulfur battery.

[0013] The method of making the application is as follows:

[0014] (1) The MXene edge-grown metal sulfide composite material, S powder, conductive agent and binder are ground and mixed in a mass ratio of 2:5:2:1, and an appropriate amount of deionized water or NMP is added and stirred evenly. The obtained slurry is evenly applied to the rough surface of the copper current collector and vacuum dried at 60-120°C to obtain a Na-S battery composite S electrode.

[0015] (2) The composite S electrode is used as the positive electrode of the Na-S battery, and metallic sodium is used as the negative electrode. The electrolyte is 1M NaSO3CF3 dissolved in DEGDME solvent or 1M NaPF6 dissolved in DEGDME solvent or 1M NaPF6 dissolved in DME solvent. The diaphragm is made of glass fiber GF / D and Celgard2325 as a double-layer diaphragm, wherein the Celgard2325 diaphragm is close to the composite S electrode side, and they are assembled in sequence into a CR2032 button-type room temperature Na-S battery.

[0016] Preferably, the conductive agent in step (1) is one or more of conductive carbon black, graphene, MXene or carbon nanotubes.

[0017] Preferably, the binder in step (1) is one or more of polyvinylidene fluoride, polyacrylic acid, polytetrafluoroethylene, polyvinyl alcohol, carboxymethyl cellulose or sodium alginate.

[0018] Advantages and beneficial effects of the present invention:

[0019] (1) The present invention proposes a novel heterostructure construction strategy based on MXene, which utilizes the attraction between positive and negative charges to make metal anion salts preferentially adsorbed on the positively charged MXene edge. A one-step hydrothermal method is used to design and construct an in-situ grown metal sulfide composite material on the MXene edge. This strategy is simple to operate and has strong repeatability, and it also has the adjustability of MXene and metal elements.

[0020] (2) The MXene edge-grown metal sulfide composite material uses MXene as the substrate, exposing a rich active surface, so that the exposed MXene surface is more exposed to S particles and S species during the reaction process, which improves the overall structural stability and electronic conductivity while also inhibiting the volume expansion during the S reaction.

[0021] (3) The metal sulfide composite material grows on the edge of the MXene. The metal sulfide grown on the edge of the MXene is like a lead sinker in a fishing net, making the MXene like a fishing net that can physically confine and capture polysulfides, thereby inhibiting the shuttling of polysulfides. In addition, the metal sulfide grown on the edge of the MXene can also serve as a catalyst for the conversion of S species, accelerating the conversion reaction of S species to Na2S, reducing the dissolution of polysulfides, and further inhibiting the shuttling effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is a transmission electron microscope image of the MoS2@MXene composite material synthesized in Example 1 and its corresponding element distribution map;

[0023] Figure 2 is the X-ray diffraction spectrum of the MoS2@MXene composite material synthesized in Example 1;

[0024] Figure 3 is a transmission electron microscope image of the ReS2@MXene composite material synthesized in Example 5;

[0025] Figure 4 is a transmission electron microscopy image of the CoS2@MXene composite material synthesized in Example 6;

[0026] Figure 5 The rate performance diagram of the S / MoS2@MXene electrode prepared in Example 7 and the pure S electrode prepared in Comparative Example 4 at current densities of 0.2, 0.5, 1, 2 and 5 A / g respectively;

[0027] Figure 6 is a cycle stability diagram of the S / MoS2@MXene electrode prepared in Example 7 at a current density of 2A / g;

[0028] Figure 7 This is a transmission electron microscope image of the MXene double-sided growth MoS2 composite material synthesized in Comparative Example 1;

[0029] Figure 8 This is a transmission electron microscope image of the MXene double-sided growth MoS2 composite material synthesized in Comparative Example 2;

[0030] Fig. 9 This is a transmission electron microscope image of the MXene double-sided growth MoS2 composite material synthesized in Example 3. DETAILED DESCRIPTION

[0031] In order to make the above-mentioned objects and advantages of the present invention clear and easy to understand, the technical solutions in the embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings in the embodiments of the present invention, but the present invention is not limited to the specific embodiments. Among them, the materials mentioned above can be obtained from commercial channels unless otherwise specified.

[0032] Embodiment 1:

[0033] This embodiment provides a synthesis and characterization analysis of a MXene edge-grown metal sulfide composite material. The specific synthesis process is as follows:

[0034] (1) 20 mg of Ti3C2T x MXene, 123.6 mg of ammonium molybdate tetrahydrate, 865 mg of thiourea, and 25 mg of polyvinyl pyrrolidone were added to 10 mL of water and 20 mL of ethylene glycol, and ultrasonic stirring was performed for 30 min to form a mixed solution.

[0035] (2) The mixed solution was added into a 50 mL polytetrafluoroethylene liner and sealed in a stainless steel reactor. The mixture was kept in an oven at 200 °C for 24 h. After cooling to room temperature, the precipitate was centrifugally washed with water and anhydrous ethanol for 3 times each. The final precipitate was freeze-dried to obtain a MXene edge-grown metal sulfide composite material (MoS2@MXene).

[0036] Figure 1 Transmission electron microscope image of MoS2@MXene composite material synthesized in this example and its corresponding element distribution map. Figure 1 It can be seen that the synthesized MoS2@MXene composite material presents a lace-like structure, that is, MoS2 nanosheets grow around the edge of MXene. The size of MoS2 nanosheets is about 30-80nm, and the size of MXene nanosheets is about 0.5-1μm. The element distribution diagram further confirms this lace-like structure. S and Mo elements are mainly distributed at the edge of MXene, while Ti represents Ti3C2T x MXene.

[0037] Figure 2 X-ray diffraction spectrum of the MoS2@MXene composite material synthesized in this example. Figure 2 It can be seen that the XRD diffraction peaks of the composite material can be indexed to the (101) and (110) crystal planes of MoS2 (PDF#77-0341).

[0038] Embodiment 2:

[0039] The same preparation method as described in Example 1, except that:

[0040] In step (1), the added amounts of MXene, ammonium molybdate tetrahydrate, thiourea and polyvinyl pyrrolidone are 20 mg, 247.2 mg, 1730 mg and 50 mg, respectively, and the other conditions and parameters are the same as those in Example 1.

[0041] Embodiment 3:

[0042] The same preparation method as described in Example 1, except that:

[0043] In step (2), the hydrothermal reaction temperature is 220° C., and other conditions and parameters are the same as those in Example 1.

[0044] Embodiment 4:

[0045] The same preparation method as described in Example 1, except that:

[0046] In step (2), the hydrothermal reaction temperature is 180° C., and other conditions and parameters are the same as those in Example 1.

[0047] Embodiment 5:

[0048] The same preparation method as described in Example 1, except that:

[0049] In step (1), ammonium molybdate tetrahydrate was replaced with 268 mg of ammonium perrhenate, and other conditions and parameters were the same as those in Example 1.

[0050] Figure 3 Transmission electron microscopy image of the ReS2@MXene composite material synthesized in this example. Figure 3 It can be seen that the synthesized ReS2@MXene composite material also presents a lace-like structure, and ReS2 nanosheets grow around the edge of MXene.

[0051] Embodiment 6:

[0052] The same preparation method as described in Example 1, except that:

[0053] In step (1), ammonium molybdate tetrahydrate was replaced with 259 mg of cobalt acetylacetonate, and other conditions and parameters were the same as those in Example 1.

[0054] Figure 4 Transmission electron microscopy image of the CoS2@MXene composite material synthesized in this example. Figure 4 It can be seen that the synthesized CoS2@MXene composite material also presents a lace-like structure. The CoS2 particles grow around the edge of the MXene. The CoS2 particles scattered on the surface of the MXene may be due to the defect position of the MXene, and the cobalt ions are preferentially adsorbed and grown in situ.

[0055] Embodiment 7:

[0056] This embodiment provides a preparation of a composite S electrode and a room temperature Na-S battery performance test. The detailed operation process is as follows:

[0057] (1) The MoS2@MXene dry powder obtained in Example 1 was used as an S carrier catalytic material, and was evenly mixed with S powder, conductive carbon black and polyacrylic acid binder in a mass ratio of 2:5:2:1. An appropriate amount of deionized water was added, and the mixture was ground into a paste in an agate mortar. The mixture was then coated on the rough surface of a copper foil using a coating machine. After drying in an oven at 60°C for 12 hours, the mixture was cut into discs with a diameter of 14 mm and maintained at a pressure of 6 MPa for 1 minute under a press to obtain a composite S electrode sheet (S / MoS2@MXene).

[0058] (2) Assemble 2032 button cells in a glove box. The electrolyte is 1 M NaSO3CF3 dissolved in DEGDME. GF / D and Celgard 2325 separators are used as battery separators. The Celgard 2325 separator is placed close to the S / MoS2@MXene electrode, and metallic sodium is used as the negative electrode.

[0059] (3) The button cell assembled in step (2) was subjected to a performance test in a Xinwei battery testing system. The battery charge and discharge voltage range was 0.4 to 3 V. The current density of the rate performance test was 0.2, 0.5, 1, 2, 5 and 0.2 A / g. The cycle performance was tested for 700 cycles at a current density of 2 A / g.

[0060] like Figure 5 As shown, the rate performance test conditions of the S / MoS2@MXene electrode are 10 cycles at 0.2, 0.5, 1, 2 and 5 A / g. The discharge capacity of the battery in the first cycle at each rate is 1559, 1181, 1162, 1130 and 830 mAh / g, respectively. At the end of the test, it returns to 0.2 A / g, and the discharge capacity is 1256 mAh / g, with excellent rate performance.

[0061] like Figure 6 As shown, the reversible specific capacity of the S / MoS2@MXene battery can be maintained at 1163.2 mAh / g after 700 cycles at a current density of 2 A / g, and the capacity retention rate is about 93.4%.

[0062] Comparative Example 1:

[0063] This example provides the synthesis and characterization of a comparative material of a MXene edge-grown metal sulfide composite material (MXene double-sided grown metal sulfide). The specific synthesis process is the same as the preparation method described in Example 1, except that:

[0064] In step (1), the amounts of water and ethylene glycol were 4 mL and 26 mL respectively, and the other conditions and parameters were the same as those in Example 1.

[0065] like Figure 7As shown, the MXene double-sided growth MoS2 composite material synthesized in this example shows a different structure from the MXene edge growth MoS2 composite material. The MoS2 synthesized under this condition no longer grows in situ only on the edge of the MXene, but grows on the entire surface of the MXene. However, this will reduce the electrical conductivity and toughness of the MXene, which is not conducive to the electron transport and structural stability of the S species.

[0066] Comparative Example 2:

[0067] This example provides the synthesis and characterization of another comparative material of MXene edge-grown metal sulfide composite material (MXene double-sided grown metal sulfide). The specific synthesis process is the same as the preparation method described in Example 1, except that:

[0068] In step (1), the amounts of water and ethylene glycol are 0 mL and 30 mL, respectively, and the other conditions and parameters are the same as those in Example 1.

[0069] like Figure 8 As shown, the structure of the MXene double-sided growth MoS2 composite material synthesized in this example is the same as that of Comparative Example 1, both of which grow MoS2 on the surface of MXene. The difference is that the size and morphology of the MoS2 nanosheets are different. The MoS2 nanosheets in this example are smaller and tend to agglomerate into balls and aggregate on the MXene surface. It can also be seen that the different addition ratios of water and ethylene glycol are crucial to the regulation of structural morphology.

[0070] Comparative Example 3:

[0071] In order to further confirm the universality of the strategy of in-situ growth of metal sulfide composite materials on the edge of MXene by the attraction between positive and negative charges, the surface of MXene is modified with positive charge, and the synthesis and characterization of a comparative material (MXene double-sided growth metal sulfide) of a MXene edge-grown metal sulfide composite material is provided. The specific synthesis process is the same as the preparation method described in Example 1, except that:

[0072] In step (1), the MXene is a positively charged PDDA-modified MXene, and the modification process is to add the original MXene to 5 mL of a polydimethylammonium chloride (PDDA) solution with a molecular weight of 100,000-200,000 and a concentration of 20%, and obtain the PDDA-modified MXene by stirring and ultrasonic dispersion and then centrifugation. The other conditions and parameters are carried out according to Example 1.

[0073] like Fig. 9As shown, the MoS2 nanosheets synthesized in this example will grow in situ on both sides of the MXene surface. This is because after the MXene surface is modified with positive charges, it also preferentially adsorbs molybdate anions, allowing the MoS2 nanosheets to grow on the entire surface. This further confirms the versatility of the strategy of utilizing the negatively charged surface and positively charged edges of the MXene to in situ grow metal sulfide composite materials at the edge of the MXene through the attraction between positive and negative charges.

[0074] Comparative Example 4:

[0075] This example provides a preparation and electrochemical performance characterization of a comparative electrode (pure S electrode) of a S / MoS2@MXene electrode. The specific preparation process is the same as the preparation method described in Example 7, except that:

[0076] In step (1), S powder, conductive carbon black and polyacrylic acid binder are uniformly mixed in a mass ratio of 7:2:1. Other conditions and parameters are the same as those in Example 7. The assembly of the room temperature Na-S battery is also the same as in Example 7.

[0077] Figure 5 The figure shows the rate performance of the pure S electrode prepared in this example at a current density of 0.2-5 A / g. Compared with the rate performance of the S / MoS2@MXene electrode in Example 7, it can be seen that the use of the MXene edge-grown metal sulfide composite material (MoS2@MXene) as an S carrier catalyst significantly improves the performance of the room temperature Na-S battery, indicating that this special structure can inhibit the dissolution shuttle of captured sodium polysulfide and act as a catalyst to accelerate the conversion reaction of polysulfide, thereby significantly improving the S sodium storage performance.

[0078] The embodiments described above are merely descriptions of preferred implementation modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing a MXene edge-grown metal sulfide composite material, comprising the following steps: (1) MXene, metal anion salt, thiourea and polyvinyl pyrrolidone were added to 10 mL of water and 20 mL of ethylene glycol in a mass ratio of 1: (5-20): (20-100): (1-5), and ultrasonic stirring was performed for 30 minutes to form a mixed solution; (2) The mixed solution was added to a 50 mL polytetrafluoroethylene liner and sealed in a stainless steel reactor. The mixture was kept in an oven at 180-220°C for 12-48 hours. After cooling to room temperature, the precipitate was centrifugally washed with water and anhydrous ethanol for 3 times each. The final precipitate was freeze-dried to obtain a MXene edge-growth metal sulfide composite material.

2. The method according to claim 1, characterized in that The MXene is Ti3C2T x 、Ti2CT x 、Mo2CT x 、V2CT x or V4C3T x One or more of .

3. The method according to claim 1, characterized in that The metal anion salt is one or more of ammonium molybdate tetrahydrate, ammonium perrhenate, ammonium vanadium oxide, vanadium acetylacetonate, ammonium tungstate, iron acetylacetonate, cobalt acetylacetonate, nickel acetylacetonate, manganese acetylacetonate, copper acetylacetonate or sodium stannate.

4. The MXene edge-growth metal sulfide composite material obtained by the method according to any one of claims 1 to 3.

5. Use of the MXene edge-grown metal sulfide composite material according to claim 4 in the preparation of composite S electrodes and room temperature Na-S batteries.

6. The use according to claim 5, characterized in that: The composite S electrode is prepared as follows: a MXene edge-grown metal sulfide composite material, S powder, a conductive agent and a binder are ground and mixed in a mass ratio of 2:5:2:1, an appropriate amount of deionized water or NMP is added dropwise, and the mixture is stirred evenly. The obtained slurry is evenly applied to the rough surface of a copper current collector and vacuum dried at 60-120° C. to obtain a composite S electrode for a Na-S battery.

7. The use according to claim 6, characterized in that The conductive agent is one or more of conductive carbon black, graphene, MXene or carbon nanotubes.

8. The use according to claim 6, characterized in that The binder is one or more of polyvinylidene fluoride, polyacrylic acid, polytetrafluoroethylene, polyvinyl alcohol, carboxymethyl cellulose or sodium alginate.

9. A room temperature Na-S battery, characterized in that: The composite S electrode sheet obtained by the method described in any one of claims 6 to 8 is assembled, the counter electrode is metallic sodium, the electrolyte is 1M NaSO3CF3 dissolved in DEGDME solvent or 1M NaPF6 dissolved in DEGDME solvent or 1M NaPF6 dissolved in DME solvent, and the diaphragm is made of glass fiber GF / D and Celgard2325 as a double-layer diaphragm, wherein the Celgard2325 diaphragm is close to one side of the composite S electrode.

Citation Information

Patent Citations

  • MXene / metal sulfide composite material, anode material and preparation and application

    CN111180694A

  • MXene-based composite material for improving performance of lithium-sulfur battery diaphragm and preparation method of MXene-based composite material

    CN115504473A

  • Preparation method of cubic-phase cobalt-nickel sulfide and few-layer Ti3C2Tx MXene nanosheet composite material for room-temperature sodium-sulfur battery

    CN116364916A

  • Self-supporting-based high-sulfur-loading flexible MXene composite electrode and preparation method and application thereof

    CN117219730A

  • MXene-bimetallic sulfide composite material modified battery diaphragm, preparation method thereof and lithium-sulfur battery

    CN117963984A

Cited By