Preparation method and application of lithium ion battery electrolyte additive
By using a cyclic washing and purification device to efficiently purify the lithium-ion battery electrolyte additive, the problems of highly toxic chemicals and low purity in the prior art are solved, and high conversion and high purity electrolyte additives are achieved Preparation, suitable for industrial production.
Patent Information
- Application Number
- CN202411194425.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-05
AI Technical Summary
The existing preparation methods for lithium-ion battery electrolyte additives involve highly toxic chemicals, with low reaction yields and low purification efficiency, and are not suitable for industrial production.
The (sub)phosphate or (sub)phosphate salt is reacted with cyano alcohol, solvent and catalyst in a distillation reactor at a temperature of 100°C to 150°C, and efficient purification is performed by circulating washing and purification equipment to avoid Hazardous chemicals, improving reaction conversion and purity.
It has achieved high conversion rate and high purity lithium-ion battery electrolyte additive preparation, which is safe and low-cost, suitable for industrial production, and avoids the generation and pollution of "three wastes".
Smart Images

Figure CN118899541A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries, and in particular relates to a preparation method of a lithium ion battery electrolyte additive and application thereof. Background Art
[0002] The electrolyte of lithium-ion batteries is mainly composed of lithium salts, solvents, and additives. Although the additives account for the smallest proportion, they have a crucial impact on battery performance. As lithium batteries pursue high voltage and high specific capacity performance, a series of problems will arise: first, it will cause chemical instability at the electrode / electrode liquid interface, causing the electrode liquid to decompose, resulting in increased interface film impedance and capacity decay; transition metal ions will dissolve at the positive electrode, which will not only cause the positive electrode material to fail, but also the dissolved transition metal ions will migrate to the negative electrode to affect the formation of the negative electrode SEI film, thereby affecting the battery performance. In order to solve the above problems, adding film-forming additives and complex metal ion additives has become an important way.
[0003] The electrolyte to which cyano (hypo)phosphite or its cyano (hypo)phosphite salt derivative is added helps to form a stable and dense SEI film on the electrode surface, inhibiting further decomposition of the electrolyte; due to the electron-donating property of phosphorus atoms, the passivation film formed is conducive to lithium ion transmission, and the addition of cyano groups not only complexes free transition metal ions to prevent migration to the negative electrode and affect the SEI film, but also physically adsorbs on the positive electrode surface to inhibit transition metal dissolution.
[0004] Patent application CN117164619A uses cyano alcohol, phosphorus oxychloride and acid binding agent as raw materials and reacts in an organic solvent system. However, the defects of this method are: the raw materials phosphorus oxychloride and acid binding agent involved are highly toxic and corrosive chemicals, and once leaked, they may cause serious consequences; at the same time, this method also has the disadvantages of low reaction yield, low purification efficiency, low product purity, heavy "three wastes", etc., and is not suitable for industrial production. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention provides a preparation method and application of a lithium ion battery electrolyte additive, which does not involve highly toxic chemical raw materials, has high atomic utilization rate, high product purity, simple process, easy operation, and is more suitable for the industrial production of cyano (hypo)phosphites and cyano (hypo)phosphite salt derivatives.
[0006] The present invention is achieved through the following technical solutions:
[0007] A method for preparing a lithium ion battery electrolyte additive comprises the following steps:
[0008] Step 1) reacting a (hypo)phosphite or a (hypo)phosphite salt with a cyano alcohol, a solvent and a catalyst in a distillation reactor at a temperature of 100° C. to 150° C. for 8 to 12 hours to generate a target product;
[0009] Wherein, the molar ratio of the (hypo)phosphite to the cyano alcohol is 1:3.1 to 1:3.5, and the molar ratio of the (hypo)phosphite salt to the cyano alcohol is 1:2.1 to 1:2.5;
[0010] Step 2) After separating the low-boiling by-products and the solvent, the target product is transferred to the washing device of the circulating washing and purification device. During the slow stirring process, the washing solvent in the boiling device of the circulating washing and purification device enters the washing device after evaporation and condensation, and overflows into the boiling device after washing, thereby circulating washing the target product to finally obtain a product with a purity of more than 99%.
[0011] Preferably, the (hypo)phosphite in step 1) includes trimethyl (hypo)phosphite and triethyl (hypo)phosphite; the (hypo)phosphite salt includes dimethyl (hypo)phosphite lithium salt, diethyl (hypo)phosphite lithium salt, dimethyl (hypo)phosphite sodium salt, diethyl (hypo)phosphite sodium salt, dimethyl (hypo)phosphite potassium salt, and diethyl (hypo)phosphite potassium salt.
[0012] Preferably, the cyano alcohol in step 1) includes 2-hydroxypropionitrile, 3-hydroxypropionitrile, 3-hydroxybutyronitrile, 4-hydroxy-3,3-dimethylbutyronitrile, cyanomethyl alcohol, and 2-hydroxyisobutyronitrile.
[0013] Preferably, the solvent in step 1) includes N,N-dimethylformamide, N,N-dimethylacetamide, toluene, xylene, N,N-diethylformamide, N-methylformamide, N-ethylformamide, dimethyl sulfoxide, and tetramethyl urea.
[0014] Preferably, the catalyst in step 1) comprises sodium hydroxide, potassium hydroxide, sodium methoxide, sodium ethoxide, potassium methoxide, potassium ethoxide; and the amount of the catalyst used is 0.1% to 2% of the mass of the (hypo)phosphite or (hypo)phosphite salt.
[0015] Preferably, the washing solvent in step 2) includes dichloromethane, 1,2-dichloroethane, ethyl acetate, toluene, acetonitrile, tetrahydrofuran, acetone, petroleum ether, 1,4-dioxane, ethylene glycol dimethyl ether, and diethyl ether.
[0016] Preferably, the circulating washing and purification device in step 2) comprises a condenser, a washing device, a boiling device, a first pipe, a second pipe, a magnetic stirrer and a third pipe, the first pipe and the third pipe are provided at the bottom of the condenser, the condenser is connected to the washing device through the third pipe, the condenser is connected to the boiling device through the first pipe, the washing device and the boiling device are connected through the second pipe, and the washing device and the boiling device are both provided with a magnetic stirrer.
[0017] Application of the lithium ion battery electrolyte additive prepared by the above preparation method in the preparation of lithium ion batteries.
[0018] The beneficial effects of the present invention are as follows:
[0019] (1) The preparation method provided by the present invention has a target product that is more stable than the raw material, and the by-product low-boiling methanol / ethanol is promptly distilled out of the reaction system, which promotes the reaction in the forward direction from both thermodynamic and kinetic aspects, achieves a high reaction conversion rate, does not generate "three wastes", and does not involve hazardous chemicals. The reaction process is safe and the operation is simple.
[0020] (2) The preparation method provided by the present invention uses solvent boiling-refluxing to circulate and wash the crude product, with high purification efficiency, achieving efficient purification of the product, recycling of materials (solvents), low cost, no pollution, and suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a schematic diagram of the structure of a circulating washing and purification device;
[0022] In the figure: 1, condenser; 2, washing kettle; 3, solvent kettle; 4, first pipeline; 5, second pipeline; 6, magnetic stirrer; 7, third pipeline. DETAILED DESCRIPTION
[0023] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0024] A method for preparing a lithium ion battery electrolyte additive, the specific steps are as follows:
[0025] (1) Preparation: At a temperature of 100° C. to 150° C., a (hypo)phosphite or (hypo)phosphite salt is reacted with a cyano alcohol, a solvent and a catalyst in a distillation reactor for 8 to 12 hours to produce the target product.
[0026] The (hypo)phosphite refers to phosphate or phosphite, and the (hypo)phosphite salt refers to phosphate or phosphite.
[0027] The molar ratio of the (hypo)phosphite to cyano alcohol is 1:3.1 to 1:3.5, and the molar ratio of the (hypo)phosphite salt to cyano alcohol is 1:2.1 to 1:2.5; the amount of the catalyst is 0.1% to 2% of the mass of the (hypo)phosphite or (hypo)phosphite salt.
[0028] The (hypo)phosphites include but are not limited to trimethyl (hypo)phosphite and triethyl (hypo)phosphite; the (hypo)phosphite salts include but are not limited to dimethyl (hypo)phosphite lithium salt, diethyl (hypo)phosphite lithium salt, dimethyl (hypo)phosphite sodium salt, diethyl (hypo)phosphite sodium salt, dimethyl (hypo)phosphite potassium salt, and diethyl (hypo)phosphite potassium salt.
[0029] The cyano alcohols include, but are not limited to, 2-hydroxypropionitrile, 3-hydroxypropionitrile, 3-hydroxybutyronitrile, 4-hydroxy-3,3-dimethylbutyronitrile, cyanomethyl alcohol, and 2-hydroxyisobutyronitrile.
[0030] The solvent includes, but is not limited to, N,N-dimethylformamide, N,N-dimethylacetamide, toluene, xylene, N,N-diethylformamide, N-methylformamide, N-ethylformamide, dimethyl sulfoxide, and tetramethyl urea.
[0031] The catalyst includes but is not limited to sodium hydroxide, potassium hydroxide, sodium methoxide, sodium ethoxide, potassium methoxide, and potassium ethoxide.
[0032] (2) Purification: After separating the low-boiling by-products and solvents, the target product (crude product) is transferred to a washing device. During the slow stirring process, the washing solvent in the boiling device evaporates and condenses into the washing device, and overflows into the boiling device after washing, thereby circulating the crude product for washing, and finally obtaining a product with a purity of more than 99%.
[0033] The washing solvent includes, but is not limited to, dichloromethane, 1,2-dichloroethane, ethyl acetate, toluene, acetonitrile, tetrahydrofuran, acetone, petroleum ether, 1,4-dioxane, ethylene glycol dimethyl ether, and diethyl ether.
[0034] The above-mentioned washing device and boiling device are both components of a circulating washing and purification device. Figure 1As shown, it includes a condenser 1, a washing kettle 2, a solvent kettle 3, a first pipe 4, a second pipe 5, a magnetic stirrer 6 and a third pipe 7; the first pipe 4 and the third pipe 7 are provided at the bottom of the condenser 1, the condenser 1 is connected to the upper part of the washing kettle 2 (i.e., the washing device) through the third pipe 7, and the condenser 1 is connected to the upper part of the solvent kettle 3 (i.e., the boiling device) through the first pipe 4; the washing kettle 2 and the solvent kettle 3 are connected through the second pipe 5, and the second pipe 5 is connected to the upper part of the solvent kettle 3 by the side wall of the washing kettle 2 and extends to the bottom of the solvent kettle 3; the washing kettle 2 and the solvent kettle 3 are both provided with a magnetic stirrer 6.
[0035] In the above-mentioned preparation method, the reaction temperature between the (hypo)phosphite or (hypo)phosphite salt and cyanohydrin and the temperature of the distillation tube are usually determined according to the boiling points of the reactants and the products. Generally, the products are allowed to leave the system while the reactants are retained while ensuring that there is sufficient temperature to promote the reaction. There is usually no special restriction on the reaction time, and the reaction can be completed within the above-mentioned range.
[0036] Example 1
[0037] A method for preparing a lithium ion battery electrolyte additive, the specific steps are as follows:
[0038] (1) Preparation: To a 1000 mL reactor equipped with a distillation apparatus, 124.1 g (1 mol) of trimethyl phosphite, 280.8 g (3.3 mol) of 3-hydroxybutyronitrile, 1 g of sodium methoxide and 50 mL of N,N-dimethylformamide were added; under stirring, the temperature of the distillation tube was maintained at 65°C, and after reacting at a temperature of 100°C for 8 hours, no liquid flowed out from the tail of the condenser, and the reaction was completed.
[0039] (2) Purification: Figure 1 As shown, after the reaction is completed, the filtrate is filtered, collected and rotary evaporated to remove low-boiling impurities, and the obtained crude tris(2-(1-cyano)propyl)phosphite is placed in a washing kettle 2 of a washing device, and a proper amount of ethylene glycol dimethyl ether is placed in a solvent kettle 3 of a boiling device and heated to 110° C. for evaporation, and the steam is condensed and refluxed in a condenser 1 through a first pipeline 4, and the condensate is collected in the washing kettle 2 through a third pipeline 7 and is in a stratified state, and the lower layer is the crude tris(2-(1-cyano)propyl)phosphite. When the liquid level rises to the second pipeline 5, the magnetic stirrer 6 is turned on and the speed is controlled so that the lower liquid level is lower than the pipe mouth, and the upper washing liquid flows back to the solvent kettle 3 through the second pipeline 5, and the end is after 30 minutes, and the lower liquid is collected and rotary dried to obtain tris(2-(1-cyano)propyl)phosphate, with a yield of 81.2% and a purity of 99.47%.
[0040] Example 2
[0041] A method for preparing a lithium ion battery electrolyte additive, the specific steps are as follows:
[0042] (1) Preparation: To a 1000 mL reactor equipped with a distillation device, 116 g (1 mol) of lithium dimethyl phosphite, 195.7 g (2.3 mol) of 3-hydroxybutyronitrile, 1 g of sodium methoxide and 400 mL of N,N-dimethylacetamide were added; under stirring, the temperature of the distillation tube was maintained at 65°C, and the reaction was carried out at a temperature of 140°C for 12 hours. The reaction was terminated when no liquid flowed out from the tail of the condenser.
[0043] (2) Purification: Figure 1 As shown, after the reaction is completed, the reaction is filtered while hot, the solid is collected and dried, and the obtained crude lithium di(2-(1-cyano)propyl)phosphite is placed in a washing kettle 2 of a washing device, and an appropriate amount of acetonitrile is placed in a solvent kettle 3 of a boiling device and heated to 105° C. for evaporation. The vapor is condensed and refluxed in a condenser 1 through a first pipe 4, and the condensate is collected in a washing kettle 2 through a third pipe 7. When the liquid level rises to the second pipe 5, the magnetic stirrer 6 is turned on and the speed is controlled so that the solid is below the pipe mouth, and the upper washing liquid flows back to the solvent kettle 3 through the second pipe 5. After 1 hour, the solid is filtered and collected, and the di(2-(1-cyano)propyl)lithium phosphate is obtained by drying with a yield of 82.7% and a purity of 99.58%.
[0044] Example 3
[0045] A method for preparing a lithium ion battery electrolyte additive, the specific steps are as follows:
[0046] (1) Preparation: To a 1000 mL reactor equipped with a distillation apparatus, 182.2 g (1 mol) of triethyl phosphate, 223.9 g (3.15 mol) of 3-hydroxypropionitrile, 1.5 g of sodium ethoxide and 50 mL of N,N-dimethylacetamide were added; under stirring, the temperature of the distillation tube was maintained at 80°C, and the reaction was carried out at a temperature of 120°C for 10 h. The reaction was terminated when no liquid flowed out from the tail of the condenser.
[0047] (2) Purification: Figure 1As shown, after the reaction is completed, the filtrate is filtered, collected and rotary evaporated to remove low-boiling impurities, and the obtained crude tris(2-cyanoethyl) phosphate is placed in a washing kettle 2 of a washing device, and an appropriate amount of 1,4-dioxane is placed in a solvent kettle 3 of a boiling device and heated to 125°C for evaporation. The steam is condensed and refluxed through a first pipe 4 to a condenser 1, and the condensate is collected in a washing kettle 2 through a third pipe 7 and is in a stratified state, wherein the lower layer is the crude tris(2-cyanoethyl) phosphate. When the liquid level rises to the second pipe 5, the magnetic stirrer 6 is turned on and the speed is controlled so that the lower liquid level is lower than the pipe mouth, and the upper washing liquid flows back to the solvent kettle 3 through the second pipe 5, and the process ends after 40 minutes. The lower liquid is collected and rotary dried to obtain tris(2-cyanoethyl) phosphate with a yield of 82.2% and a purity of 99.31%.
[0048] Example 4
[0049] A method for preparing a lithium ion battery electrolyte additive, the specific steps are as follows:
[0050] (1) Preparation: To a 1000 mL reactor equipped with a distillation apparatus, 160 g (1 mol) of lithium diethyl phosphate, 160 g (2.25 mol) of 3-hydroxypropionitrile, 1.5 g of sodium ethoxide and 400 mL of tetramethylurea were added; under stirring, the temperature of the distillation tube was maintained at 80° C., and the reaction was carried out at a temperature of 130° C. for 11 h. The reaction was terminated when no liquid flowed out from the tail of the condenser.
[0051] (2) Purification: Figure 1 As shown, after the reaction is completed, the reaction is filtered while hot, the solid is collected and dried, and the obtained crude lithium di(2-cyanoethyl) phosphate is placed in a washing kettle 2 of a washing device. An appropriate amount of acetone is placed in a solvent kettle 3 of a boiling device and heated to 80° C. for evaporation. The vapor is condensed and refluxed in a condenser 1 through a first pipe 4. The condensate is collected in a washing kettle 2 through a third pipe 7. When the liquid level rises to the second pipe 5, the magnetic stirrer 6 is turned on and the speed is controlled so that the solid is below the pipe mouth. The upper washing liquid flows back to the solvent kettle 3 through the second pipe 5. After 1 hour, the solid is filtered and collected, and the lithium di(2-cyanoethyl) phosphate is obtained by drying with a yield of 78.5% and a purity of 99.44%.
[0052] The embodiments described above are only some embodiments of the present invention, rather than all embodiments. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. The scope of protection of the present invention shall be subject to the scope required by the claims. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work shall fall within the scope of protection of the present invention.
Claims
1. A method for preparing a lithium ion battery electrolyte additive, characterized in that: The following steps are involved: Step 1) reacting a (hypo)phosphite or a (hypo)phosphite salt with a cyano alcohol, a solvent and a catalyst in a distillation reactor at a temperature of 100° C. to 150° C. for 8 to 12 hours to generate a target product; Wherein, the molar ratio of the (hypo)phosphite to the cyano alcohol is 1:3.1 to 1:3.5, and the molar ratio of the (hypo)phosphite salt to the cyano alcohol is 1:2.1 to 1:2.5; Step 2) After separating the low-boiling by-products and the solvent, the target product is transferred to the washing device of the circulating washing and purification device. During the slow stirring process, the washing solvent in the boiling device of the circulating washing and purification device enters the washing device after evaporation and condensation, and overflows into the boiling device after washing, thereby circulating washing the target product to finally obtain a product with a purity of more than 99%.
2. The method for preparing a lithium ion battery electrolyte additive according to claim 1, characterized in that: In step 1), the (hypo)phosphite includes trimethyl (hypo)phosphite and triethyl (hypo)phosphite; the (hypo)phosphite salt includes dimethyl (hypo)phosphite lithium salt, diethyl (hypo)phosphite lithium salt, dimethyl (hypo)phosphite sodium salt, diethyl (hypo)phosphite sodium salt, dimethyl (hypo)phosphite potassium salt, and diethyl (hypo)phosphite potassium salt.
3. The method for preparing a lithium ion battery electrolyte additive according to claim 1, characterized in that: The cyano alcohol in step 1) includes 2-hydroxypropionitrile, 3-hydroxypropionitrile, 3-hydroxybutyronitrile, 4-hydroxy-3,3-dimethylbutyronitrile, cyanomethyl alcohol, and 2-hydroxyisobutyronitrile.
4. The method for preparing a lithium ion battery electrolyte additive according to claim 1, characterized in that: Step 1) The solvent includes N,N-dimethylformamide, N,N-dimethylacetamide, toluene, xylene, N,N-diethylformamide, N-methylformamide, N-ethylformamide, dimethyl sulfoxide, and tetramethyl urea.
5. The method for preparing a lithium ion battery electrolyte additive according to claim 1, characterized in that: The catalyst in step 1) includes sodium hydroxide, potassium hydroxide, sodium methoxide, sodium ethoxide, potassium methoxide, and potassium ethoxide; the amount of the catalyst used is 0.1% to 2% of the mass of the (hypo)phosphite or (hypo)phosphite salt.
6. The method for preparing a lithium ion battery electrolyte additive according to claim 1, characterized in that: Step 2) The washing solvent includes dichloromethane, 1,2-dichloroethane, ethyl acetate, toluene, acetonitrile, tetrahydrofuran, acetone, petroleum ether, 1,4-dioxane, ethylene glycol dimethyl ether, and ethyl ether.
7. The method for preparing a lithium ion battery electrolyte additive according to claim 1, characterized in that: Step 2) The circulating washing and purification device includes a condenser, a washing device, a boiling device, a first pipeline, a second pipeline, a magnetic stirrer and a third pipeline. The first pipeline and the third pipeline are provided at the bottom of the condenser. The condenser is connected to the washing device through the third pipeline. The condenser is connected to the boiling device through the first pipeline. The washing device and the boiling device are connected through the second pipeline. The washing device and the boiling device are both provided with a magnetic stirrer.
8. Use of the lithium ion battery electrolyte additive prepared by the preparation method according to any one of claims 1 to 7 in the preparation of lithium ion batteries.